Low-temperature high-activity ammonia decomposition hydrogen production catalyst as well as preparation method and application thereof

By using rare earth metal oxide Pr6O11 carrier and alkali metal cocatalyst to prepare nano-Ru particles, the problem of poor activity of existing catalysts at low temperatures is solved, and efficient ammonia decomposition hydrogen production is realized. It has the characteristics of low cost and high activity, and is suitable for hydrogen production. Can be applied.

CN118788337APending Publication Date: 2024-10-18SHANGHAI JIAOTONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410995793.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing ammonia decomposition hydrogen production catalysts have poor activity at low temperatures and high costs, making it difficult to achieve efficient and low-energy ammonia decomposition reactions.

Method used

Rare earth metal oxide Pr6O11 is used as a carrier, combined with Ru and alkali metals (such as K, Na, Cs) as cocatalysts, and nano-Ru particles are prepared through ultrasonic, stirring, drying, calcination and other steps to form a low-temperature and highly active ammonia decomposition hydrogen production catalyst. , the loaded metal particles are small in size and have good dispersion.

Benefits of technology

The decomposition rate of NH3 reaches 74.3% at 350°C and 93.0% at 400°C, which significantly improves the activity and stability of the catalyst, reduces the preparation cost, and has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788337A_ABST
    Figure CN118788337A_ABST
Patent Text Reader

Abstract

The invention relates to an ammonia decomposition hydrogen production catalyst and a preparation method and application thereof in the technical field of thermocatalytic ammonia decomposition hydrogen production, the catalyst comprises an active component, a carrier and a cocatalyst, the active component is Ru, the carrier is a rare earth metal oxide Pr6O11, the cocatalyst is one of alkali metals (Na, K and Cs), and the mass fraction of the active component is 5 wt%. Preferably, the catalyst is prepared by combining a modified colloid precipitation method with a wet impregnation method, and finally the low-temperature high-activity ammonia decomposition hydrogen production catalyst is prepared. The catalyst is filled in a quartz tube of an ammonia decomposition hydrogen production reaction device, and is subjected to ammonia decomposition hydrogen production reaction after high-temperature reduction in an NH3 atmosphere. The prepared catalyst has the advantages of high activity, high dispersity and low precious metal content, has wide industrial application prospects, and is beneficial to realizing blue drawings of ammonia hydrogen green circular economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst in the technical field of thermal catalytic ammonia decomposition to hydrogen production, in particular to a low-temperature high-activity ammonia decomposition to hydrogen production catalyst with small metal particle size and good dispersibility, and a preparation method and application thereof. Background Art

[0002] In order to give full play to the advantages of hydrogen's high energy density and green and pollution-free products, promote global energy industry reform, and achieve carbon neutrality and carbon peak goals, economical and efficient hydrogen fuel cell technology as well as safe and efficient hydrogen storage and transportation methods urgently need to be developed.

[0003] Ammonia has unique advantages as a hydrogen storage carrier: (1) it can be stored and transported in liquid form at room temperature and 0.8 MPa; (2) it has a considerable volume energy density (11.38 MJ·L -1 ) and hydrogen mass fraction (17.8%); (3) have a small explosion limit (16%-25%) and high safety; (4) have mature and complete ammonia production facilities and storage and transportation infrastructure; (5) the hydrogen production process has zero carbon emissions and low post-processing costs. Therefore, optimizing ammonia decomposition hydrogen production technology provides an effective way to solve the problems of high hydrogen storage and transportation costs and poor supply system flexibility.

[0004] From a thermodynamic point of view, at 673K ​​and 1 standard atmosphere, the theoretical decomposition rate of ammonia decomposition reaction can reach 99.9%, but the high energy consumption, high equipment quality requirements and high equipment manufacturing cost have promoted the development of catalysts for ammonia decomposition reaction. Ru-based catalysts are currently the most excellent type of catalysts, but as a precious metal, their low reserves and high cost limit their application in large-scale industrialization. Therefore, it is of great value to develop low-temperature, low-Ru content, and high-catalytic activity ammonia decomposition hydrogen production catalysts.

