Curable resin composition, dry film, cured product, and printed wiring board

By using a curable resin composition containing an alkali-soluble resin, a photopolymerization initiator and an amine curing agent on a transparent substrate, the problems of insufficient transparency and heat resistance in the prior art are solved and high transmittance is achieved. , low haze and resistant to yellowing, suitable for flexible displays and printed wiring boards.

CN118786390APending Publication Date: 2024-10-15TAIYO HOLDINGS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380023848.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to form a cured product on a transparent substrate with high total light transmittance, low haze value, and excellent transparency that is resistant to yellowing with the existing technology. It also has insufficient chemical resistance and moisture and heat resistance, especially when using resistant products. Displays made of organic materials with lower thermal properties than glass substrates.

Method used

A curable resin composition containing an alkali-soluble resin, a photopolymerization initiator and an amine curing agent is used to achieve excellent optical properties and mechanical properties through photo-curing and thermal curing, including the use of Cyclomer P (ACA) Z250, Propylene glycol diacrylate and specific photopolymerization initiator control film thickness and exposure to improve deep curability and transmittance.

Benefits of technology

It achieves high total light transmittance, low haze value and transparency that is resistant to yellowing in the curable resin composition. It has low warpage, chemical resistance and moisture and heat resistance, and is suitable for use in flexible substrates. and solder resists and coverings for printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012066110000031
    Figure BDA0005012066110000031
  • Figure BDA0005012066110000081
    Figure BDA0005012066110000081
  • Figure BDA0005012066110000191
    Figure BDA0005012066110000191
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a cured product which, in cases where a curable resin composition is photocured and thermally cured, has optical properties such as a high total light transmittance, a low haze value, and excellent transparency that is not susceptible to yellowing, while having low warpage, excellent chemical resistance, and excellent moist heat resistance; and a curable resin composition which provides the cured product. A cured product obtained by curing a curable resin composition containing (A) an alkali-soluble resin, (B) a predetermined photopolymerization initiator, and (C) an amine-based curing agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable resin composition, a dry film, a cured product and a printed wiring board. Background Art

[0002] In electronic devices used in fields requiring transparency such as displays, touch screens, windshields, and window glasses, a conductive circuit is sometimes formed on a transparent substrate, and an insulating layer is formed for the purpose of protecting the circuit. As such an insulating layer, for example, a curable resin composition having excellent flatness, low hygroscopicity, low gas generation, heat resistance, etc. by using a specific siloxane resin is disclosed (for example, Patent Document 1).

[0003] In addition, in these fields, thinning, lightening and flexibility are developing, and the use of resin films in transparent substrates is being studied. As resin films, polyimide, polyethylene terephthalate, cycloolefin polymers, etc. can be cited, and in particular, polyimide with excellent heat resistance, etc. has been widely studied (for example, Patent Document 2).

[0004] However, since polyimide is expensive, resin films that replace polyimide are also needed. However, resin films with low heat resistance cannot withstand the curing temperature of curable resin compositions generally used in insulating layers, resulting in a problem of increased haze value.

[0005] Furthermore, as electronic devices become more advanced in functionality, resin compositions used in insulating layers are required to have various properties such as low warpage, chemical resistance, and moisture and heat resistance in addition to optical properties such as transparency.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent document 1: Japanese Patent Application Publication No. 2021-59657.

[0009] Patent document 2: Japanese Patent Application Publication No. 2020-73689. Summary of the invention

[0010] Problems to be solved by the invention

[0011] In view of the above circumstances, an object of the present invention is to provide a cured product having optical properties such as a large total light transmittance, a small haze value, and excellent transparency that is not prone to yellowing when a curable resin composition is photocured and thermally cured, and having low warpage, chemical resistance, and excellent resistance to moisture and heat, and a curable resin composition for providing the cured product.

[0012] Means for solving problems

[0013] The present inventors have conducted intensive studies to achieve the above-mentioned purpose and have found that a cured product obtained by curing a curable resin composition containing (A) an alkali-soluble resin, a specified (B) photopolymerization initiator and (C) an amine curing agent provides a cured product having excellent optical properties, low warpage, chemical resistance and moisture and heat resistance, thereby completing the present invention.

[0014] In the curable resin composition of the embodiment of the present invention, as the (B) photopolymerization initiator, a test curable resin composition composed of 100 parts by mass of Cyclomer P(ACA) Z250, 20 parts by mass of dipropylene glycol diacrylate and 1.2 parts by mass of the (B) photopolymerization initiator was used to obtain a film thickness of 4 μm and a cumulative light intensity of 4000 mJ / cm 2 (B) a photopolymerization initiator having a rate of change in absorbance at a wavelength of 410 nm before and after curing of 100% or less when irradiated with active energy rays in a manner to cure.

[0015] By incorporating the above-mentioned (B) photopolymerization initiator into the curable resin composition, the total light transmittance and b* value of a cured product obtained by curing the curable resin composition can be improved.

[0016] In addition, by using the above-mentioned (B) photopolymerization initiator, active energy rays can easily reach the deep part of the coating film, and the deep curability of the coating film can be improved. In addition, by improving the deep curability of the coating film, chemical resistance and adhesion can be improved.

[0017] By including (C) an amine curing agent in the curable resin composition of the present invention, the curing temperature of the curable resin composition can be suppressed to 130° C. or less, and the generation of haze on the substrate can be suppressed. Therefore, the curable resin composition of the present invention can also be suitably used as a flexible substrate for a display using an organic material having lower heat resistance than a glass substrate.

[0018] In addition, by using an amine curing agent having an average particle size of 1 μm or less as the (C) amine curing agent, it is possible to prevent the cured product from becoming white turbid.

[0019] The curable resin composition of the embodiment of the present invention may further contain a urethane (meth)acrylate resin.

[0020] The curable resin composition of the embodiment of the present invention provides a film having a thickness of 10 μm and a cumulative light intensity of 150 mJ / cm 2 The b* value of the cured product obtained by irradiating active energy rays in a manner, developing and thermally curing is 1.5 or less in the CIE L*a*b* color system.

[0021] In addition, the curable resin composition of the embodiment of the present invention provides a film having a thickness of 10 μm and a cumulative light intensity of 150 mJ / cm 2 The total light transmittance of the cured product obtained by irradiating the active energy ray in a manner, developing and thermally curing is 90% or more.

[0022] A dry film according to another aspect of the present invention is characterized in that it is a dry film having a first film and a resin layer composed of a dried coating film of the curable resin composition formed on the first film.

[0023] Furthermore, a cured product according to another aspect of the present invention is a cured product obtained by curing the curable resin composition or the resin layer of the dry film.

[0024] Furthermore, a printed wiring board according to another aspect of the present invention is characterized in having the above-mentioned cured product.

