Composite hydrogel, preparation method thereof and functional dressing

By combining the polyvinyl alcohol cycle freeze-thawing method with the physical cross-linking method of bacterial cellulose and chitosan oligosaccharide, a composite hydrogel with multiple biological functions is prepared, which solves the mechanical properties and self-healing capabilities of existing hydrogel dressings. deficiencies, achieving efficient wound healing and wide application.

CN118787776APending Publication Date: 2024-10-18GUANGDONG NO 2 PROVINCIAL PEOPLES HOSPITAL
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410767055.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing hydrogel dressings have limitations in mechanical properties, self-healing capabilities, and versatility. It is difficult to combine good adhesion, frost resistance, toughness, elasticity, and multiple biological functions. They are also costly and have limited applications. due to the complex wound microenvironment.

Method used

Using polyvinyl alcohol (PVA) cycle freeze-thaw method-physical cross-linking method, combined with bacterial cellulose and chitosan oligosaccharide, through hydrogen bond cross-linking and metal-organic interaction, we prepared a product with antibacterial, anti-inflammatory, antioxidant, and promotion properties. Composite hydrogels with cell proliferation and migration properties related to angiogenesis and skin healing.

Benefits of technology

It achieves good adhesion, anti-freeze, toughness, elasticity and self-healing properties of the composite hydrogel. It also has excellent comprehensive properties of antibacterial, anti-inflammatory, antioxidant and promotion of skin healing, reduces production costs and is suitable for a variety of applications. types of wounds, broadening the scope of clinical application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118787776A_ABST
    Figure CN118787776A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hydrogel dressings, in particular to composite hydrogel and a preparation method thereof and functional dress.The preparation method of the composite hydrogel comprises the following steps that chitosan oligosaccharide and bacterial cellulose are mixed and added into a first solvent for first dispersion, and first mixed material liquid is prepared; the first solvent comprises glycerol and water, and optionally comprises zinc ions; polyvinyl alcohol is added into the first mixed material liquid for second dispersion, and second mixed material liquid is prepared; taking the second mixed material liquid, and heating while carrying out third dispersion to form the gel; the gel is subjected to circulating freeze thawing, and the composite hydrogel is obtained. The composite hydrogel and dressing provided by the invention have good adhesion, freezing resistance, toughness and elasticity and self-repairing performance, and also have excellent properties of resisting bacteria, resisting inflammation, resisting oxidation, promoting angiogenesis, promoting proliferation and migration of skin healing related cells and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of hydrogel dressings, and in particular to a composite hydrogel and a preparation method thereof and a functional dressing. Background Art

[0002] Hydrogel dressings are innovative materials used in the medical field, especially in wound management. They are usually made of natural or synthetic polymers and can absorb large amounts of fluid while maintaining their structure and shape. Due to their unique physical and chemical properties, hydrogel dressings have shown great potential in promoting wound healing, reducing pain and preventing infection.

[0003] The mechanical properties of hydrogel dressings are an important factor in determining their application effect. An ideal hydrogel dressing should have good mechanical strength, appropriate ductility and compressibility, and excellent adhesion so that it can fit the wound closely and provide effective protection and treatment.

[0004] Functional hydrogel dressings are a type of gel material with special functions such as anti-oxidation, antibacterial or promoting wound repair. With the increasing clinical demand for skin wound repair strategies, the development of functional hydrogel dressings has also been steadily progressing.

[0005] Growth factors play an indispensable role in the skin healing process. New hydrogel carriers carrying growth factors can significantly shorten the wound healing time. However, this design process is often complicated and the preparation is cumbersome, which limits its large-scale promotion. As a new and promising wound repair treatment method, stem cells and their derivatives have shown excellent skin healing performance, but their cost is high and the treatment effect is easily disturbed by the wound microenvironment, especially in cases of infection, excessive inflammation and angiogenesis disorders. Their application is relatively limited. For infectious wounds, drug delivery hydrogel materials can slowly release antibiotics to the wound surface, thereby promoting wound repair. However, the biological properties of this type of hydrogel material are single, and it is inevitable to increase the risk of bacterial resistance, which limits its clinical application value.

[0006] Therefore, developing a functionalized hydrogel dressing with good mechanical properties, adhesion properties, and self-healing ability, which is suitable for various types of wounds, has important clinical translation value. Summary of the invention

[0007] Based on this, one or more embodiments of the present application provide a composite hydrogel, a preparation method thereof and a functional dressing, wherein the composite hydrogel has good adhesion, frost resistance, toughness, elasticity and self-repairing properties, and also has comprehensive excellent properties of antibacterial, anti-inflammatory, antioxidant, angiogenesis-promoting and skin healing-related cell proliferation and migration.

[0008] The technical solution of this application includes the following contents:

[0009] A method for preparing a composite hydrogel comprises the following steps:

[0010] The chitosan oligosaccharide and the bacterial cellulose are mixed and added into a first solvent for first dispersion to obtain a first mixed liquid; the first solvent includes the glycerol and the water, and optionally includes the zinc ions;

[0011] Adding the polyvinyl alcohol into the first mixed liquid for second dispersion to obtain a second mixed liquid;

[0012] Taking the second mixed liquid, and heating it while performing the third dispersion to obtain the gel;

[0013] The gel is subjected to cyclic freeze-thaw cycles to obtain the composite hydrogel.

[0014] A composite hydrogel prepared by the preparation method described above.

[0015] A functional dressing, the material of which includes the composite hydrogel or the composite hydrogel prepared by the preparation method.

[0016] This application is based on the polyvinyl alcohol (PVA) cyclic freeze-thaw method-physical crosslinking method, and bacterial cellulose (BC) is added to the system to prepare PVA-BC hydrogel with adjustable mechanical properties, and ingredients such as chitosan oligosaccharides (COS) are introduced to improve the stability of the hydrogel network through multiple bonding and give it multiple biological functions such as antibacterial, anti-inflammatory, antioxidant, angiogenesis promotion, and skin healing related cell proliferation and migration. In addition, mixing glycerol into the system can provide more hydrogen bonding sites to enhance the stability of the hydrogel network on the one hand, and glycerol gives the hydrogel dressing excellent antifreeze properties on the other hand, enabling it to withstand low temperature environments and broaden its scope of clinical use.

