Selective ammoxidation catalyst as well as preparation method and application thereof

By loading precious metals on a titanium-tin composite oxide carrier, a selective ammonia oxidation catalyst is prepared, which solves the problems of low ammonia conversion rate and serious ammonia leakage in the existing technology, achieves high catalytic activity and nitrogen selectivity, and is suitable for diesel Car exhaust treatment.

CN118788334APending Publication Date: 2024-10-18TIANJIN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410794716.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing selective ammonia oxidation catalysts have low ammonia conversion rates and serious ammonia leakage problems in diesel vehicle exhaust treatment, making it difficult to meet increasingly stringent emission standards.

Method used

Titanium-tin composite oxide is used as a carrier to support precious metals (such as palladium, platinum, and silver) through co-precipitation and impregnation methods to prepare selective ammonia oxidation catalysts to improve catalytic activity and nitrogen selectivity.

Benefits of technology

It maintains high nitrogen selectivity under low temperature conditions, significantly improves the catalytic activity of ammonia catalytic oxidation, effectively reduces ammonia leakage, and is suitable for diesel vehicle exhaust treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788334A_ABST
    Figure CN118788334A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ammoxidation catalysts, in particular to a selective ammoxidation catalyst and a preparation method and application thereof. The invention provides a selective ammoxidation catalyst in an optional embodiment, the catalyst comprises a carrier and an active component, the carrier is TixSn1-xO2, and the active component is precious metal; wherein x is the molar ratio of Ti to Sn, and x is more than 0 and less than 1. The carrier of the selective ammoxidation catalyst provided by the invention is the titanium-tin composite oxide, and the titanium-tin composite oxide carrier supports the noble metal catalyst, so that in the ammonia catalytic oxidation process at 150-500 DEG C, the catalyst has high catalytic activity on the basis of keeping high nitrogen selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ammonia oxidation catalysts, and in particular to a selective ammonia oxidation catalyst and a preparation method and application thereof. Background Art

[0002] NH3 is a colorless, toxic, flammable, irritating and corrosive gas that is potentially harmful to human health and the environment. The human nose can detect the smell of ammonia at 5-10ppm; below 50ppm, it will irritate the respiratory system, skin and eyes; excessive exposure to ammonia exceeding 300ppm can cause lung disease; and 500ppm and above will seriously threaten life and health; NH3 exceeding 10,000ppm will kill people within 5-10 minutes. NH3 discharged into the atmosphere will cause a series of environmental problems, such as acid rain, photochemical smog and other problems.

[0003] Since the most common NO x Treatment technologies often require the use of excess automotive urea to reduce NO x , in order to achieve complete conversion of NO, but the actual NH3 / NO is greater than 1, which is prone to ammonia leakage. At the same time, the deactivation of the SCR catalyst, the high flow rate of NH3 / NO and the large flow rate or uneven mixing of diesel exhaust will inevitably lead to an increase in ammonia leakage. Since 2019, various regions in China have been implementing the National VI standard, which limits ammonia emissions to 10ppm. Therefore, the removal of leaked ammonia has attracted more and more attention. Considering the increasingly stringent exhaust emission standards for diesel vehicles and the characteristics of their after-treatment systems, the development of NH3-SCO catalysts with excellent low-temperature activity, high N2 selectivity and good hydrothermal stability is of great practical significance.

[0004] The selective ammonia oxidation catalysts in the prior art, such as precious metal-loaded titanium dioxide catalysts, precious metal-loaded tin oxide catalysts, or precious metal-loaded tin oxide and titanium dioxide mixed catalysts, can also catalyze the oxidation of ammonia, but their conversion rates of ammonia are not high. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a selective ammonia oxidation catalyst and a preparation method and application thereof, wherein the selective ammonia oxidation catalyst has high catalytic activity and nitrogen selectivity in the process of ammonia catalytic oxidation.

[0006] To this end, the present invention provides the following technical solutions:

[0007] In a first aspect, the present invention provides a selective ammonia oxidation catalyst in an optional embodiment, the catalyst comprising a carrier and an active component, the carrier being Ti x Sn 1-xO2, the active component is a noble metal; wherein x represents the molar ratio of Ti to Sn, 0<x<1, and x is preferably 0.05-0.3.