[0025] The cured product of the present invention is characterized in that it is a cured product obtained by curing a curable resin composition containing (A) an alkali-soluble resin, (B) a photopolymerization initiator and (C) an amine-based curing agent, and has a b* value of 1.5 or less in the CIE L*a*b* colorimetric system and a total light transmittance of 90% or more.

[0026] The cured product of the embodiment of the present invention is characterized in that it is a cured product obtained by curing a curable resin composition containing an oxime-based photopolymerization initiator or an acylphosphine oxide-based photopolymerization initiator as the (B) photopolymerization initiator.

[0027] The cured product of the embodiment of the present invention is characterized in that it is a cured product obtained by curing a curable resin composition containing an oxime-based photopolymerization initiator as (B) a photopolymerization initiator, wherein the oxime-based photopolymerization initiator has a structure represented by the following formula (1).

[0028]

[0029] The cured product of the embodiment of the present invention is characterized in that it is obtained by curing a curable resin composition containing an amine curing agent having an average particle size of 1 μm or less as (C) an amine curing agent.

[0030] The cured product according to the embodiment of the present invention is characterized in that it is obtained by curing a curable resin composition further containing a urethane (meth)acrylate resin.

[0031] Effects of the Invention

[0032] According to the present invention, when the curable resin composition is photocured and thermally cured, a cured product having excellent optical properties such as high total light transmittance, low haze value, and transparency that is not prone to yellowing, low warpage, chemical resistance, and moisture and heat resistance, and a curable resin composition providing the cured product can be provided. The cured product of the present invention has good low warpage, chemical resistance, and moisture and heat resistance, and is also useful as a solder resist or cover layer of a printed wiring board. DETAILED DESCRIPTION

[0033] Hereinafter, preferred embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0034] In the present specification, "(meth)acrylate" is a term that collectively refers to "acrylate", "methacrylate" and a mixture thereof, and other similar expressions are the same.

[0035] In this specification, haze refers to the degree of blurriness and is used to indicate the degree of transparency of transparent materials such as glass and plastics. It is expressed as the percentage of the value obtained by dividing the scattered light transmittance of the test piece by the total light transmittance. Therefore, the smaller the haze value, the lower the transmittance of scattered light and the less blurry the material.

[0036] The haze value can be measured in accordance with JIS K 7361:2000.

[0037] In this specification, the total light transmittance refers to the ratio of the amount of transmitted light to the amount of light incident on a material to be measured, and is obtained as a value taking into account reflection on the surface of the material and absorption inside the material.

[0038] The total light transmittance can be measured in accordance with JIS K 7361-1.

[0039] In this specification, the b* value (positive value indicates yellow, negative value indicates bluish tendency) before and after curing and its change Δb* in the CIE L*a*b* color system are used as indicators of yellowing of the cured product. The b* value and Δb* can be measured in accordance with JIS K7373:2006.

[0040] [1. Curable resin composition]

[0041] The curable resin composition according to one embodiment of the present invention contains (A) an alkali-soluble resin, (B) a predetermined photopolymerization initiator, and (C) an amine-based curing agent.

[0042] [1-1. (A) Alkali-soluble resin]

[0043] The (A) alkali-soluble resin used in the present embodiment can be any alkali-soluble resin, and a known and commonly used resin can be used. (A) Alkali-soluble resins can be used alone or in combination of two or more. For example, water-soluble resins such as carboxyl-containing resins and phenolic hydroxyl-containing resins can be cited. Among them, from the viewpoint of excellent developability, carboxyl-containing resins and phenolic hydroxyl-containing resins are preferred, and carboxyl-containing resins are more preferred. The carboxyl-containing resin can be a carboxyl-containing photosensitive resin having an ethylenically unsaturated group (i.e., having photosensitivity), or a carboxyl-containing resin not having an ethylenically unsaturated group. By making the curable resin composition contain (A) alkali-soluble resin, it is easy to form a pattern by alkali development of the coating formed by the curable resin composition. It should be noted that, when making the curable resin composition photosensitive, it is preferably a carboxyl-containing photosensitive resin. When the photosensitive resin containing a carboxyl group is not included, it can be made photosensitized by using a urethane (meth)acrylate resin or a (meth)acrylate monomer described later.

[0044] Specific examples of the carboxyl group-containing resin include the following compounds (which may be either oligomers or polymers).

[0045] (1) Carboxyl group-containing resins obtained by copolymerization of an unsaturated carboxylic acid such as (meth)acrylic acid and a compound containing an unsaturated group such as styrene, α-methylstyrene, a lower alkyl (meth)acrylate, or isobutylene.

[0046] (2) Carboxyl-containing urethane resins produced by the addition polymerization of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylol propionic acid and dimethylol butyric acid, and dihydroxy compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0047] (3) Carboxyl-containing photosensitive urethane resins produced by the polyaddition reaction of diisocyanates with difunctional epoxy resins such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin and diphenylphenol epoxy resin and monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, and carboxyl-containing diol compounds and dihydroxy compounds.

[0048] (4) In the synthesis of the resin of (2) or (3), a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as hydroxyalkyl (meth)acrylate is added to obtain a carboxyl-containing photosensitive urethane resin with terminal (meth)acryloylation.

[0049] (5) In the synthesis of the resin of (2) or (3), a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as equimolar reactants of isophorone diisocyanate and pentaerythritol triacrylate, is added to produce a carboxyl-containing photosensitive urethane resin with terminal (meth)acryloyl groups.

[0050] (6) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or higher polyfunctional (solid) epoxy resin with (meth)acrylic acid to add a dibasic acid anhydride to a hydroxyl group present in a side chain.

[0051] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin obtained by epoxidizing the hydroxyl groups of a bifunctional (solid) epoxy resin with epichlorohydrin with (meth)acrylic acid, and adding a dibasic acid anhydride to the generated hydroxyl groups.

[0052] (8) A carboxyl-containing polyester resin obtained by reacting a bifunctional oxetane resin with a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid, and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the generated primary hydroxyl group.

[0053] (9) A carboxyl-containing photosensitive resin is obtained by reacting an epoxy compound having a plurality of epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule such as p-hydroxyphenylethanol and a monocarboxylic acid containing an unsaturated group such as (meth)acrylic acid, so that the alcoholic hydroxyl group of the reaction product reacts with a polyacid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, etc.

[0054] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.

[0055] (11) A carboxyl-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, the resulting reaction product with a monocarboxylic acid containing an unsaturated group, and reacting the resulting reaction product with a polyacid anhydride.

[0056] (12) A carboxyl-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins of (1) to (11).