[0017] The composite hydrogel of the present application can be used to meet the biological function requirements of various types of wounds. The preparation method is simple, green and environmentally friendly, the raw materials are easily available, and the cost is low, providing a hydrogel dressing material with wide application value and economic friendliness. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Fourier transform infrared spectrum analysis diagram of the composite hydrogel PB-1, PBC-1, PB-2, PBC-2, PB-3, PBC-3 and the raw materials for preparation of the present application;

[0019] Figure 2 The Fourier transform infrared spectrum analysis diagram of the composite hydrogel PB-3, PBC-3 and PBCZ of the present application and their respective preparation raw materials;

[0020] Figure 3 The EDS chemical element analysis results of the composite hydrogels PB-3, PBC-3 and PBCZ of the present application;

[0021] Figure 4 The comparison results of the viscoelastic properties of the composite hydrogels PBC-1, PBC-2 and PBC-3 of the present application;

[0022] Figure 5 Schematic diagram of the macroscopic self-healing performance test of the composite hydrogel PBC-3 of the present application;

[0023] Figure 6 The comparison results of the tensile and compressive properties of the composite hydrogels PBC-1, PBC-2, and PBC-3 of the present application;

[0024] Figure 7 This is a schematic diagram of characterizing the macroscopic adhesion performance of the composite hydrogel PBC-3 of the present application at different joint sites and on different material surfaces;

[0025] Figure 8 The swelling performance comparison results of the composite hydrogels PBC-1, PBC-2 and PBC-3 of the present application are shown;

[0026] Fig. 9 The results of the antibacterial colony test and the antibacterial growth inhibition curve comparison of the composite hydrogels PB-3, PBC-3, and PBCZ of the present application are shown;

[0027] Fig.10 The comparison results of the antioxidant performance of the composite hydrogels PB-3, PBC-3, and PBCZ in the DPPH free radical scavenging rate of the present application;

[0028] Fig.11 The comparison results of the biocompatibility of the composite hydrogels PB-3, PBC-3, and PBCZ of the present application;

[0029] Fig.12 The comparison results of the composite hydrogels PB-3, PBC-3, and PBCZ of the present application in promoting the migration of NIH-3T3 cells;

[0030] Fig.13 The results are compared on the ability of the composite hydrogels PB-3, PBC-3 and PBCZ of the present application to promote HUVEC cell migration;

[0031] Fig.14 For this application, RT-qPCR was used to verify the comparative results of the expression of skin healing related genes such as anti-inflammatory, angiogenesis and connective tissue growth factor of composite hydrogels PB-3, PBC-3 and PBCZ;

[0032] Fig.15 The comparison results of the composite hydrogels PB-3, PBC-3 and PBCZ of the present application in promoting the closure of rat skin wounds;

[0033] Fig.16 The comparison results of HE staining analysis of the composite hydrogels PB-3, PBC-3 and PBCZ in the present application in promoting rat skin healing;

[0034] Fig.17 Comparative results of Masson staining analysis of the composite hydrogels PB-3, PBC-3, and PBCZ of the present application in promoting rat skin healing. DETAILED DESCRIPTION

[0035] The present application will be further described below in conjunction with the embodiments and examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. In addition, it should be understood that after reading the content taught in the present application, those skilled in the art may make various changes or modifications to the present application, and these equivalent forms also fall within the protection scope of the claims attached to the present application.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0037] the term:

[0038] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0039] The terms "and / or", "or / and", and "and / or" used in this article include any one of two or more related listed items, and also include any and all combinations of related listed items, and the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in this application, the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B.

[0040] In the present application, "further" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0041] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0042] In the present application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges included therein.

[0043] In the present application, weight may be μg, mg, g, kg or other mass units known in the chemical industry.

[0044] Functional hydrogel dressings are materials with broad application prospects in the field of wound treatment. Due to their unique physical and chemical properties, they can effectively promote wound healing, reduce the risk of infection, and improve the quality of life of patients.

[0045] Functional hydrogel dressings are usually modified to have at least one of the following properties: (1) Good biocompatibility: Hydrogel materials are usually composed of highly biocompatible polymers, such as chitosan, cellulose, sodium alginate and silk protein, which are friendly to human tissue and are not easy to cause immune response. (2) High water content: The three-dimensional network structure of hydrogel can retain a large amount of water inside, which helps to maintain a moist environment for the wound and promote cell growth and migration. (3) Mechanical strength: Hydrogels have a certain mechanical strength, which can avoid the replacement cost caused by external force causing hydrogel rupture and damage, and they cover the wound surface and can effectively isolate external physical damage. (4) Degradability: The degradation rate of hydrogels can be adjusted according to the healing needs of different wounds to adapt to different clinical applications. (5) Multifunctionality: By adding different functional substances, such as metal ions, biopolysaccharides, photothermal materials, antibacterial agents, etc., hydrogels can build a good microenvironment for the wound surface through their antibacterial, anti-inflammatory and antioxidant biological properties, and promote tissue regeneration from multiple angles such as cell proliferation, migration and skin remodeling.

[0046] Functional hydrogel dressings have a wide range of applications, including the following aspects: (1) Antibacterial and anti-inflammatory: By adding antibacterial agents or utilizing photodynamic and photothermal effects, functional hydrogel dressings can effectively inhibit or kill bacteria in wounds and reduce the risk of infection. (2) Promote wound healing: Some functional hydrogels can release growth factors or drugs, stimulate cell proliferation and the formation of new blood vessels, and accelerate the wound healing process. (3) Drug delivery system: Hydrogels can be used as drug delivery systems to control the release rate of drugs, achieve local treatment, and reduce systemic side effects. (4) Self-repair ability: Some hydrogels have self-repair functions and can automatically restore their structure and function after damage, extending the use time of the dressing. (5) Good tissue adhesion: The tissue adhesion of hydrogels can achieve stable adhesion to wounds in different parts, so as to improve the patient's experience and is widely used in clinical practice.

[0047] In recent years, researchers have made significant progress in the research of functional hydrogel dressings. For example, by combining metal ions, nanoparticles and bioactive glass, polysaccharide polymer-based hydrogels with different functions have been developed. These hydrogels not only have antibacterial and anti-inflammatory properties, but also can promote wound healing and tissue regeneration. However, it cannot be ignored that these hydrogels have certain limitations in improving physical properties. It is difficult to combine excellent physical properties such as self-repair, adhesion, and mechanical strength with multiple biological functions required for clinical use, resulting in the existing hydrogels on the market. The performance is quite single and cannot cope with the complexity of different clinical wounds. The mechanical properties of hydrogels can be significantly improved by chemical cross-linking, but cross-linking agents are often required, and their potential biological toxicity affects the biocompatibility of biomaterials. Hydrogels carrying stem cells and their derivatives can promote wound healing. However, their production cost is expensive, and the performance requirements for hydrogel carriers are high. In actual application, the effect may be affected by the harsh microenvironment of the wound, so the application is limited.