[0008] In the catalyst of the present invention, the noble metal may be one or more of palladium, platinum or silver, or other noble metals, and the present invention is not limited thereto. The selective ammonia oxidation catalyst provided by the present invention has high catalytic activity while maintaining high nitrogen selectivity.

[0009] In a second aspect, the present invention provides, in an optional embodiment, a method for preparing the above-mentioned selective ammonia oxidation catalyst, comprising the following steps:

[0010] S1: Dissolve titanium salt in water and add tin salt to stir, adjust the pH value of the mixed solution, then let it stand, age, filter, wash, dry and calcine the obtained solid to obtain the carrier Ti x Sn 1-x O2;

[0011] S2: The carrier Ti x Sn 1-x After O2 is dissolved in water, a noble metal solution is added, stirred, rotary evaporated, dried, and calcined to obtain the selective ammonia oxidation catalyst;

[0012] Wherein, the molar ratio of the titanium salt to the tin salt is x, 0 <x<1。

[0013] In the present invention, the carrier Ti is prepared by coprecipitation method. x Sn 1-x O2, and then the precious metal is impregnated into the carrier by an impregnation method. The preparation and synthesis method is simple, and the prepared selective ammonia oxidation catalyst has better catalytic activity while maintaining a high nitrogen selectivity.

[0014] Preferably, the titanium salt is selected from one or more of titanium sulfate, tetrabutyl titanate or titanium tetrachloride; the tin salt is selected from one or more of tin tetrachloride, stannous sulfate or stannous chloride.

[0015] In the present invention, the choice of titanium salt is not limited to one or more of titanium sulfate, tetrabutyl titanate or titanium tetrachloride, and any inorganic salt or organic salt containing metallic titanium can achieve the purpose of the present invention. The choice of tin salt is not limited to one or more of tin tetrachloride, stannous sulfate or stannous chloride, and any inorganic salt containing metallic tin can achieve the purpose of the present invention.

[0016] Preferably, in step S1, the pH value of the solution is adjusted to 9-11; the solution for adjusting the pH value is an alkali solution, the alkali solution is selected from one or more of ammonia water, sodium bicarbonate or potassium bicarbonate, and the concentration of the alkali solution is 0.05-1 mol / L. The aging time is 8-14 hours; the drying temperature is 100-120°C, and the time is 8-12 hours. The calcination temperature is 400-600°C; the calcination time is 3-5 hours, and the stirring time is 20-40 minutes.

[0017] Preferably, in step S2, the noble metal in the noble metal solution is selected from one or more of palladium, platinum or silver; the carrier Ti x Sn 1-x The mass ratio of O2 to the precious metal in the precious metal solution is 500:(1-5). The temperature of the rotary evaporation is 65-90°C; the temperature of the roasting is 350-600°C, the time is 3-5 hours, and the stirring time is 2-4 hours.

[0018] In the present invention, the selection of precious metals is not limited to one or more of palladium, platinum or silver. Other precious metals, such as ruthenium, rhodium, etc., can also achieve the purpose of the present invention.

[0019] In a third aspect, the present invention provides, in an optional embodiment, an application of the above-mentioned selective ammonia oxidation catalyst or the selective ammonia oxidation catalyst obtained by the above-mentioned preparation method in treating ammonia in diesel vehicle exhaust.

[0020] Preferably, the conditions for treating ammonia in diesel exhaust are: temperature of 150-500°C, ammonia concentration of 500 ppm in exhaust gas, oxygen volume fraction of 10%, nitrogen as balance gas, gas flow rate of 300 ml / min, space velocity of 100000 h -1 The dosage of the selective ammoxidation catalyst is 0.15-0.20 ml.

[0021] Compared with the prior art, the present invention has one of the following beneficial effects:

[0022] 1. The carrier of the selective ammonia oxidation catalyst provided by the present invention is a titanium-tin composite oxide. The catalyst of the titanium-tin composite oxide carrier loaded with a precious metal has a high catalytic activity while maintaining a high nitrogen selectivity during the catalytic oxidation of ammonia at 150-500°C.