[0057] As the resin containing phenolic hydroxyl group, as long as there is a phenolic hydroxyl group, i.e. a hydroxyl group bonded to a benzene ring, on the main chain or the side chain, there is no particular limitation. It is preferably a resin containing two or more phenolic hydroxyl groups in one molecule. As the resin containing two or more phenolic hydroxyl groups in one molecule, catechol, resorcinol, hydroquinone, dihydroxytoluene, naphthalene diol, tert-butylcatechol, tert-butylhydroquinone, pyrogallol, phloroglucinol, bisphenol A, bisphenol F, bisphenol S, biphenol, bimethylol, novolac type phenolic resin, novolac type alkylphenol resin, novolac resin of bisphenol A, dicyclopentadiene type phenolic resin, new phenolic resin (Xylok) type phenolic resin, terpene modified phenolic resin, polyvinylphenol, phenol and the condensation product of aromatic aldehyde with phenolic hydroxyl group, 1-naphthol or 2-naphthol and aromatic aldehyde condensation product etc. can be cited, but it is not limited to these.

[0058] The acid value of the alkali-soluble resin is preferably 20 to 180 mgKOH / g, more preferably 30 to 150 mgKOH / g, and even more preferably 40 to 120 mgKOH / g, from the viewpoint of improving the alkali developability of the curable resin composition.

[0059] From the viewpoint of film-forming ability, the weight average molecular weight of the alkali-soluble resin is preferably 3000 to 30000, more preferably 5000 to 20000, and further preferably 7000 to 15000. The weight average molecular weight can be determined from a standard polystyrene conversion value by gel permeation chromatography (GPC).

[0060] The content of the alkali-soluble resin in the curable resin composition is preferably 20 to 80 parts by mass, more preferably 30 to 75 parts by mass, and even more preferably 40 to 70 parts by mass, based on 100 parts by mass of the total solid content of the curable resin composition.

[0061] As (A) alkali-soluble resin, from the viewpoint of low warpage of cured product, it is preferred to include an alkali-soluble resin having a urethane skeleton. When only an alkali-soluble resin without a urethane skeleton is used as the alkali-soluble resin, a urethane (meth)acrylate resin may be appropriately used in combination as an optional component.

[0062] [1-2. (B) Photopolymerization initiator]

[0063] The photopolymerization initiator is a compound that generates active species capable of initiating polymerization of a polymerizable compound by irradiation with active energy rays.

[0064] As the photopolymerization initiator (B) used in the curable resin composition of the present embodiment, from the viewpoint of improving the deep curability of the coating film and making the total light transmittance and b* value after curing good, it is preferable to use a test curable resin composition composed of 100 parts by mass of Cyclomer P(ACA) Z250, 20 parts by mass of dipropylene glycol diacrylate and 1.2 parts by mass of the photopolymerization initiator (B) to have a film thickness of 4 μm and a cumulative light amount of 4000 mJ / cm 2 (B) a photopolymerization initiator having a rate of change in absorbance at a wavelength of 410 nm before and after curing of 100% or less when irradiated with active energy rays in a manner to cure.

[0065] Examples of the (B) photopolymerization initiator include oxime-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, benzoin-based photopolymerization initiators, and benzophenone-based photopolymerization initiators.

[0066] As the photopolymerization initiator, an oxime-based photopolymerization initiator and / or an acylphosphine oxide-based photopolymerization initiator is preferred from the viewpoint of improving the deep curability of the coating film and improving the total light transmittance and b* value after curing.

[0067] The photopolymerization initiator may be used alone or in combination of two or more.

[0068] The content of the photopolymerization initiator is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the total solid content of the curable resin composition. In the case of 0.01 parts by mass or more, the photocurability of the curable resin composition is good, the coating is difficult to peel, and the coating properties such as chemical resistance are also good. In addition, in the case of 10 parts by mass or less, the effect of reducing outgassing can be obtained, and further, the light absorption of the surface of the solder resist coating is good, and the deep curability is difficult to reduce.

[0069] <Oxime-based photopolymerization initiator>

[0070] As the oxime photopolymerization initiator, an oxime photopolymerization initiator having a structure represented by the following formula (1) is preferably used.

[0071]

[0072] Examples of the oxime-based photopolymerization initiator having a structure represented by formula (1) include 1-pentanone, 1-[4-[[4-(2-benzofuranylcarbonyl)phenyl]thio]phenyl]-4-methyl, 1-(o-acetoxime), 1-propanone, 1-[4-[[4-(2-naphthylcarbonyl)phenyl]thio]phenyl], 1-(o-acetoxime), and the like.

[0073] Examples of commercially available products of the oxime-based photopolymerization initiator having a structure represented by the formula (1) include "Irgacure OXE04" manufactured by BASF Japan KK.

[0074] <Acylphosphine oxide-based photopolymerization initiator>

[0075] Examples of the acylphosphine oxide-based photopolymerization initiator include benzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyl-diphenylphosphine oxide, 3,4-dimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-phenylethoxyphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,6-dimethylbenzoyl)-ethylphosphine oxide.

[0076] Examples of commercially available products of the acylphosphine oxide-based photopolymerization initiator include "Omnirad TPO H" and "Omnirad 819" manufactured by IGM Resins BV.

[0077] [1-3. (C) Amine curing agent]

[0078] By incorporating an amine-based curing agent into the curable resin composition, the curing temperature can be lowered to 130° C. or less.

[0079] Examples of the amine curing agent include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine. Amine compounds such as melamine resins, alkyl etherified melamine resins (for example, melamine resins substituted with methoxy and / or butoxy groups, etc.) and other melamine resin derivatives; Benzotriazole derivatives in which one or two substituents such as methyl, methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl, etc., linear or branched alkyl groups having 1 to 4 carbon atoms, mercapto, amino, phenyl, oxo, carboxyl, halogen groups, etc. are substituted on the benzotriazole heterocycle.

[0080] As the amine curing agent, from the viewpoint of further accelerating the curing rate, a melamine resin derivative and / or a benzotriazole derivative is preferably used.

[0081] As an amine curing agent, from the viewpoint of making the total light transmittance and haze value of the cured product good, it is preferred to use an amine curing agent with an average particle size (D50) of 1 μm or less, and more preferably, the average particle size is 1 μm or less and the D95 value is 5 μm or less.

[0082] It should be noted that, in this specification, "average particle size" (D50) refers to the particle size when the cumulative value in the particle size distribution obtained by the laser diffraction / scattering method is 50%. Similarly, D95 refers to the particle size when the cumulative value in the particle size distribution obtained by the laser diffraction / scattering method is 95%. As a measuring device using the laser diffraction / scattering method, for example, Microtrac MT3300EXII manufactured by Microtrac BEL, Inc. can be cited.

[0083] The content of the amine curing agent is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total solid content of the curable resin composition.

[0084] [1-4. Optional components of curable resin composition]

[0085] The curable resin composition of the present embodiment may contain a urethane (meth)acrylate resin, a (meth)acrylate monomer, a thermosetting compound, a surface tension adjuster, other additive components, and the like.