[0048] In one aspect of the present application, a method for preparing a composite hydrogel by a cyclic freeze-thaw method using hydrogen bond crosslinking is provided. This method can physically introduce bioactive polysaccharides and optionally added zinc ions into the hydrogel system without using additional chemical crosslinking agents. This crosslinking method not only improves the mechanical strength of the composite hydrogel, but also gives it the ability to self-repair. At the same time, this physical preparation method is more environmentally friendly than chemical crosslinking agents, and can better maintain the activity and safety of the original bioactive substances.

[0049] The composite hydrogel prepared by the preparation method of the composite hydrogel of the present application has good adhesion, frost resistance, toughness, elasticity and self-repairing properties, and also has comprehensive excellent properties of antibacterial, anti-inflammatory, antioxidant, promoting angiogenesis and promoting the proliferation and migration of skin healing related cells.

[0050] Bacterial cellulose has very high mechanical strength and a unique three-dimensional network structure. Compared with pure polyvinyl alcohol-based hydrogels, the addition of bacterial cellulose helps to improve the overall mechanical properties of the hydrogel, enhance the structural stability and durability of the hydrogel, and make it more suitable for application scenarios that require high strength and high stability. Through the rational combination of bacterial cellulose in polyvinyl alcohol, chitosan oligosaccharides and optionally added zinc ions, the mechanical properties and other functional properties of the hydrogel can be finely controlled. At the same time, chitosan oligosaccharides have positively charged amino groups and abundant hydroxyl groups, and the synergistic metal zinc ions can provide a synergistic biomodification strategy for hydrogels. The two also further consolidate the cross-linking of the hydrogel through hydrogen bond cross-linking and metal-organic interactions in the hydrogel, enhance the hydrogel network structure, and realize the design of a new type of multifunctional integrated biomaterial.

[0051] In one embodiment, the preparation method of the composite hydrogel comprises the following steps:

[0052] Chitosan oligosaccharide and bacterial cellulose are mixed and added into a first solvent for first dispersion to obtain a first mixed liquid; the first solvent includes glycerol and water, and optionally includes zinc ions;

[0053] Adding polyvinyl alcohol to the first mixed liquid for second dispersion to obtain a second mixed liquid;

[0054] Taking the second mixed liquid, heating it while performing the third dispersion to obtain a gel;

[0055] The gel was subjected to cyclic freeze-thaw cycles to obtain a composite hydrogel.

[0056] In one embodiment, the second mixed liquid includes 10 wt % to 20 wt % of polyvinyl alcohol, 0.1 wt % to 0.3 wt % of bacterial cellulose and 1 wt % to 3 wt % of chitosan oligosaccharide, based on the total weight percentage of the second mixed liquid being 100 wt %;

[0057] Optionally, 0.2 wt% to 0.8 wt% of zinc ions are further included.

[0058] Optionally, in the second mixed liquid, the weight ratio of polyvinyl alcohol, the bacterial cellulose and the chitosan oligosaccharide is 1:(0.005-0.02):(0.1-0.15).

[0059] Preferably, in the second mixed liquid, the weight ratio of polyvinyl alcohol, the bacterial cellulose and the chitosan oligosaccharide is 1:

[0060] (0.0067~0.02):0.133.

[0061] In one embodiment, the first dispersion comprises stirring at 300 r / min to 500 r / min for 10 min to 20 min.

[0062] In one embodiment, the rate of adding polyvinyl alcohol into the first mixed liquid is 1 g / min to 1.5 g / min.

[0063] In one embodiment, the second dispersion comprises stirring at 300 r / min to 500 r / min for 5 min to 15 min.

[0064] In one embodiment, in the step of heating while performing the third dispersion, the third dispersion includes stirring at 100 r / min to 300 r / min and heating at a temperature of 90° C. to 100° C. Preferably, the duration of this step is until the second mixed liquid forms a gel.

[0065] In one embodiment, the freeze-thaw cycle procedure includes: freezing at -30°C to -20°C for 5h to 7h, then transferring to room temperature for thawing, and then thawing at room temperature for 1h to 3h, and the number of cycles is at least three times. Preferably, the freezing time is 6h to 7h, and the thawing time is 2h to 3h.

[0066] In one embodiment, the weight ratio of glycerol to water in the first solvent is (0.7-0.8):1; for example, the weight ratio of glycerol to water can be 0.7:1, 0.75:1, 0.8:1, etc. It can be understood that the ratio of glycerol to water as a solvent is close to (0.7-0.8):1, more preferably close to 3:4, and a weighing error is allowed, and the error value can be within ±10%, and more preferably within ±5%.

[0067] In another aspect of the present application, a composite hydrogel prepared by the preparation method described in any of the above technical solutions is provided.

[0068] In another aspect of the present application, a functional dressing is provided, the material of which includes the composite hydrogel described in any of the above technical solutions.

[0069] Biofunctionalized hydrogel dressings give hydrogels the ability to promote wound healing by adding growth factors, stem cells and their derivatives, biopolysaccharides, bioactive glass, and photothermal effect materials. However, growth factor and stem cell-loaded hydrogels have high requirements for their carriers themselves, and the actual treatment effect will also be affected by the complex microenvironment of the wound; in addition, the photothermal effect can kill common bacterial tumor cells on the wound through non-antibiotic mechanisms, but it will inevitably damage the surrounding adjacent healthy cells and cause certain side effects to the body; biopolysaccharides have a significant promoting effect on wound healing, but some have functional limitations and poor solubility, which makes it difficult to utilize and transform them in a simple way. Finally, balancing mechanical strength and self-healing properties is also a research hotspot where it is difficult to improve the physical properties of hydrogels.

[0070] In one embodiment, the functional dressing has at least one of the following characteristics:

[0071] (1) Adhesion;

[0072] (2) Freeze resistance;

[0073] (3) Toughness and elasticity;

[0074] (4) Self-healing performance;

[0075] (5) Antibacterial, the antibacterial bacteria include Staphylococcus aureus, Pseudomonas aeruginosa and Escherichia coli;

[0076] (6) Anti-inflammatory;

[0077] (7) Antioxidant;

[0078] (8) promoting angiogenesis; and

[0079] (9) Promote skin healing.