[0005] In recent years, the field of hydrogen production by ammonia decomposition has received increasing attention and importance. Many research results show that the type of carrier has an important influence on catalytic activity. The interaction between metal and suitable carrier helps to improve the dispersion and stability of Ru. Electronic conductive carrier materials with large surface area and alkaline surface groups are most active for Ru-based catalysts. Therefore, CNT, SiO2, porous Al2O3, metal oxides, etc. are usually selected. Zhejiang University of Technology studied that the decomposition rate of 4% Ru / La2Ce2O7 at 400°C can be increased to 88.18% when the metal composite oxide M2Ce2O7 is used as a carrier, but the use of organic solvents in the preparation process may pose a safety hazard [CN 111939907 A]. In order to overcome the problems of poor low-temperature activity and poor stability, the National Engineering Research Center for Fertilizer Catalysts of Fuzhou University used a colloidal precipitation method to prepare a Ru-based catalyst with ZrO2 as a carrier. The decomposition rate of ammonia reached 95.5% at 530°C, which improved the low-temperature activity of the catalyst, but the decomposition temperature was still high and the energy consumption was large [CN 113058595 A]. The Dalian Institute of Chemical Physics of the Chinese Academy of Sciences used magnesium oxalate as a carrier precursor and adopted a deposition precipitation method to prepare a highly efficient ruthenium-based catalyst having good stability. It can stably react for 259 hours at 450°C while its activity remains basically unchanged. However, this invention does not involve its catalytic performance at low temperatures [CN 112387274 A].

[0006] In summary, although many research advances have been made in catalytic activity and stability, there is still no existing ammonia decomposition hydrogen production catalyst that is truly low-cost and has high activity and high stability at low temperatures. Therefore, it is necessary to develop a new ammonia decomposition hydrogen production catalyst to meet the above requirements, which is of great significance for promoting the development of ammonia decomposition hydrogen production technology and the application of hydrogen energy. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention proposes the preparation and application of a low-temperature, high-activity ammonia decomposition hydrogen production catalyst, which, on the one hand, meets the requirements of low-temperature, high efficiency, stable structure and low loading; at the same time, the preparation process of the method is simple, the cost is low, and it is easy to achieve scale-up production, thus having good industrial application prospects.

[0008] The present invention is achieved through the following technical solutions:

[0009] The present invention provides a low-temperature high-activity ammonia decomposition hydrogen production catalyst, comprising an active component, a carrier and a promoter, wherein the active component is Ru and the carrier is a rare earth metal oxide Pr6O 11 , the co-catalyst is an alkali metal.

[0010] Furthermore, in the present invention, the co-catalyst is one of K, Na and Cs.

[0011] Furthermore, in the present invention, the particle size of the catalyst is 40-60 mesh.

[0012] The present invention also provides a method for preparing a low-temperature high-activity ammonia decomposition hydrogen production catalyst, comprising the following steps:

[0013] S1: Evenly dissolving the Ru precursor in a certain amount of solvent to prepare a Ru solution of a specified concentration;

[0014] S2: Take a certain amount of Pr6O 11 The powder was placed in deionized water and ultrasonically stirred at room temperature to obtain a uniformly dispersed Pr6O 11 A carrier solution is prepared, and a certain amount of an alkali metal solution is added dropwise to the carrier solution, followed by stirring, drying, and calcining to obtain a modified carrier;

[0015] S3: placing the modified support in a certain amount of deionized water, stirring until uniformly dispersed, adding a certain volume of Ru solution, continuing to stir for a period of time and sequentially performing separation, washing, drying, calcining, tableting, grinding, and sieving operations to obtain a low-temperature and high-activity ammonia decomposition hydrogen production catalyst.

[0016] Furthermore, in the above step S1, the Ru precursor is RuCl3, Ru(OH)3, Ru3(CO) 12 One of them.

[0017] Furthermore, when the Ru precursor is Ru3(CO) 12 In step S1, a Ru precursor is uniformly dissolved in tetrahydrofuran; in step S3, a specified amount of Ru solution is added dropwise to the modified carrier, and stirring, rotary evaporation, drying, calcination, tableting, grinding, and sieving are performed in sequence to obtain a low-temperature and high-activity ammonia decomposition hydrogen production catalyst.

[0018] Furthermore, in the above step S2, the molar ratio of the added amount of alkali metal to the active component Ru is 1:1; the stirring treatment time after adding the alkali metal solution is 48 hours; the temperature of the drying treatment is 80°C, and the time is 48 hours; the gas environment of the calcination treatment is Ar; the temperature of the calcination treatment is 300°C; and the calcination treatment time is 1 hour.

[0019] Furthermore, in the above step S3, the mass fraction of the active component Ru is 5wt% with the mass of the modified carrier as the reference standard; the stirring time is 48 hours; the deionized water washing number is not less than three times; the drying temperature is 80°C; the calcination operation temperature is 300°C, and the time is 1 hour.

[0020] The present invention also provides an application of the catalyst, wherein the catalyst is used for decomposing ammonia to prepare hydrogen.

[0021] Furthermore, in the application of the above catalyst, the catalyst is loaded into a quartz tube of an ammonia decomposition hydrogen production reaction device, and then the ammonia decomposition hydrogen production reaction is carried out after high-temperature reduction under NH3 atmosphere.