[0023] 2. The method for preparing a selective ammonia oxidation catalyst provided by the present invention can obtain the catalyst by using a co-precipitation method plus an impregnation method. The synthesis method is simple and can be promoted on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a graph showing the NH3 conversion rate results of the SCO activity test of the catalysts prepared in Examples 1-7 of the present invention;

[0026] Figure 2 This is a graph showing the NH3 conversion rate results of the SCO activity test of the catalysts of Example 1 of the present invention and Comparative Examples 1-3;

[0027] Figure 3 This is a graph showing the N2 selectivity results of the SCO activity test of the catalysts prepared in Examples 1-7 of the present invention;

[0028] Figure 4 This is a graph showing the N2 selectivity results of the SCO activity test of the catalysts in Example 1 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] In a specific embodiment of the present invention, the carrier is Ti x Sn 1-x O2, wherein x is the molar ratio of Ti to Sn, 0<x<1, x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc. The specific value of x is determined by the added amount of titanium salt and tin salt.

[0031] The noble metal is selected from one or more of palladium, platinum or silver. The noble metal can be any combination of palladium, platinum or silver. The mass ratio of any two noble metal combinations in the present invention can be 1:0.5-2, but the present invention is not limited thereto.

[0032] The titanium salt is selected from one or more of titanium sulfate, tetrabutyl titanate or titanium tetrachloride. The titanium salt can be any combination of titanium sulfate, tetrabutyl titanate or titanium tetrachloride. The mass ratio of any two titanium salt combinations in the present invention can be 1:0.5-2, but the present invention is not limited thereto.

[0033] The tin salt is selected from one or more of tin tetrachloride, stannous sulfate or stannous chloride. The tin salt can be any combination of tin tetrachloride, stannous sulfate or stannous chloride. The mass ratio of any two tin salt combinations in the present invention can be 1:0.5-2, but the present invention is not limited thereto.

[0034] The following is a specific example to illustrate the solution of the present invention.

[0035] Example 1

[0036] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.05 Sn 0.95 O2, the active component is Ag.

[0037] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0038] S1: Weigh 0.71997g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution, add 19.9842g of tin tetrachloride precursor, stir for 30min, slowly drop 0.5mol / L ammonia water into the mixed solution until pH=10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, dry it at 120℃ for 12h to obtain a solid; place the above solid in a muffle furnace, calcine it at 500℃ in air atmosphere for 4 hours to obtain the carrier Ti 0.05 Sn 0.95 O2.

[0039] S2: 5g of carrier Ti 0.05 Sn 0.95 O2 was placed in a beaker, deionized water was added and stirred, and an aqueous solution of silver nitrate containing 0.05g Ag was added to form a mixed solution, which was stirred for 3 hours; the mixed solution was placed in a flask, and the water was evaporated at 70°C, and the sample was scraped out and dried; the above sample was placed in a muffle furnace and calcined for 4h at 450°C in an air atmosphere to obtain Ag / Ti 0.05 Sn 0.95 O2 catalyst, wherein the Ag loading is 1 wt%.

[0040] Example 2

[0041] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.05 Sn 0.95 O2, the active component is Pt, and the loading amount is 1wt%.

[0042] The preparation method of the selective ammonia oxidation catalyst of this embodiment is different from the preparation method of Example 1 only in that the noble metal is chloroplatinic acid, and the remaining steps are the same as those of Example 1.

[0043] Example 3

[0044] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.05 Sn 0.95 O2, the active component is Pd, and the loading amount is 1wt%.

[0045] The preparation method of the selective ammonia oxidation catalyst of this embodiment is different from the preparation method of Example 1 only in that the noble metal is palladium nitrate, and the remaining steps are the same as those of Example 1.

[0046] Example 4

[0047] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.1 Sn 0.9 O2, the active component is Ag.

[0048] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0049] S1: Weigh 1.44 g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution, add 18.93 g of tin tetrachloride precursor, stir for 30 min, slowly drop 0.5 mol / L ammonia water into the mixed solution until pH = 10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, dry it at 120°C for 12 hours to obtain a solid; place the above solid in a muffle furnace, calcine it at 500°C in an air atmosphere for 4 hours to obtain the carrier Ti 0.1 Sn 0.9 O2.

[0050] S2: 5g of carrier Ti 0.1 Sn 0.9 O2 was placed in a beaker, deionized water was added and stirred, and an aqueous solution of silver nitrate containing 0.05g Ag was added to form a mixed solution, which was stirred for 3 hours; the mixed solution was placed in a flask, and the water was evaporated at 70°C, and the sample was scraped out and dried; the above sample was placed in a muffle furnace and calcined for 4h at 450°C in an air atmosphere to obtain Ag / Ti 0.1 Sn 0.9 O2 catalyst with an Ag loading of 1 wt%.