[0080] In one embodiment, the functional dressing has excellent physical and chemical properties and self-healing ability, and also has the above-mentioned comprehensive excellent properties such as antibacterial, cell proliferation promotion, cell migration promotion, anti-inflammatory, antioxidant, angiogenesis promotion and promotion of skin tissue repair related gene expression.

[0081] Optionally, the functional dressing with antimicrobial properties targets bacteria including Staphylococcus aureus, Pseudomonas aeruginosa and Escherichia coli.

[0082] The following are some specific embodiments.

[0083] For experimental parameters not specified in the following specific embodiments, reference is made to the instructions given in the present application document, and reference may also be made to experimental manuals in the art or other experimental methods known in the art, or to experimental conditions recommended by manufacturers.

[0084] The raw materials and reagents involved in the following specific examples can be obtained from commercial sources, or can be prepared by those skilled in the art according to known methods.

[0085] in:

[0086] The bacterial cellulose dispersion is a water dispersion of bacterial cellulose with a solid content of 0.75w%;

[0087] Polyvinyl alcohol was purchased from Aladdin, product number P139540 (500 g);

[0088] Chitosan oligosaccharide was purchased from Aladdin, product number C302935 (100 g);

[0089] Glycerol was of analytical grade.

[0090] 1. Preparation of composite hydrogel

[0091] Example 1

[0092] This embodiment provides a method for preparing a PVA-BC-COS hydrogel (PBC-1). The raw materials and their amounts are shown in Table 1. The preparation steps are as follows:

[0093] (1) Pour the aqueous dispersion of oligosaccharide (COS) and bacterial cellulose (BC dispersion) into a clean beaker containing glycerol and water, with the mass ratio of glycerol to water being 3:4. Then, stir the mixed system in the beaker with a magnetic stirrer for 15 min (400 r / min) at room temperature to fully dissolve and disperse the components, remove bubbles by ultrasonic dispersion, and further mix to obtain a first mixed liquid.

[0094] (2) Add polyvinyl alcohol (PVA) to the first mixed liquid and stir at room temperature for 10 min (400 r / min) to obtain a second mixed liquid; then seal the beaker with plastic wrap and a rubber ring and place in a high-temperature heating magnetic stirrer and stir until completely dissolved. The temperature of the heating magnetic stirrer is slowly increased to 95°C and the speed is 200 r / min.

[0095] (3) The completely dissolved hydrogel mixture system was taken out and collected in a centrifuge tube, and the bubbles generated by the dissolution of polyvinyl alcohol were removed by centrifugation. Then, the mixture was poured into a customized mold, frozen at -20°C for 6 hours, and then thawed at room temperature for 2 hours. This cycle was repeated three times and then demolded to obtain the PVA-BC-COS composite hydrogel.

[0096] Table 1 Formula of PVA-BC-COS hydrogel PBC-1 of Example 1

[0097]

[0098]

[0099] Example 2

[0100] This embodiment provides a method for preparing PVA-BC-COS hydrogel (PBC-2). The raw materials and their amounts are shown in Table 2, and the preparation steps are the same as those in Example 1.

[0101] Table 2 Formulation of PVA-BC-COS hydrogel PBC-2 of Example 2

[0102]

[0103] Example 3

[0104] This embodiment provides a method for preparing PVA-BC-COS hydrogel (PBC-3). The raw materials and their amounts are shown in Table 3, and the preparation steps are the same as those in Example 1.

[0105] Table 3 Formula of PVA-BC-COS hydrogel PBC-3 of Example 3

[0106]

[0107] Example 4

[0108] This embodiment provides a method for preparing PVA-BC-COS / Zn hydrogel (PBCZ). The raw materials and their amounts are shown in Table 4. The preparation steps are as follows:

[0109] (1) Take a certain amount of zinc acetate and add water to prepare a solution, take oligosaccharide (COS) and bacterial cellulose (BC) and pour them into a clean beaker containing glycerol and zinc acetate aqueous solution, and the mass ratio of glycerol to water is 3:4. Then, the mixed system in the beaker is stirred for 15 minutes (400r / min) at room temperature with a magnetic stirrer to fully dissolve and disperse the components, and ultrasonic dispersion is used to remove bubbles and further mix to obtain a first mixed liquid.

[0110] (2) Add polyvinyl alcohol (PVA) to the first mixed liquid and stir at room temperature for 10 min (400 r / min) to obtain a second mixed liquid; then seal the beaker with plastic wrap and a rubber ring and place in a high-temperature heating magnetic stirrer and stir until completely dissolved. The temperature of the heating magnetic stirrer is slowly increased to 95°C and the speed is 200 r / min.

[0111] (3) The completely dissolved hydrogel mixture system was collected into a centrifuge tube, and the bubbles generated by the dissolution of polyvinyl alcohol were removed by centrifugation. Then, the mixture was poured into a customized mold, frozen at -20 °C for 6 h, and then thawed at room temperature for 2 h. This cycle was repeated three times and then demolded to obtain the PVA-BC-COS / Zn composite hydrogel.

[0112] Table 4 Formula of PVA-BC-COS / Zn hydrogel PBCZ of Example 4

[0113]

[0114] Comparative Example 1

[0115] This comparative example provides a preparation method of a PVA-BC hydrogel (PB-1) for comparison. The raw materials and their amounts are shown in Table 5. The preparation steps are as follows:

[0116] (1) Pour bacterial cellulose (BC) into a clean beaker containing glycerol and water, with the mass ratio of glycerol to water being 3:4. Then, stir the mixed system in the beaker at room temperature with a magnetic stirrer for 15 min (400 r / min) to fully dissolve and disperse the components, remove bubbles with ultrasonic dispersion, and further mix to obtain a first mixed liquid.

[0117] (2) Add polyvinyl alcohol (PVA) to the first mixed liquid and stir at room temperature for 10 min (400 r / min) to obtain a second mixed liquid; then seal the beaker with plastic wrap and a rubber ring and place in a high-temperature heating magnetic stirrer and stir until completely dissolved. The temperature of the heating magnetic stirrer is slowly increased to 95°C and the speed is 200 r / min.

[0118] (3) The completely dissolved hydrogel mixture system was collected into a centrifuge tube, and the bubbles generated by the dissolution of polyvinyl alcohol were removed by centrifugation. The mixture was then poured into a customized mold, frozen at -20°C for 6 hours, and then thawed at room temperature for 2 hours. This cycle was repeated three times and then demolded to obtain the PVA-BC hydrogel.