[0022] Compared with the prior art, the beneficial effects of the present invention are:

[0023] The present invention adopts Pr6O with high-density basic sites and abundant oxygen vacancies. 11 As a catalyst carrier, the interaction with Ru is beneficial to adjust the electronic properties of Ru nanoparticles and improve the intrinsic activity of the catalyst. Furthermore, Ru is loaded onto Pr6O modified by alkali metals (Na, K, Cs). 11 It is an effective way to increase the decomposition rate of NH3, and the stronger the alkalinity, the more obvious the effect on improving the catalyst activity.

[0024] The present invention adopts ethylene glycol reduction method to prepare nano-Ru colloidal solution, converts RuCl3 into Ru(OH)3 and then loads it on Pr6O 11 Compared with RuCl3, the catalyst obtained by the method has better catalytic activity for ammonia decomposition reaction. 12 The ammonia decomposition catalyst prepared for the Ru precursor showed the best catalytic activity. The test results showed that the NH3 decomposition rate reached 74.3% at 350°C and 93.0% at 400°C. The supported metal particles prepared by this preparation method have small size and good dispersibility, and show better activity in the ammonia decomposition hydrogen production reaction. It is a low-temperature and high-activity ammonia decomposition hydrogen production catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A curve diagram showing the decomposition rate of NH3 in ammonia decomposition hydrogen production reaction using the catalysts prepared in Examples 1, 2 and 3 of the present invention;

[0026] Figure 2 This is a curve diagram of the NH3 decomposition rate in the ammonia decomposition hydrogen production reaction using the catalysts prepared in Examples 3, 4 and 5 of the present invention. DETAILED DESCRIPTION

[0027] In order to make the contents of the present invention easier to understand, the technical scheme of the present invention is further explained below in conjunction with specific embodiments. The examples are only used to illustrate the present invention, but the present invention is not limited to the contents. The operation methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the product instructions. The chemical reagents without specifying the manufacturer are all conventional drugs that comply with national standards and can be purchased on the market.

[0028] Example 1

[0029] Weigh 0.15g of RuCl3 and dissolve it in ethylene glycol, and then add it to a 50mL volumetric flask. -1 NaOH was added to the above solution under magnetic stirring and stirred for 30 minutes. The salt solution was then refluxed at 160° C. for 3 hours to obtain a dark brown nano-Ru colloidal solution.

[0030] Weigh 2.0 g Pr6O 11 The powder was uniformly dispersed in deionized water by ultrasonication and stirring. 0.04 g of NaOH was then added to the solution and stirred at 500 r·min -1 The mixture was stirred for 48 hours, and the obtained reactant was dried at 60°C for 48 hours, and then Ar was introduced to calcine the obtained product for 1 hour to obtain alkali metal Na-modified Pr6O 11 carrier.

[0031] The nano-Ru colloidal solution was measured and added dropwise to the prepared Na-modified Pr6O 11 carrier and at 500r·min -1 The product was then dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-particle ratio, which was finally obtained by tableting to obtain Na / Ru(OH)3 / Pr6O 11 Catalyst samples.

[0032] Example 2

[0033] Weigh 0.15g of RuCl3 and dissolve it in ethylene glycol, and then add it to a 50mL volumetric flask. -1 NaOH was added to the above solution under magnetic stirring and stirred for 30 minutes. The salt solution was then refluxed at 160° C. for 3 hours to obtain a dark brown nano-Ru colloidal solution.

[0034] Weigh 2.0 g Pr6O 11 The powder was uniformly dispersed in deionized water by ultrasonication and stirring. 0.055 g KOH was added to the solution and stirred at 500 r·min -1 The reaction mixture was stirred for 48 hours at 60 °C, and the obtained product was dried for 48 hours, and then Ar was introduced to calcine the obtained product for 1 hour to obtain alkali metal K-modified Pr6O 11 carrier.

[0035] Take the nano-Ru colloidal solution and add it dropwise to the prepared K-modified Pr6O 11 carrier and at 500r·min -1The mixture was stirred for 48 hours. Then, the obtained product was dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio. The mixture was pressed into tablets to obtain K / Ru(OH)3 / Pr6O 11 Catalyst samples.

[0036] Example 3

[0037] Weigh 0.15 g of RuCl3 and dissolve it in ethylene glycol, and then add it to a 50 mL volumetric flask. -1 NaOH was added to the above solution under magnetic stirring and stirred for 30 minutes. The salt solution was then refluxed at 160° C. for 3 hours to obtain a dark brown nano-Ru colloidal solution.