[0086] <Urethane (meth)acrylate resin>

[0087] The urethane (meth)acrylate resin is a compound having a urethane skeleton and a (meth)acryloyl group in the molecule.

[0088] The urethane (meth)acrylate resin can be produced by, for example, synthesizing a urethane prepolymer from a polyol and a polyisocyanate, and adding a (meth)acrylate having a hydroxyl group thereto.

[0089] As the polyol, for example, known polyols such as hydrocarbon polyols, polyether polyols, polyester polyols, and polycarbonate polyols can be used.

[0090] As the polyisocyanate, for example, known polyisocyanates such as aromatic polyisocyanate, aliphatic polyisocyanate, aromatic aliphatic polyisocyanate and alicyclic polyisocyanate can be used.

[0091] In addition, as the acrylate having a hydroxyl group, for example, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-acryloyloxyethyl-2-hydroxyethyl phthalate, 2-methacryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, ethylene glycol mono(meth)acrylate, glycerol (meth)acrylate, dipentaerythritol mono(meth)acrylate, etc. can be used.

[0092] Examples of commercially available products of urethane (meth)acrylate resins include “UA-4200”, “UA-160TM”, “UA-290TM”, “UA-7100”, “UA-W2A”, “UA-4400”, “UA-122P”, and “U-200PA” manufactured by Shin-Nakamura Chemical Co., Ltd., and “Beamset AQ-19” manufactured by Arakawa Chemical Industries, Ltd.

[0093] <(Meth)acrylate monomer>

[0094] The (meth)acrylate monomer used in the curable resin composition of the present embodiment is not particularly limited, and any known and commonly used monomer may be used. For example, polyfunctional (meth)acrylate monomers such as alkyl acrylate, polyethylene glycol acrylate, polypropylene glycol acrylate, polytetramethylene glycol acrylate, alkoxylated bisphenol A acrylate, alkoxylated trimethylolpropane acrylate, alkoxylated glycerol acrylate, caprolactone-modified isocyanurate acrylate, pentaerythritol acrylate, and alkoxylated pentaerythritol acrylate can be used.

[0095] The (meth)acrylic acid ester monomers may be used alone or in combination of two or more.

[0096] Examples of commercially available (meth)acrylate monomers include "AA-HD-N", "A-NOD-N", "A-DOD-N", "A-NPG", "A-200", "A-400", "A-600", "A-1000", "APG-200", "APG-400", "APG-700", "A-PTMG65", "A-BPE-2.2", "ABE-300", "A-BPE-4", "A-BPE-10", "A-BPE-20", "A-BPP-3", "A-TMPT", "A-TMPT-3EO", "A-TMPT-9EO", "AT-20E ... AT-30E", "A-TMPT-3PO", "A-TMPT-6PO", "A-GLY-3E", "A-GLY-20E", "A-9300", "A-9200YN", "A-9300-1CL", "A-9300-3CL", "A-TMM-3", "A-TMM-3L", "A-TM M-3LM-N", "ATM-4EL", "ATM-4PL", "A-TMMT", "ATM-4E", "ATM-35E", "ATM-4P", "BPE-80N", "BPE-100", "BPE-200", "BPE-500", "BPE-900", "BPE-1300N", etc.

[0097] The content of the (meth)acrylate monomer is preferably 5 to 30 parts by mass, more preferably 10 to 20 parts by mass, based on 100 parts by mass of the total solid content of the curable resin composition.

[0098] <Thermosetting compounds>

[0099] The thermosetting compound used in the curable resin composition of the present embodiment is not particularly limited, and any known and commonly used thermosetting compound may be used. Examples thereof include epoxy resins, triazine resins, phenolic resins, polyester resins, and epoxy resins are preferably used.

[0100] The thermosetting compound may be used alone or in combination of two or more.

[0101] As the epoxy resin, an epoxy resin having two or more epoxy groups in the molecule can be used, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenol type epoxy resin, hydroquinone type epoxy resin, bisphenol fluorene type epoxy resin, naphthalene diol type epoxy resin, bisphenol S type epoxy resin, disulfide type epoxy resin, resorcinol type epoxy resin, hydrogenated bisphenol A type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, alkyl novolac type epoxy resin, etc. can be mentioned.

[0102] Examples of commercially available epoxy resins include "jER828", "jER834", "jER1001", and "jER1004" manufactured by Mitsubishi Chemical Corporation, "EPICLON 840", "EPICLON 850", "EPICLON 1050", and "EPICLON 2055" manufactured by DIC Corporation, Epotohto "YD-011", "YD-013", "YD-127", and "YD-128" manufactured by Nippon Steel Chemicals Co., Ltd., and "Dow Chemical" manufactured by Dow Chemical Co., Ltd. Chemical), Sumi-epoxy "ESA-011", "ESA-014", "ELA-115", "ELA-128" manufactured by Sumitomo Chemical, "AER330", "AER331", "AER661", "AER664" manufactured by Asahi Kasei Industries, "JER152", "JER154" manufactured by Mitsubishi Chemical Corporation, "DEN431", "DEN438" manufactured by Dow Chemical, "EPICLON N-730", "EPICLON N-770", "EPICLON N-780" manufactured by DIC Corporation, and other bisphenol A epoxy resins. N-865", Epotohto "YDCN-701", "YDCN-704" manufactured by Nippon Steel Chemical Materials Co., Ltd., "EPPN-201", "EOCN-1025", "EOCN-1020", "EOCN-104S", "RE-306", "NC-3000H" manufactured by Nippon Kayaku Co., Ltd., Sumi-epoxy "ESCN-195X", "ESCN-220" manufactured by Sumitomo Chemical Co., Ltd., AER manufactured by Asahi Kasei Industries, Ltd.Novolac epoxy resins such as "ECN-235" and "ECN-299"; bisphenol F epoxy resins such as "EPICLON 830" manufactured by DIC Corporation, "jER807" manufactured by Mitsubishi Chemical Corporation, and Epotohto "YDF-170", "YDF-175", and "YDF-2004" manufactured by Nippon Steel Chemical Materials Co., Ltd.; "TECHMORE VG3101L" and other triphenol type epoxy resins; hydrogenated bisphenol A type epoxy resins such as Epotohto "ST-2004", "ST-2007", "ST-3000", "ST-4000D", and "ST-6100" manufactured by Nippon Steel Chemical Materials Co., Ltd.; glycidylamine type epoxy resins such as "jER604" manufactured by Mitsubishi Chemical Corporation, Epotohto "YH-434" manufactured by Nippon Steel Chemical Materials Co., Ltd., and Sumi-epoxy "ELM-120" manufactured by Sumitomo Chemical Industries, Ltd.; hydantoin type epoxy resins; alicyclic epoxy resins such as "Selloxide 2021P" manufactured by Japan Daicel Co., Ltd. and "CY179" manufactured by Huntsman Advanced Materials; "YL-933" manufactured by Mitsubishi Chemical Corporation and "Dow Chemical Company" "TEN Chemical"", "EPPN-501", "EPPN-502" and other trihydroxyphenylmethane type epoxy resins; "YL-6056", "YX-4000", "YL-6121" and other biphenylol type or biphenol type epoxy resins or mixtures thereof manufactured by Mitsubishi Chemical Corporation; "EBPS-200" manufactured by Nippon Kayaku Co., Ltd., "EPX-30" manufactured by ADEKA, "EXA-1514" manufactured by DIC Corporation and other bisphenol S type epoxy resins; "jER157S" and other bisphenol A novolac type epoxy resins manufactured by Mitsubishi Chemical Corporation; "jERYL-931" and other tetrahydroxyphenylethane type epoxy resins manufactured by Mitsubishi Chemical Corporation; "TEPIC" and other heterocyclic epoxy resins manufactured by Nissan Chemical Co., Ltd.; "Blenmer DGT" and other diglycidyl phthalate resins; tetraglycidyl xylenoyl ethane resins such as "ZX-1063" manufactured by Nippon Steel Chemicals Co., Ltd.; naphthyl-containing epoxy resins such as "ESN-190", "ESN-360" manufactured by Nippon Steel Chemicals Co., Ltd., "HP-4032", "EXA-4750", "HP-4700" manufactured by DIC Corporation; epoxy resins having a dicyclopentadiene skeleton such as "HP-7200", "HP-7200H" manufactured by DIC Corporation; "890", "YL6810", "1750", "YX7700", "YX8000", "YX8034", "YX8800" manufactured by Mitsubishi Chemical Corporation. 00", "YL980", "YL983U", "YX7400N", "YX7105", "YX7110B80", "YX7760" and other special functional epoxy resins; "EXA-4816", "EXA-4822", "EXA-4850" series of soft and tough epoxy resins made by DIC Corporation; "CP-50S", "CP-50M" and other methacrylate glycidyl copolymer epoxy resins made by NOF Corporation; and cyclohexylmaleimide and methacrylate glycidyl copolymer epoxy resins, etc.