[0119] Table 5 Formula of PVA-BC hydrogel PB-1 of comparative example 1

[0120]

[0121]

[0122] Comparative Example 2

[0123] This comparative example provides a preparation method of a PVA-BC hydrogel (PB-2) for comparison. The raw materials and their amounts are shown in Table 6. The preparation steps are as follows:

[0124] (1) Pour bacterial cellulose (BC) into a clean beaker containing glycerol and water, with the mass ratio of glycerol to water being 3:4. Then, stir the mixed system in the beaker at room temperature with a magnetic stirrer for 15 min (400 r / min) to fully dissolve and disperse the components, remove bubbles with ultrasonic dispersion, and further mix to obtain a first mixed liquid.

[0125] (2) Add polyvinyl alcohol (PVA) to the first mixed liquid and stir at room temperature for 10 min (400 r / min) to obtain a second mixed liquid; then seal the beaker with plastic wrap and a rubber ring and place in a high-temperature heating magnetic stirrer and stir until completely dissolved. The temperature of the heating magnetic stirrer is slowly increased to 95°C and the speed is 200 r / min.

[0126] (3) The completely dissolved hydrogel mixture system was collected into a centrifuge tube, and the bubbles generated by the dissolution of polyvinyl alcohol were removed by centrifugation. The mixture was then poured into a customized mold, frozen at -20°C for 6 hours, and then thawed at room temperature for 2 hours. This cycle was repeated three times and then demolded to obtain the PVA-BC hydrogel.

[0127] Table 6 Formula of PVA-BC hydrogel PB-2 of comparative example 2

[0128]

[0129] Comparative Example 3

[0130] This comparative example provides a preparation method of a PVA-BC hydrogel (PB-3) for comparison. The raw materials and their amounts are shown in Table 7. The preparation steps are as follows:

[0131] (1) Pour bacterial cellulose (BC) into a clean beaker containing glycerol and water, with the mass ratio of glycerol to water being 3:4. Then, stir the mixed system in the beaker at room temperature with a magnetic stirrer for 15 min (400 r / min) to fully dissolve and disperse the components, remove bubbles with ultrasonic dispersion, and further mix to obtain a first mixed liquid.

[0132] (2) Add polyvinyl alcohol (PVA) to the first mixed liquid and stir at room temperature for 10 min (400 r / min) to obtain a second mixed liquid; then seal the beaker with plastic wrap and a rubber ring and place in a high-temperature heating magnetic stirrer and stir until completely dissolved. The temperature of the heating magnetic stirrer is slowly increased to 95°C and the speed is 200 r / min.

[0133] (3) The completely dissolved hydrogel mixture system was collected into a centrifuge tube, and the bubbles generated by the dissolution of polyvinyl alcohol were removed by centrifugation. The mixture was then poured into a customized mold, frozen at -20°C for 6 hours, and then thawed at room temperature for 2 hours. This cycle was repeated three times and then demolded to obtain the PVA-BC hydrogel.

[0134] Table 7 Formula of PVA-BC hydrogel PB-3 of comparative example 3

[0135]

[0136] 2. Product physical and chemical performance test results

[0137] The composite hydrogels of the above examples and comparative examples were sampled for physical and chemical properties, including structure and functional group analysis, chemical element analysis, viscoelastic properties, self-healing properties, tensile properties and compression properties, adhesion properties and swelling properties. The data are as follows:

[0138] (1) Fourier transform infrared spectroscopy (FTIR)

[0139] ① The chemical structure and functional group composition of polyvinyl alcohol (PVA), bacterial cellulose (BC-1), chitosan oligosaccharide (COS), and the composite hydrogels PB-1, PBC-1 (PBCOS-1), PB-2, PBC-2 (PBCOS-2), PB-3, and PBC-3 (PBCOS-3) prepared in the above embodiments and comparative examples were tested by Fourier transform infrared spectrometer. The results are as follows. Figure 1 As shown, Figure 1 The horizontal axis is the wavelength (cm -1 ), the ordinate is the transmittance (%). Figure 1 With the introduction of COS, the PBC hydrogels showed a shift change in the -OH characteristic peak and the appearance of the amide I band, indicating that cross-linking occurred between PVA, BC and COS; in addition, with the change of BC content, the chemical structure of the hydrogel did not show a different change, indicating that changing the BC content will not destroy the structure of the hydrogel itself.

[0140] ② Fourier transform infrared spectrometer was used to test the individual polyvinyl alcohol (PVA), bacterial cellulose (BC), chitosan oligosaccharide (COS), zinc (Zinc) and the composite hydrogels PB-3, PBC-3 and PBCZ prepared in the above embodiments and comparative examples. The test results are summarized as follows Figure 2 , Figure 2 The horizontal axis is the wavelength (cm -1 ), the ordinate is the transmittance (%). Figure 2 It can be seen that the chemical structure of PBCZ hydrogel basically retains the typical chemical structure of PVA, BC and COS. The shift change of the -OH characteristic peak and the emergence of new peaks indicate that the hydrogel has a strong interaction with zinc acetate, indicating the successful introduction of zinc ions.

[0141] (2) Elemental analysis

[0142] EDS was used to test and analyze the prepared PB-3, PBC-3, and PBCZ. The results are as follows: Figure 3 ,according to Figure 3 It can be seen that PBCZ hydrogel contains zinc, and the proportion of free oxygen is slightly lower than that of PB and PBC, indicating that the addition of zinc may prompt it to form chemical bonds with hydroxyl oxygen in other components, further confirming the successful introduction of zinc ions into the hydrogel.

[0143] (3) Viscoelastic properties

[0144] The viscoelastic properties of hydrogels PBC-1, PBC-2, and PBC-3 were tested using a rotational dynamic rheometer. The test results are shown in Figure 4 , Figure 4 (a) is the trend diagram of storage modulus (Pa) at different scanning frequencies (Hz). Figure 4 (b) is the trend diagram of loss modulus (Pa) at different scanning frequencies (Hz). Figure 4 B in the figure is the test result of cyclic viscoelastic properties under different strains. Figure 4 The storage modulus G' is always greater than the loss modulus G", indicating that the BC-modified hydrogel behaves like an elastomer rather than a fluid. As the frequency changes, G' and G" change gradiently with the amount of BC introduced, indicating that BC can improve the viscoelastic properties of PVA-based hydrogels.