[0051] Example 5

[0052] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.3 Sn 0.7 O2, the active component is Ag.

[0053] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0054] S1: Weigh 4.32g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution, add 14.72g of tin tetrachloride precursor, stir for 30min, slowly drop 0.5mol / L ammonia water into the mixed solution until pH=10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, dry it at 120℃ for 12h to obtain a solid; place the solid in a muffle furnace, calcine it at 500℃ in air atmosphere for 4 hours to obtain the carrier Ti 0.3 Sn 0.7 O2.

[0055] S2: 5g of carrier Ti 0.3 Sn 0.7 O2 was placed in a beaker, deionized water was added and stirred, and an aqueous solution of silver nitrate containing 0.05g Ag was added to form a mixed solution, which was stirred for 3 hours; the mixed solution was placed in a flask, and the water was evaporated at 70°C, and the sample was scraped out and dried; the above sample was placed in a muffle furnace and calcined for 4h at 450°C in an air atmosphere to obtain Ag / Ti 0.3 Sn 0.7 O2 catalyst with an Ag loading of 1 wt%.

[0056] Example 6

[0057] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.8 Sn 0.2 O2, the active component is Ag.

[0058] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0059] S1: Weigh 11.52g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution, add 4.21g of tin tetrachloride precursor, stir for 30min, slowly drop 0.5mol / L ammonia water into the mixed solution until pH=10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, dry it at 120℃ for 12h to obtain a solid; place the solid in a muffle furnace, calcine it at 500℃ in air atmosphere for 4 hours to obtain the carrier Ti 0.8 Sn 0.2O2.

[0060] S2: 5g of carrier Ti 0.3 Sn 0.7 O2 was placed in a beaker, deionized water was added and stirred, and an aqueous solution of silver nitrate containing 0.05g Ag was added to form a mixed solution, which was stirred for 3 hours; the mixed solution was placed in a flask, and the water was evaporated at 70°C, and the sample was scraped out and dried; the above sample was placed in a muffle furnace and calcined for 4h at 450°C in an air atmosphere to obtain Ag / Ti 0.8 Sn 0.2 O2 catalyst with an Ag loading of 1 wt%.

[0061] Example 7

[0062] This embodiment provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is Ti 0.9 Sn 0.1 O2, the active component is Ag.

[0063] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0064] S1: Weigh 12.96g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution, add 2.10g of tin tetrachloride precursor, stir for 30min, slowly drop 0.5mol / L ammonia water into the mixed solution until pH=10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, dry it at 120℃ for 12h to obtain a solid; place the solid in a muffle furnace, calcine it at 500℃ in air atmosphere for 4 hours to obtain the carrier Ti 0.9 Sn 0.1 O2.

[0065] S2: 5g of carrier Ti 0.9 Sn 0.1 O2 was placed in a beaker, deionized water was added and stirred, and an aqueous solution of silver nitrate containing 0.05g Ag was added to form a mixed solution, which was stirred for 3 hours; the mixed solution was placed in a flask, and the water was evaporated at 70°C, and the sample was scraped out and dried; the above sample was placed in a muffle furnace and calcined for 4h at 450°C in an air atmosphere to obtain Ag / Ti 0.9 Sn 0.1 O2 catalyst with an Ag loading of 1 wt%.

[0066] Comparative Example 1

[0067] This comparative example provides a selective ammonia oxidation catalyst, comprising a carrier and an active component, wherein the carrier is TiO2 and the active component is Ag.

[0068] The selective ammoxidation catalyst of this comparative example is prepared by the following steps:

[0069] S1: Weigh 10g of titanium sulfate precursor and dissolve it in deionized water to form a mixed solution and stir for 30min. Slowly add 0.5mol / L ammonia water to the mixed solution until pH = 10, let the mixed solution stand and age for 12 hours, filter and wash the precipitate with deionized water until it is neutral, put the precipitate into an oven, and dry it at 120℃ for 12h to obtain a solid; place the above solid in a muffle furnace and calcine it at 500℃ in an air atmosphere for 4 hours to obtain a carrier TiO2.