[0103] The amount of the thermosetting compound to be added is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, based on 100 parts by mass of the total solid content in the curable resin composition.

[0104] <Other added ingredients>

[0105] As required, the curable resin composition of the present embodiment can also be equipped with organic solvents, photopolymerization initiation aids, cyanate compounds, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, close-fitting promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper poison inhibitors, antioxidants, rust inhibitors, acrylic acid, silicon-based surface tension adjusters, organic bentonite, montmorillonite and other thickeners, silicon-based, fluorine-based, polymer-based defoamers and leveling agents, at least any one of silane coupling agents, phosphonates, phosphate derivatives, phosphorus compounds such as phosphazenes compounds, etc., imidazole-based, thiazole-based, triazole-based silane coupling agents, phosphonates, phosphate derivatives, phosphazenes compounds and other flame retardants and other ingredients. These can use substances known in the field of electronic materials.

[0106] [2. Dry film]

[0107] The curable resin composition of the present embodiment can also be set to the form of a dry film having a first film and a resin layer composed of the above-mentioned curable resin composition formed on the first film. The first film in the present embodiment refers to a film that is at least bonded to the resin layer when the resin layer side composed of the above-mentioned curable resin layer formed on the dry film is contacted with a substrate such as a substrate by heating, etc. and laminated and integrally molded. The first film can be peeled off from the resin layer in the process after lamination. In particular, in the present embodiment, it is preferably peeled off from the resin layer in the process after exposure. When the dry film is formed, the curable resin composition of the present embodiment is diluted with the above-mentioned organic solvent and adjusted to an appropriate viscosity, and the first film is coated with a uniform thickness by a comma coater, a blade coater, a lip coater, a rod coater, an extrusion coater, a reverse coating method, a transfer roller coater, a gravure coater, a spray coater, etc., and is usually dried at a temperature of 50 to 130°C for 1 to 30 minutes, so that a film can be obtained. The coating film thickness is not particularly limited, but is usually appropriately selected within the range of 1 to 150 μm, preferably 10 to 60 μm, as the film thickness after drying.

[0108] As the first film, any known film can be used without particular limitation. For example, films made of thermoplastic resins such as polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamide-imide films, polypropylene films, and polystyrene films can be preferably used. Among them, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, and operability. In addition, a laminate of these films can also be used as the first film.

[0109] Furthermore, from the viewpoint of improving mechanical strength, the thermoplastic resin film as described above is preferably a film stretched in a uniaxial direction or a biaxial direction.

[0110] The thickness of the first film is not particularly limited, and can be, for example, 10 μm to 150 μm.

[0111] After forming the resin layer of the curable resin composition of the present embodiment on the first film, further, in order to prevent dust from adhering to the surface of the resin layer, etc., it is preferred that the second film that can be peeled off is laminated on the surface of the resin layer. The second film in the present embodiment refers to a film that is peeled off from the curable resin layer before lamination when the resin layer side of the photosensitive film laminate is contacted with a substrate such as a substrate by heating, etc. As the second film that can be peeled off, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used, as long as the adhesive force between the resin layer and the second film is smaller than the adhesive force between the resin layer and the first film when the second film is peeled off.

[0112] The thickness of the second film is not particularly limited, and can be, for example, 10 μm to 150 μm.

[0113] It should be noted that, in the present embodiment, the curable resin composition of the present embodiment may be applied to the second film and dried to form a resin layer, and the first film may be laminated on the surface thereof. That is, in the present embodiment, as the film to which the curable resin composition of the present invention is applied when manufacturing the dry film, either the first film or the second film may be used.

[0114] [3. Cured product]

[0115] When the curable resin composition of the present embodiment is used to form a cured product, the curable resin composition is applied to the substrate, and the resin layer obtained after the organic solvent is evaporated and dried is exposed (light irradiated), so that the exposed portion (the portion after light irradiation) is cured. Specifically, a contact or non-contact method is used to form a patterned photomask and selectively exposed using active energy rays or directly exposed using a laser direct exposure machine, and the unexposed portion is developed with an alkaline aqueous solution (for example, a 0.3-3% sodium carbonate aqueous solution by mass) to form a solder resist pattern. Furthermore, by heating it at a temperature of about 100 to 180°C to thermally cure it (post-curing), a cured product with excellent transparency, low warping, chemical resistance, and moisture and heat resistance can be formed.