[0145] (4) Self-healing performance

[0146] The hydrogel PBC-3 was sheared and separated for a while, and then placed together to reattach. It was found that after reattaching, it only took a moment (about 5 minutes) for the two cut surfaces of the hydrogel sheet to be cross-linked again. The macroscopic observation picture is as follows Figure 5 .

[0147] according to Figure 5 as well as Figure 4 The test results of cyclic viscoelastic properties under different strains shown in B indicate that the hydrogel sheets can be re-cross-linked together after being cut and separated for a moment and maintain the same level of storage modulus and loss modulus under different strains, indicating that the hydrogel has good self-healing properties and can buffer external pressure through the reversibility of internal network cross-linking, thereby increasing the service life of the hydrogel dressing.

[0148] (5) Tensile and compressive properties

[0149] The tensile and compressive properties of hydrogels PBC-1, PBC-2, and PBC-3 were tested using a universal mechanical testing machine. The test structure was as follows: Figure 6 ,according to Figure 6 It can be seen that with the increase of BC addition, the hydrogel has a higher elongation at break, indicating that it has good tensile strength and toughness. After the compression test, the hydrogel sample can still return to its original state, and the compressive strength and compression modulus with gradient changes are measured, indicating that it has good compressive resistance and elasticity, which is conducive to avoiding the rupture of the hydrogel caused by external forces during use.

[0150] (6) Adhesion performance

[0151] Paste the hydrogel PBC-3 on centrifuge tubes, glass slides, gloves ( Figure 7 Middle A), knuckles ( Figure 7 Middle B), macroscopic observation of the adhesion of the hydrogel. According to the observation results, it adheres well to the surfaces of different materials and can resist flowing water without slipping, and remains firmly attached under different joint movements.

[0152] (7) Swelling properties

[0153] The mass of the freeze-dried samples of hydrogels PBC-1, PBC-2, and PBC-3 before and after soaking in water was tested to verify their swelling properties. The test results are as follows: Figure 8 ,according to Figure 8 It can be seen that the hydrogel of the present application has good swelling properties. It can also be found that as the concentration of the introduced BC increases, the swelling properties change in a positive correlation, and the rich hydroxyl groups of BC can improve the hydrophilicity of the hydrogel.

[0154] 3. In vitro test results of product pharmaceutical properties

[0155] This chapter studies the biological effects of different groups of hydrogel dressings in an in vitro environment, including: antibacterial properties, antioxidant properties, cell proliferation, cell migration, wound recovery, etc. The experimental data are as follows:

[0156] (1) Antibacterial properties

[0157] In this experiment, Staphylococcus aureus (S. aureus), Escherichia coli (E. coli) and Pseudomonas aeruginosa (P. aeruginosa) were used to evaluate the antibacterial properties of the hydrogel. A small amount of frozen bacteria was inoculated into a centrifuge tube containing liquid LB medium, and the centrifuge tube was placed on a constant temperature shaker at 37°C. The culture was activated at an appropriate speed (200 rpm) for 12-24 hours to reach the logarithmic growth phase. The concentration of the bacterial suspension was tested by an ultraviolet spectrophotometer and expressed as colony forming units (CFU). It was diluted to an OD600 of about 1.0, that is, the bacterial concentration was approximately 1.0×10 8~9 CFU / mL of bacterial solution was used for subsequent antibacterial property characterization.

[0158] Weigh 0.5g of freeze-dried hydrogel sample and place it in a centrifuge tube containing 10mL of PBS solution. Shake it in a constant temperature shaker for 24h (37℃, 200rpm) to obtain the leaching solution of PB-3, PBC-3, and PBCZ hydrogels, and filter it through a 0.22μm filter for later use. Centrifuge the bacterial suspension in the logarithmic growth phase (5000rpm, 1min), resuspend it in sterile PBS solution, measure the concentration of the bacterial solution with an ultraviolet spectrophotometer, and then add an appropriate amount to the PBS leaching solution of different groups to make the bacterial concentration range roughly 1.0×10 4~6CFU / mL, invert and mix to make the bacteria fully contact with the gel extracts of different groups, and then place in a constant temperature shaker (37°C, 200rpm) for co-culture for 12 hours. Take 100μL of the mixed bacterial solution after co-culture and disperse it on the surface of the solid LB culture medium. Use a disposable bacterial coating stick to quickly and gently spread it evenly, then invert it and put it in a 37°C constant temperature incubator. After 24 hours, use an optical camera to observe and record the colony formation.

[0159] In the same way, take an appropriate amount of the above revived and activated bacterial suspension and add it to the LB culture medium of different groups of hydrogels, pipetting and mixing, so that the initial bacterial concentration range is quantitatively 1.0×10 6~8 CFU / mL. Subsequently, the mixed LB culture medium of different groups was transferred to a 96-well plate, and at least 3 parallel samples were set up for each group. The absorbance value at 600nm was dynamically measured within 24 hours using an ELISA reader to monitor the bacterial growth by the change of absorbance value.

[0160] Fig. 9 The growth curve and antibacterial colony formation test results of bacteria in LB medium containing aqueous gel extract are based on Fig. 9 The hydrogels PB-3, PBC-3, and PBCZ all had good inhibitory effects on Pseudomonas aeruginosa, and the hydrogel PBCZ had good inhibitory effects on Staphylococcus aureus, Pseudomonas aeruginosa, and Escherichia coli, and had broad-spectrum antibacterial activity.

[0161] (2) Antioxidant properties

[0162] The antioxidant properties of the hydrogel were evaluated using the total antioxidant capacity assay kit-enzyme labeling method (DPPH method). First, the corresponding material extract was prepared with the extract solution of the freeze-dried hydrogel and stored at 2-8°C for later use. Preheat the microplate reader 30 minutes in advance, adjust the wavelength to 515nm, and prepare each group of hydrogel reaction systems with clean EP tubes according to the instructions. After fully mixing, react at room temperature in the dark for 20 minutes. After the reaction, transfer to a 96-well plate and use a microplate reader for determination. Finally, the following formula is used for calculation:

[0163] DPPH free radical scavenging rate (%) = (A 空白 -A 测定 ) / A 空白 ×100%.

[0164] Fig.10 is the free radical scavenging experimental result of the hydrogel of the present application, according to Fig.10 The hydrogel of the present application can significantly reduce the level of DPPH free radicals, which shows that PBCZ hydrogel has a positive antioxidant effect.