[0070] S2: Place 5g of carrier TiO2 in a beaker, add deionized water and stir, add an aqueous solution of silver nitrate containing 0.05g Ag to form a mixed solution, and stir for 3 hours; place the mixed solution in a flask, evaporate the water at 70°C, scrape out the sample and dry it; place the above sample in a muffle furnace, calcine it at 450°C in an air atmosphere for 4h to obtain an Ag / TiO2 catalyst with an Ag loading of 1wt%.

[0071] Comparative Example 2

[0072] This comparative example provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is SnO2 and the active component is Ag.

[0073] The selective ammonia oxidation catalyst of this embodiment is prepared by the following steps:

[0074] S1: Weigh 10g of tin tetrachloride precursor and dissolve it in deionized water to form a mixed solution and stir it for 30 minutes. Slowly add 0.5mol / L ammonia water to the mixed solution until the pH value is 10, and let the mixed solution stand for 12 hours. Filter and wash the precipitate with deionized water until it is neutral. Put the precipitate into an oven and dry it at 120℃ for 12 hours to obtain a solid. Place the above solid in a muffle furnace and calcine it at 500℃ in an air atmosphere for 4 hours to obtain the carrier SnO2.

[0075] S2: Place 5 g of carrier SnO2 in a beaker, add deionized water and stir, add an aqueous solution of silver nitrate containing 0.05 g of Ag to form a mixed solution, and stir for 3 hours; place the mixed solution in a flask, evaporate the water at 70°C, scrape out the sample and dry it; place the above sample in a muffle furnace, calcine it at 450°C in an air atmosphere for 4 hours to obtain an Ag / SnO2 catalyst with an Ag loading of 1 wt%.

[0076] Comparative Example 3

[0077] This comparative example provides a selective ammonia oxidation catalyst, including a carrier and an active component, wherein the carrier is TiO2-SnO2 and the active component is Ag.

[0078] The selective ammoxidation catalyst of this comparative example is prepared by the following steps:

[0079] S1: Weigh 0.72 g of titanium dioxide precursor and 19.98 g of tin dioxide precursor into a ball mill, and add silicon nitride grinding balls;

[0080] S2: Start the ball mill with a rotation frequency of 500 rpm, take a break every 5 minutes, and then continue grinding. Continue ball milling for 2 hours to obtain a mechanically mixed TiO2-SnO2 carrier;

[0081] S3: placing the above carrier in a beaker, adding deionized water and stirring, adding silver nitrate solution to form a mixed solution, and stirring for 3 hours;

[0082] S4: Place the mixed solution in a flask, evaporate the water at 70°C, scrape out the sample and dry it;

[0083] S5: The above sample was placed in a muffle furnace and calcined for 4 hours at 450°C in an air atmosphere to obtain an Ag / TiO2-SnO2 catalyst with an Ag loading of 1 wt%.

[0084] Test Case

[0085] The selective ammonia oxidation catalysts obtained in Examples 1-7 and Comparative Examples 1-3 were added to a quartz tube and subjected to a simulated diesel exhaust reaction. The simulated diesel exhaust contained 500 ppm NH3 and 10% O2 by volume, the balance gas was N2, the total flow rate was 300 ml / min, and the air velocity was 100,000 h -1 The conversion rate of NH3 and the selectivity of N2 of the catalysts of the examples and comparative examples at different temperatures were tested. The results are shown in Figure 1-4 and Table 1 and Table 2:

[0086] The conversion rate of NH3 is calculated as follows: (NH3 concentration at the reactor inlet - NH3 concentration at the reactor outlet) / (NH3 concentration at the reactor inlet) × 100%;

[0087] The formula for calculating the selectivity of N2 is: (NH3 concentration at the reactor inlet - NH3 concentration at the reactor outlet - NO concentration at the reactor outlet - NO2 concentration at the reactor outlet - N2O concentration at the reactor outlet) / (NH3 concentration at the reactor inlet - NH3 concentration at the reactor outlet) × 100%.