[0116] The curable resin composition of the present embodiment is adjusted to a viscosity suitable for the coating method using, for example, an organic solvent, and after being coated on a substrate by an inkjet method, dip coating, flow coating, roller coating, rod coating, screen printing, curtain coating, or the like, the organic solvent contained in the composition is evaporated and dried at a temperature of about 60 to 100° C., thereby forming a tack free resin layer.

[0117] As the substrate, in addition to printed wiring boards or flexible printed wiring boards with circuits pre-formed with copper or the like, substrates made of materials such as copper-clad laminates for high-frequency circuits made of paper phenolic resin, paper epoxy resin, glass cloth epoxy resin, glass polyimide, glass cloth / non-woven fabric epoxy resin, glass cloth / paper epoxy resin, synthetic fiber epoxy resin, fluororesin-polyethylene-polyphenylene ether (polyphenylene ether), polyphenylene oxide (polyphenylene oxide)-cyanate ester, etc. are also used. All grades (FR-4, etc.) of copper-clad laminates, as well as metal substrates, polyimide films, PET films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, chip boards, etc. can be cited.

[0118] The above-mentioned volatilization drying or thermal curing can be carried out using a hot air circulation drying furnace, IR furnace, hot plate, convection heating furnace, etc. (a device using a heat source with a steam-based air heating method, a method of making the hot air in the dryer contact by convection, and a method of blowing from a nozzle to the support body).

[0119] It should be noted that when the dry film of another embodiment is used, after being bonded to the substrate in a manner that the resin layer contacts the substrate by a laminator, the first film is peeled off, so that the resin layer can be formed on the substrate. Preferably, the dry film is bonded to the substrate under pressurized and heated conditions using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate having a circuit is used, even if there are concave-convex portions on the surface of the circuit substrate, the dry film is closely attached to the circuit substrate, so that bubbles are not mixed in, and the filling property of the concave portion on the surface of the substrate is also improved. The pressurized conditions are preferably about 0.1 to 2.0 MPa, and the heating conditions are preferably 40 to 120°C.

[0120] As an exposure machine for irradiating the above-mentioned active energy rays, any device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, etc. and irradiating active energy rays in the range of 350 to 450 nm can be used. Furthermore, a direct drawing device (for example, a laser direct imaging device that directly draws an image with a laser using CAD data from a computer) can also be used. The lamp light source or laser light source of the direct drawing machine can be a light source with a maximum wavelength in the range of 350 to 410 nm. The exposure amount used to form an image varies depending on the film thickness, etc., and can usually be set to 20 to 1000 mJ / cm 2 , preferably 20 to 800 mJ / cm 2 within the range.

[0121] As the above-mentioned development method, an immersion method, a shower method, a spray method, a brush method, etc. can be used, and as the developer, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, and amines can be used.

[0122] The cured product of the present embodiment, which is obtained by exposing and developing the curable resin composition and then thermally curing it, not only has excellent optical properties, but also has optical properties such as a large total light transmittance, a small haze value, and excellent transparency that is difficult to yellow even when left at 120° C. for 100 hours.

[0123] More specifically, regarding the total light transmittance, the film thickness of the curable resin composition is 10 μm and the cumulative light intensity is 150 mJ / cm 2 The total light transmittance of the cured product obtained by irradiating the active energy ray in a manner, developing and thermally curing is preferably 90% or more, more preferably 92% or more. In addition, the total light transmittance of the cured product after further standing at 120° C. for 100 hours is preferably 85% or more, more preferably 90% or more.

[0124] The b* value used as an indicator of yellowing is calculated based on the film thickness of the curable resin composition being 10 μm and the accumulated light intensity being 150 mJ / cm 2 The b* value of the cured product obtained by irradiating active energy rays in a manner, developing and thermally curing is preferably 1.5 or less, and more preferably 1.2 or less. In addition, when the cured product is further placed at 120°C for 100 hours, the b* value of the cured product after placement is preferably 2.0 or less, and more preferably 1.5 or less. In particular, when the cured product is placed at 120°C for 100 hours, the change in the b* value of the cured product before and after placement (Δb*) is preferably 1.5 or less, and more preferably 1.0 or less.

[0125] Furthermore, regarding the haze value, the film thickness of the curable resin composition is 10 μm and the accumulated light intensity is 150 mJ / cm 2 The haze value of the cured product obtained by irradiating the cured product with active energy rays in a manner and developing and heat curing is preferably 2.0 or less, and more preferably 1.5 or less. In addition, when the cured product is further placed at 120°C for 100 hours, the haze value of the cured product after placement is preferably 5.0 or less, and more preferably 3.5 or less. In particular, when the cured product is placed at 120°C for 100 hours, the change in the haze value of the cured product before and after placement is preferably 4.0 or less, and more preferably 3.0 or less.

[0126] [4. Printed wiring board]

[0127] The curable resin composition or the resin layer of the dry film of this embodiment can be suitably used to form a surface protective film such as a solder resist on a printed wiring board. In addition, the curable resin composition of this embodiment can also be used as an interlayer insulating layer of a multilayer printed wiring board.

[0128] By applying the curable resin composition or the resin layer of the dry film of the present embodiment to a substrate of a printed wiring board and curing it, a printed wiring board having a cured product having transparency, low warpage, chemical resistance, and excellent moisture and heat resistance can be produced.

[0129] Example

[0130] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples.

[0131] [1. Preparation of curable resin composition]

[0132] An alkali-soluble resin, a urethane (meth)acrylate resin, a (meth)acrylate monomer, a photopolymerization initiator, an amine curing agent, an additive, and an epoxy resin were mixed so that the content of each component became the amount shown in Table 1 (unit: parts by mass), pre-mixed with a stirrer, and then kneaded with a three-roll mill to prepare curable resin compositions of Examples 1 to 6 and Comparative Examples 1 to 5.

[0133] In addition, unless otherwise specified, the values ​​of the blending amounts in Table 1 represent parts by mass.

[0134] The details of the components described in Table 1 are as follows. In addition, the blending amount of each component is a value based on solid content.

[0135] <Alkali-soluble resin>

[0136] Cyclomer P (AZA) Z250 (manufactured by Daicel-Allnex): a carboxyl group-containing acrylic copolymer having an alicyclic skeleton.

[0137] VB-5305 (manufactured by Mitsubishi Rayon Co., Ltd.): a carboxyl group-containing acrylic acid-styrene copolymer.

[0138] DAUA-167 (manufactured by Kyoeisha Chemical Co., Ltd.): a urethane resin containing an acryloyl group and a carboxyl group.

[0139] UXE-3000 (manufactured by Nippon Kayaku Co., Ltd.): a bisphenol A-type urethane acrylate resin containing a carboxyl group.

[0140] <Urethane (meth)acrylate resin>

[0141] UA-7100 (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.): a polyether skeleton bifunctional urethane acrylate resin.