[0165] (3) Promoting cell proliferation

[0166] Calcein / PI cell viability and cytotoxicity assay kits were used to evaluate the cytotoxicity of PB-3, PBC-3, and PBCZ hydrogels to mouse embryonic fibroblasts (NIH-3T3) and human umbilical vein endothelial cells (HUVEC). 4 Cells / mL) were subcultured and inoculated into a 35 mm diameter confocal culture dish. After overnight attachment, the old culture medium was removed, washed twice with PBS, and then different groups of gel immersion solutions were added. After culturing in the incubator for 1 day and 3 days, a working solution containing Calcein-AM / PI was added to stain live and dead cells (37°C, protected from light) for 30 minutes. Five different fields of view were randomly selected from each well for observation and imaging with a laser confocal microscope. Red fluorescence indicates dead cells, and green fluorescence indicates live cells, which intuitively evaluates the effect of hydrogel on cell growth vitality.

[0167] The CCK-8 kit was used to evaluate the effects of PB-3, PBC-3 and PBCZ hydrogels on cell proliferation. The two types of cells were subcultured and inoculated on 96-well plates, with a cell density of 2000 cells per well, and at least 3 replicates per group. After overnight adherence, the old culture medium was removed, washed twice with PBS, and replaced with complete culture medium for gel immersion for 1 and 3 days. During the test, the old culture medium was discarded, and 100 μL of serum-free CCK-8DMEM mixed solution was quickly added to each well (according to the instructions, the ratio of CCK-8 to DMEM was 1:10). The 96-well plate was wrapped with tin foil and transferred to a cell culture incubator for incubation in the dark for 0.5h to 1h. The absorbance value was measured at 450nm using an enzyme reader, and each sample was read at least 3 times. The proliferation of cells in each group was plotted and analyzed based on the OD values ​​measured in the experiment.

[0168] Fig.11 The results of the CCK-8 cell and cell proliferation test and cell live-death staining test of the hydrogel of the present application are as follows: Fig.11 The hydrogel promoted the proliferation of mouse embryonic fibroblasts (NIH-3T3 cells) and human umbilical vein endothelial cells (HUVEC cells).

[0169] (4) Promote cell migration

[0170] Scratch test: First, use a marker pen to draw horizontal lines on the back of the 6-well plate to locate the field of view when taking pictures. 5The cells were plated at a density of 100 / well and cultured until they reached 100% confluence. Then, a 200 μL sterile yellow gun tip was used to make cell scratches perpendicular to the bottom of the plate, the culture medium was removed, and the floating cells and their debris were washed with PBS. Serum-free culture medium was added to observe and photograph, and the result was recorded as 0h. Subsequently, gel immersion containing low-concentration serum (2% for NIH-3T3 cells and 0% for HUVEC cells) was added and cultured for 24h. The culture medium was discarded, and the cells were gently washed twice with PBS solution. The cells were observed and photographed under a microscope, and the result was recorded as 24h. The images were collected and quantitatively analyzed using Image J software. The difference in cell migration ability was defined as the percentage of the cell recovery area to the original scratch area.

[0171] Transwell experiment: The two cells were pretreated with different groups of gel immersion solution for 24 hours, and the NC group was treated with blank H-DMEM complete medium. After 24 hours, the cells were digested and resuspended in serum-free DMEM medium. After counting the cells, the concentration of the cell suspension in each group was adjusted to 5×10 5 Pipette 100 μL of cell suspension (5×10 4 Cells) were inoculated into the upper chamber of the Transwell with a pore size of 8μm and placed in a 24-well plate. The gel immersion solution containing 2% FBS was added to the lower chamber of the Transwell, and the NC group was a DMEM medium with the same serum concentration. After incubation at 37°C for a certain period of time (36h for NIH-3T3 cells and 24h for HUVEC cells), the culture medium in the upper chamber was removed, and the cells remaining inside the upper chamber were wiped with a cotton swab, rinsed with PBS, and fixed in 4% paraformaldehyde for 15min. The chamber was removed with tweezers, and the residual paraformaldehyde was washed off with PBS and then placed in 0.1% (w / v) crystal violet for staining for 15min. Finally, the upper chamber was placed on a slide, observed under an inverted microscope, and 3 fields of view were randomly selected for photography. Image J software was used for quantitative analysis. The difference in cell migration ability was defined as the number of cells that migrated to the outer side of the chamber.

[0172] Figure 12-13 The results of the scratch test and Transwell test of the hydrogel in this application are as follows. Figure 12-13 The hydrogel promoted the planar and transmembrane migration of NIH-3T3 and HUVEC cells.

[0173] (4) Promoting wound recovery

[0174] RNA extraction: The above two cell lines were subcultured and inoculated, and after overnight attachment, different groups of gel immersion solutions were added for intervention for 3 days. The culture medium was discarded, and the cells were collected on ice. The total RNA of the cells was extracted according to the instructions of RNAFast200 total RNA rapid extraction kit, and the concentration was determined by NanoDrop 2000.

[0175] cDNA synthesis: using BeyoRT TM The extracted total cellular RNA was reverse transcribed into cDNA using the III cDNA synthesis kit (with gDNA EZeraser).

[0176] 1) Removal of genomic DNA: According to the RNA concentration, pipette 1 μg of RNA sample into a 200 μL PCR tube, add 1 μL of gDNA Ezeraser and 1 μL of gDNA EZeraser Buffer (10×), respectively, and standardize the mixed system to 10 μL with diethylpyrocarbonate water (DEPC), mix well and incubate at 37°C for 2 min.

[0177] 2) Reverse transcription: Continue to add 6 μL DEPC water and 4 μL BeyoRT TM III cDNA first-strand synthesis premix (5×) was gently mixed and centrifuged, and reverse transcribed into cDNA according to the program of 42°C, 10 min, 80°C, 10 min, and 4°C, +∞. The product was directly used for fluorescent quantitative PCR reaction or stored at -20°C.

[0178] PCR amplification: using BeyoFast TM SYBR Green qPCR Mix kit was used to quantitatively detect the expression of target genes, including interleukin-1beta (IL-1β), interleukin-6 (IL-6), connective tissue growth factor (CTGF), beta-fibroblast growth factor (β-FGF), angiogenin (Ang), and platelet-derived growth factor A (PDGFA). According to the instructions, 20 μL of reaction system was prepared on ice, and the reaction program of the PCR amplification instrument was set according to the instructions.