[0088] Table 1 NH3 conversion rate of the catalysts of the examples and comparative examples at different temperatures

[0089]

[0090] Table 2 Selectivity of N2 of the catalysts of the examples and comparative examples at different temperatures

[0091]

[0092]

[0093] Through Tables 1, 2 and Figure 1-4 It can be seen that by comparing the data of Examples 1, 4-7 and Comparative Examples 1-3, it is not difficult to find that the selective ammonia oxidation catalyst of the present application has substantially the same nitrogen selectivity as the catalyst of Comparative Examples 1-3, but when the molar ratio of Ti and Sn in the catalyst of the present application is in the range of 0.05-0.3, the catalytic activity of the catalyst of the present application is better than that of the catalyst of Comparative Examples 1-3. Therefore, the selective ammonia oxidation catalyst prepared by the present invention can have a higher catalytic activity while maintaining a higher nitrogen selectivity.

[0094] Although the principles of the present invention are described in detail above in conjunction with the preferred embodiments of the present invention, those skilled in the art should understand that the above embodiments are merely explanations of the exemplary implementations of the present invention, and are not intended to limit the scope of the present invention. The details in the embodiments do not constitute limitations on the scope of the present invention, and any obvious changes such as equivalent transformations, simple replacements, etc. based on the technical solution of the present invention, without departing from the spirit and scope of the present invention, fall within the protection scope of the present invention.

Claims

1. A selective ammonia oxidation catalyst, characterized in that: The catalyst comprises a carrier and an active component, wherein the carrier is Ti x Sn 1-x O2, the active component is a noble metal; Wherein, x represents the molar ratio of Ti to Sn, 0<x<1.

2. A method for preparing the selective ammonia oxidation catalyst according to claim 1, characterized in that: The following steps are involved: S1: Dissolve titanium salt in water and add tin salt to stir, adjust the pH value of the mixed solution, then let it stand, age, filter, wash, dry and calcine the obtained solid to obtain the carrier Ti x Sn 1-x O2; S2: The carrier Ti x Sn 1-x After O2 is dissolved in water, a noble metal solution is added, stirred, rotary evaporated, dried, and calcined to obtain the selective ammonia oxidation catalyst; Wherein, the molar ratio of the titanium salt to the tin salt is x, 0 <x<1。 3. The method for preparing the selective ammonia oxidation catalyst according to claim 2, characterized in that: The titanium salt is selected from one or more of titanium sulfate, tetrabutyl titanate or titanium tetrachloride; and / or, The tin salt is selected from one or more of tin tetrachloride, stannous sulfate or stannous chloride.

4. The method for preparing the selective ammonia oxidation catalyst according to claim 2, characterized in that: In step S1, adjusting the pH value of the solution to 9-11; and / or, The solution for adjusting the pH value is an alkali solution, which is selected from one or more of ammonia water, sodium bicarbonate or potassium bicarbonate, and the concentration of the alkali solution is 0.05-1 mol / L.

5. The method for preparing the selective ammonia oxidation catalyst according to claim 2, characterized in that: In step S1, the aging time is 8-14 hours; and / or, The drying temperature is 100-120° C. and the drying time is 8-12 hours.

6. The method for preparing the selective ammonia oxidation catalyst according to claim 2, characterized in that: In step S1, the calcination temperature is 400-600°C; and / or, The calcination time is 3-5 hours.

7. The method for preparing a selective ammonia oxidation catalyst according to claim 2, characterized in that: In step S2, the noble metal in the noble metal solution is selected from one or more of palladium, platinum or silver; and / or, The carrier Ti x Sn 1-x The mass ratio of O2 to the precious metal in the precious metal solution is 500:(1-5).

8. The method for preparing a selective ammonia oxidation catalyst according to claim 2, characterized in that: In step S2, the rotary evaporation temperature is 65-90° C.; and / or, The calcination temperature is 350-600° C. and the calcination time is 3-5 hours.

9. Use of the selective ammonia oxidation catalyst according to claim 1 or the selective ammonia oxidation catalyst obtained by the preparation method according to any one of claims 2 to 8 in treating ammonia in diesel vehicle exhaust.

10. The use according to claim 9, characterized in that: The conditions for treating ammonia in diesel exhaust are: temperature 150-500℃, air velocity 100000h -1 , the gas flow rate is 300 ml / min, and the dosage of the selective ammonia oxidation catalyst is 0.15-0.20 ml.

Citation Information

Patent Citations

  • Method for oxidizing ammonia

    CN111051238A

  • Titanium-tin composite oxide loaded noble metal catalyst and preparation method thereof

    CN111185156A

  • Method for preparing ammoxidation catalyst based on impregnation method

    CN112691661A

  • Production of catalyst and denitration method

    JP1979083696A