[0142] <(Meth)acrylate monomer>

[0143] BPE-900 (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.): ethoxylated bisphenol A dimethacrylate.

[0144] <Photopolymerization initiator>

[0145] Irgacure OXE04 (manufactured by BASF Japan): 1-pentanone, 1-[4-[[4-(2-benzofuranylcarbonyl)phenyl]thio]phenyl]-4-methyl, 1-(o-acetoxime).

[0146] Omnirad TPO H (manufactured by IGM Resins BV): 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0147] Irgacure OXE02 (manufactured by BASF Japan): ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(o-acetyl oxime)

[0148] Ominirad 379 (manufactured by IGM Resins BV): 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one.

[0149] <Amine curing agent>

[0150] Melamine slurry

[0151] Mix the organic filler and the organic solvent and adjust the particle size using a roll mill or a bead mill. Average particle size (D50) ≤ 1.0 μm

[0152] ·Benzotriazole (manufactured by Yamato Chemical Co., Ltd.)

[0153] Since benzotriazole is in powder form and is dissolved in the curable resin composition, it is processed to have an average particle size (D50) of 1 μm or less.

[0154] Melamine: 1,3,5-triazine-2,4,6-triamine (average particle size (D50)>2 μm).

[0155] <Epoxy resin>

[0156] YX8034 (manufactured by Mitsubishi Chemical Corporation): hydrogenated bisphenol A type epoxy resin.

[0157]

[0158] [2. Preparation of dry film and cured product for evaluation and evaluation of properties of cured product for evaluation]

[0159] <Preparation of dry film for evaluation>

[0160] The curable resin composition ink prepared according to the blending amount shown in Table 1 was applied to a 25 μm thick PET film (E-5041 manufactured by Toyobo Co., Ltd.) using a coater and dried in a hot air circulation drying oven at 80° C. for 30 minutes to prepare a dry film having a film thickness of 10 μm.

[0161] <Total light transmittance>

[0162] A soda lime glass substrate having a glass thickness of 1 mm was washed with alcohol and dried, and the above-obtained dry film for testing was laminated and subjected to a 150 mJ / cm2 irradiation with EXP-2960 manufactured by ORC MANUFACTURING CO., LTD. 2 The entire surface was exposed with an exposure amount of 100%. After developing with a 1wt% Na2CO3 aqueous solution at 30°C for 60 seconds under a spray pressure of 0.1MPa, a cured product for evaluation was obtained by heating at 130°C for 60 minutes. For the obtained test cured product, the total light transmittance was measured respectively with 1mm soda lime glass as a reference. The total light transmittance was measured in accordance with JIS K 7361-1 using a UV-visible spectrophotometer V-670EX (manufactured by JASCO Corporation). The measurement results are shown in Table 2.

[0163] <Haze value>

[0164] The haze value of the coating film of the above-mentioned cured product for evaluation was measured with respect to 1 mm soda lime glass as a reference. The haze value was measured using a haze meter (Haze Meter NDH 7000II manufactured by Nippon Denshoku Industries Co., Ltd.). The measurement results are shown in Table 2.

[0165] <b* value>

[0166] The transmitted light of the evaluation cured product was measured using a spectrophotometer CM-5 (manufactured by Konica Minolta Japan Ltd.), and b* was numerically expressed using the CIE 1976 colorimetric system with 1 mm soda lime glass as a reference.

[0167] <High temperature storage test>

[0168] The obtained cured product for evaluation was placed in a box oven at 120° C. for 100 hours. After the high temperature placement test, the total light transmittance, haze value, and b* value were measured by the same method as above.

[0169] <Low warpage>

[0170] A contact exposure machine EXP-2960 manufactured by ORC MANUFACTURING CO., LTD. was used at 150 mJ / cm 2 The substrate obtained by laminating the above-obtained dry film for evaluation on a polyimide film "Kapton 100H" (manufactured by DuPont Toray Co., Ltd.) with a thickness of 25 μm was exposed to the entire surface, and developed with a 1 wt% Na2CO3 aqueous solution at 30°C for 60 seconds under a spray pressure of 0.1 MPa, and then cured by heating at 130°C for 60 minutes. The obtained substrate was cut into 50 mm×50 mm pieces, and the height of the warpage at the four corners was measured, and the total value was calculated and evaluated according to the following judgment criteria. The results are shown in Table 2.

[0171] ⊚: The total value of the warping heights at the four corners is less than 5 mm.

[0172] ○: The total value of the warpage heights of the four corners is 5 mm or more and less than 10 mm.

[0173] ×: The total value of the warping heights at the four corners is 10 mm or more.

[0174] <Chemical resistance>

[0175] The substrate was prepared by the same method as described in the above-mentioned low warpage. The substrate was immersed in propylene glycol methyl ether acetate at room temperature for 30 minutes, and then taken out and dried. The state of the coating film was visually confirmed for the dried substrate, and evaluated according to the following criteria. The results are shown in Table 2.

[0176] ○: The state of the coating film did not change.

[0177] ×: The coating film floated and peeled off.

[0178] <Moisture and heat resistance>

[0179] The dry film for evaluation obtained above was laminated on a 1 mm thick soda lime glass and exposed at 150 mJ / cm2 using a contact exposure machine EXP-2960 manufactured by ORC MANUFACTURING CO., LTD. 2The solder resist pattern was exposed to an exposure amount of , and a 1wt% Na2CO3 aqueous solution at 30°C was developed for 60 seconds under a spray pressure of 0.1MPa to obtain a solder resist pattern. The substrate was heated at 130°C for 60 minutes for curing. The obtained substrate was placed in a constant temperature and humidity chamber at 85°C and 85%RH, taken out after 240 hours, and the haze was measured based on 1mm soda lime glass. The haze value was measured using a haze meter (Haze Meter NDH 7000II manufactured by Nippon Denshoku Industries Co., Ltd.) and evaluated according to the following criteria. The results are shown in Table 2.

[0180] ◎: Haze is less than 3.5.

[0181] ○: Haze is 3.5 or more and less than 5.

[0182] △: The haze is 5 or more and less than 10.

[0183] ×: The haze is 10 or more.

[0184] Table 2

[0185]

[0186] The coating films for evaluation produced using the curable resin compositions of Comparative Examples 1 and 2 had large b* values, and the cured products for evaluation turned yellow.

[0187] On the other hand, from Tables 1 and 2, the components of the curable resin compositions of Examples 1 and 5 and Comparative Examples 1 and 2 and the properties of the cured products for evaluation thereof are compared. It can be seen that the cured products for evaluation prepared using the curable resin compositions containing Irgacure OXE04 (Example 1) or Omnirad TPO H (Example 5) as the photopolymerization initiator have better total light transmittance and b* value in the cured products for evaluation than the cured products for evaluation prepared using the curable resin compositions containing Irgacure OXE02 (Comparative Example 1) or Omnirad 379 (Comparative Example 2) as the photopolymerization initiator. In addition, the total light transmittance, haze value and b* value in the cured products for evaluation after the high temperature storage test are better.