[0179] Fig.14It is the result of the repair-promoting experiment of the hydrogel of the present application, which was detected by reverse transcription fluorescence quantitative polymerase chain reaction (RT-qPCR). According to the test results, the hydrogel can promote the expression of fibroblast growth factor β-FGF, connective tissue growth factor CTGF, and angiogenesis-related genes Ang and PDGFA, and inhibit the expression of IL-6 and IL-1β pro-inflammatory related genes, indicating that the hydrogel has a positive effect in promoting tissue repair, inhibiting inflammatory response and promoting the generation of vascular endothelial cells.

[0180] (5) Rat model construction process

[0181] Furthermore, a full-thickness skin defect model of SD rats was established. The steps are as follows: 24 male SD rats (8 weeks old, 250±30g) were purchased from Zhuhai Baishitong Company and adaptively raised in the animal experiment center of the hospital for 1 week. The 24 rats were randomly divided into 4 groups, namely NC group, PB group, PBC group and PBCZ group, with 6 rats in each group. The rats were placed in an anesthesia box and adjusted to 3% isoflurane for anesthesia. After confirming that the anesthesia effect took effect, the rats were taken out and placed on the operating table, and the anesthesia mask was buckled to maintain anesthesia. Skin preparation and disinfection: Use a shaver to remove the hair on the back of the rat, and then apply an appropriate amount of depilatory cream to the surgical area. After 5 minutes, use gauze to wipe off the depilatory cream and hair, spray the surface with alcohol to remove the residual depilatory cream, wipe the surgical field with alcohol gauze for disinfection, lay a hole towel, and change sterile gloves. Wound modeling: Use a skin puncher with a diameter of 15 mm to make two circular incisions on the back of SD rats. Pay attention to the depth of modeling to avoid damage to subcutaneous tissue. Use curved forceps to bluntly separate the surface fascia, and use ophthalmic scissors to cut the skin in the area along the incision to obtain a circular wound model with a diameter of 15 mm. After the wound is made, a silicone ring with an inner diameter of 15 mm is used to fix the skin wound to reduce incision contraction. After modeling, a hydrogel patch 3M sterile breathable film is placed in different groups to cover the skin wound and protect it with gauze and mesh sleeves, and 2 rats are raised per cage. By placing PB, PBC, PBCZ hydrogel dressings and traditional gauze dressings in the wound area, the wound healing was observed and photographed on days 0, 4, 7, and 14 after surgery, and the rats were killed on days 7 and 14 for tissue section analysis, so as to systematically study the biological effects of PBCZ hydrogel dressings in the in vivo environment.

[0182] The wound healing status was recorded by dynamic observation and quantitative analysis. Fig.15 , Fig.15 It can be seen that the PBCZ hydrogel prepared in the present application can effectively promote the closure of defect wounds. Figure 16-17 The tissue sections were stained with HE and Masson staining, respectively, and the results showed that the hydrogel of the present application has a good effect in promoting skin wound healing and regenerating skin reconstruction.

[0183] The technical features of the above-mentioned implementation modes and examples can be combined in any appropriate manner. To make the description concise, not all possible combinations of the technical features in the above-mentioned implementation modes and examples are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0184] The above-described embodiments only express several implementation methods of the present application, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for those of ordinary skill in the art, without departing from the concept of the present application, several variations and improvements can also be made, which all belong to the protection scope of the present application. In addition, it should be understood that after reading the above-mentioned teaching content of the present application, those skilled in the art can make various changes or modifications to the present application, and the equivalent forms obtained also fall within the protection scope of the present application. It should also be understood that the technical solutions obtained by those skilled in the art on the basis of the technical solutions provided in the present application through logical analysis, reasoning or limited experiments are all within the protection scope of the claims attached to the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A method for preparing a composite hydrogel, characterized in that: The steps include: Chitosan oligosaccharide and bacterial cellulose are mixed and added into a first solvent for first dispersion to obtain a first mixed liquid; the first solvent includes glycerol and water, and optionally includes zinc ions; Adding polyvinyl alcohol to the first mixed liquid for second dispersion to obtain a second mixed liquid; Taking the second mixed liquid, and heating it while performing the third dispersion to form the gel; The gel is subjected to cyclic freeze-thaw cycles to obtain the composite hydrogel.

2. The preparation method according to claim 1, characterized in that: Taking the total weight percentage of the second mixed liquid as 100wt%, the second mixed liquid includes 10wt% to 20wt% of the polyvinyl alcohol, 0.1wt% to 0.3wt% of the bacterial cellulose and 1wt% to 3wt% of the chitosan oligosaccharide; Optionally, it further comprises 0.2wt% to 0.8wt% of the zinc ion; Optionally, in the second mixed liquid, the weight ratio of the polyvinyl alcohol, the bacterial cellulose and the chitosan oligosaccharide is 1:(0.005-0.02):(0.1-0.15).

3. The preparation method according to claim 1, characterized in that: The first dispersion includes stirring at 300 r / min to 500 r / min for 10 min to 20 min.

4. The preparation method according to claim 1, characterized in that: The rate of adding the polyvinyl alcohol to the first mixed liquid is 1 g / min to 1.5 g / min; and / or The second dispersion includes stirring at 300 r / min to 500 r / min for 5 min to 15 min.

5. The preparation method according to claim 1, characterized in that: In the step of performing the third dispersion and heating simultaneously, the third dispersion includes stirring at 100 r / min to 300 r / min, and the heating temperature is 90° C. to 100° C.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The freeze-thaw cycle procedure includes: freezing at -30°C to -20°C for 5h to 7h and then transferring to room temperature for thawing for 1h to 3h, and the number of cycles is at least three times.

7. The preparation method according to any one of claims 1 to 5, characterized in that: The weight ratio of glycerol to water in the first solvent is (0.7-0.8):

1.

8. A composite hydrogel prepared by the preparation method according to any one of claims 1 to 7.

9. A functional dressing, characterized in that: The material of the functional dressing includes the composite hydrogel according to claim 8.

10. The functional dressing according to claim 9, characterized in that: Have at least one of the following characteristics: (1) Adhesion; (2) Freeze resistance; (3) Toughness and elasticity; (4) Self-healing performance; (5) Antibacterial, optionally, the antibacterial bacteria include Staphylococcus aureus, Pseudomonas aeruginosa and Escherichia coli; (6) Anti-inflammatory; (7) Antioxidant; (8) promoting angiogenesis; and (9) Promote skin healing.

Citation Information

Cited By

  • Inulin gel loaded with callicarpa nudiflora-derived extracellular vesicles as well as preparation method and application of inulin gel

    CN121714639A

  • A inulin gel carrying a naked flower of source of extracellular vesicle of purple olive and a preparation method and application thereof