[0188] The evaluation cured product made of the curable resin composition of Comparative Example 3 containing an amine curing agent having an average particle size greater than 1 μm has poor moisture and heat resistance, and the total light transmittance of the evaluation cured product and after the high-temperature placement test is small, and the haze value is large. In addition, the evaluation cured product made of the curable resin composition of Comparative Example 4 not containing an amine curing agent is not sufficiently cured under the curing temperature condition of 130° C., so the chemical resistance and moisture and heat resistance are poor, and the haze value and b* value of the evaluation cured product after the high-temperature placement test become large.

[0189] In contrast, according to Tables 1 and 2, the components of the curable resin compositions of Examples 1 and 6 and Comparative Example 3 and the properties of their evaluation cured products are compared. It can be seen that for the evaluation cured products made from the curable resin compositions of Examples 1 and 6 containing an amine-based curing agent having an average particle size of less than 1 μm, compared with the evaluation cured product made from the curable resin composition of Comparative Example 3 containing an amine-based curing agent having an average particle size of more than 1 μm, both the total light transmittance and the haze value in the evaluation cured products and the evaluation cured products after the high-temperature storage test give good results.

[0190] [3. Measurement of absorbance change at a wavelength of 410 nm before and after curing of a test curable resin composition containing a photopolymerization initiator]

[0191] <Preparation of curable resin composition for test>

[0192] An alkali-soluble resin, an acrylate monomer, and a photopolymerization initiator were blended so that the contents of the components were the amounts shown in Table 3 (unit: parts by mass), and mixed with a stirrer to prepare test curable resin compositions of Examples 7 and 8 and Comparative Examples 7 and 8.

[0193] It should be noted that, unless otherwise specified, the values ​​of the blending amounts in Table 3 represent parts by mass.

[0194] The details of the components described in Table 3 are as follows.

[0195] <Alkali-soluble resin>

[0196] Cyclomer P (AZA) Z250 (manufactured by Daicel-Allnex): a carboxyl group-containing acrylic copolymer having an alicyclic skeleton.

[0197] <Acrylate Monomer>

[0198] DPGDA (manufactured by Daicel-Allnex): dipropylene glycol diacrylate.

[0199] <Photopolymerization initiator>

[0200] Irgacure OXE04 (manufactured by BASF Japan): 1-pentanone, 1-[4-[[4-(2-benzofuranylcarbonyl)phenyl]thio]phenyl]-4-methyl, 1-(o-acetoxime).

[0201] Omnirad TPO H (manufactured by IGM Resins BV): 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0202] Irgacure OXE02 (manufactured by BASF Japan): ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(o-acetoxime).

[0203] Ominirad 379 (manufactured by IGM Resins BV): 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one.

[0204] <Measurement of absorbance change before and after curing>

[0205] The test curable resin compositions of Examples 7 and 8 and Comparative Examples 7 and 8 were applied to a glass having a thickness of 1 μm using a bar coater (manufactured by Matsuo Industries, Ltd.) so as to have a film thickness of 4 μm, and dried in a box oven at 90° C. for 30 minutes. The absorbance of the prepared coating film at a wavelength of 410 nm was measured using an ultraviolet-visible-infrared spectrophotometer V-670 (manufactured by JASCO Corporation).

[0206] Then, a high pressure mercury lamp was used to provide a cumulative light intensity of 4000 mJ / cm 2 The active energy rays were irradiated in a manner to perform photocuring. The absorbance of the obtained cured product at a wavelength of 410 nm was measured using an ultraviolet-visible-infrared spectrophotometer V-670, and the change rate of the absorbance before and after photocuring was calculated using the following formula. The results are shown in Table 3.

[0207] Absorbance change rate (%) = [(absorbance at a wavelength of 410 nm after photocuring) - (absorbance at a wavelength of 410 nm before photocuring)] / (absorbance at a wavelength of 410 nm before photocuring) × 100

[0208] Table 3

[0209]

[0210] As can be seen from Table 3, the change rate of the absorbance at a wavelength of 410 nm before and after photocuring of the test curable resin compositions of Examples 7 and 8 was 100% or less.

[0211] On the other hand, it is found that the change rate of the absorbance at a wavelength of 410 nm before and after photocuring of the test curable resin compositions of Comparative Examples 7 and 8 clearly exceeds 100%.

[0212] As can be seen from Tables 1 to 3, by containing Irgacure OXE04 or Omnirad TPO H as a photopolymerization initiator in which the change rate of absorbance at a wavelength of 410 nm before and after photocuring of the test curable resin composition does not exceed 100%, when the curable resin composition is cured, a cured product having good values ​​of total light transmittance, haze value and b* value and excellent low warpage, chemical resistance and moisture-heat resistance can be provided.

Claims

1. A solidified product, characterized in that: The cured product is obtained by curing a curable resin composition containing (A) an alkali-soluble resin, (B) a photopolymerization initiator, and (C) an amine-based curing agent. The cured product has a b* value of 1.5 or less in the CIE L*a*b* colorimetric system and a total light transmittance of 90% or more.

2. The cured product according to claim 1, wherein The average particle size of the (C) amine curing agent is 1 μm or less.

3. The cured product according to claim 1, wherein The curable resin composition further includes a urethane (meth)acrylate resin.

4. A printed wiring board, wherein: The printed wiring board comprises the cured product according to claims 1 to 3.

5. A curable resin composition, characterized in that The present invention is a curable resin composition comprising (A) an alkali-soluble resin, (B) a photopolymerization initiator, and (C) an amine curing agent. The photopolymerization initiator (B) was used in a test curable resin composition consisting of 100 parts by mass of Cyclomer P(ACA) Z250, 20 parts by mass of dipropylene glycol diacrylate, and 1.2 parts by mass of the photopolymerization initiator (B) to obtain a film thickness of 4 μm and a cumulative light intensity of 4000 mJ / cm 2 (B) a photopolymerization initiator having a rate of change in absorbance at a wavelength of 410 nm before and after curing of 100% or less when irradiated with active energy rays in a manner to cure the photopolymerization initiator, (C) The average particle size of the amine-based curing agent is 1 μm or less.

6. A dry film, wherein: The dry film includes: a first film; and a resin layer composed of a dry coating film of the curable resin composition according to claim 5 formed on the first film.

Citation Information

Patent Citations

  • Process for preparing butyl-p-benzoylbenzoates

    EP0000502A1

  • 1-Methylisoguanosin, processes and intermediates for its preparation, its pharmaceutical compositions and their preparation

    EP0000770A2

  • Liquid level measuring device

    EP0001050A1