[0038] Weigh 2.0 g Pr6O 11 The powder was uniformly dispersed in deionized water by ultrasonication and stirring. 0.3 g of CsOH solution (50 wt%) was then dropped into the carrier solution and the mixture was stirred at 500 r·min. -1 The reaction mixture was stirred for 48 hours at 60 °C, and the obtained product was dried for 48 hours, and then Ar was introduced to calcine the obtained product for 1 hour to obtain alkali metal Cs-modified Pr6O 11 carrier.

[0039] The nano-Ru colloidal solution was measured and added dropwise to the prepared Cs-modified Pr6O 11 carrier and at 500r·min -1 The product was then dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio, which was finally obtained by tableting to obtain Cs / Ru(OH)3 / Pr6O 11 Catalyst samples.

[0040] Example 4

[0041] Weigh 0.15 g of RuCl3 and dissolve it in a certain amount of deionized water, and make up to volume in a 50 mL volumetric flask.

[0042] Weigh 2.0 g Pr6O 11 The powder was uniformly dispersed in deionized water by ultrasonication and stirring. 0.3 g of CsOH solution (50 wt%) was then dropped into the carrier solution and the mixture was stirred at 500 r·min. -1 The mixture was stirred for 48 hours, and the obtained reactant was dried at 60°C for 48 hours, and then Ar was introduced to calcine the obtained product for 1 hour to obtain alkali metal Cs-modified Pr6O 11 carrier.

[0043] The RuCl3·xH2O solution was measured and added dropwise to the prepared Cs-modified Pr6O 11 carrier and at 500r·min -1 The product was then dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-particle ratio, which was finally obtained by tableting to obtain Cs / RuCl3 / Pr6O 11 Catalyst samples.

[0044] Example 5

[0045] Weigh 2.0 g Pr6O 11 The powder was uniformly dispersed in deionized water by ultrasonication and stirring. 0.3 g of CsOH solution (50 wt%) was then dropped into the carrier solution and the mixture was stirred at 500 r·min. -1 The mixture was stirred for 48 hours, and the obtained reactant was dried at 60°C for 48 hours, and then Ar was introduced to calcine the obtained product for 1 hour to obtain alkali metal Cs-modified Pr6O 11 carrier.

[0046] Measure 0.15g Ru3(CO) 12 Dissolved in tetrahydrofuran (THF) and stirred at 500 r·min -1 The prepared Cs-modified Pr6O was added to the above solution under magnetic stirring. 11 The carrier was stirred for 12 hours and then vacuumed and rotary evaporated in a rotary evaporator. The resulting precipitate was then dried at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio, which was finally obtained by tableting to obtain Cs / Ru3(CO) 12 / Pr6O 11 Catalyst samples.

[0047] Comparative Example 1

[0048] Weigh 0.15g RuCl3 and dissolve it in a certain amount of deionized water, and then add it to a 50mL volumetric flask. Add the RuCl3·xH2O solution dropwise to 2.0g Pr6O 11 In the carrier and at 500r·min -1 The product was then dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio, which was finally obtained by tableting. 11 Catalyst samples.

[0049] Comparative Example 2

[0050] Weigh 0.15g of RuCl3 and dissolve it in ethylene glycol, and then add it to a 50mL volumetric flask. -1 NaOH was added to the above solution under magnetic stirring and stirred for 30 minutes. The salt solution was then refluxed at 160° C. for 3 hours to obtain a dark brown nano-Ru colloidal solution.

[0051] Take the nano-Ru colloidal solution and add it dropwise to 2.0 g Pr6O 11 carrier and at 500r·min -1 The product was then dried in air at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio, which was finally obtained by tableting to obtain Ru(OH)3 / Pr6O 11 Catalyst samples.

[0052] Comparative Example 3

[0053] Measure 0.15g Ru3(CO) 12 Dissolved in tetrahydrofuran (THF) and stirred at 500 r·min -1 2.0 g Pr6O was added to the above solution under magnetic stirring. 11 The powder was stirred for 12 hours and then vacuumed and rotary evaporated in a rotary evaporator. The resulting precipitate was then dried at 80°C for 24 hours and calcined at 300°C for 1 hour to obtain a mixture with a certain powder-to-particle ratio, which was finally obtained by tableting to obtain Ru3(CO) 12 / Pr6O 11 Catalyst samples.

[0054] Application Example 1

[0055] In order to better illustrate the catalytic effect of the present invention, the catalytic activity of the ammonia decomposition catalyst prepared in Example 1-X was tested in an SCR reaction system. The test process is as follows:

[0056] Take 0.5g of the catalyst (40-60 mesh) in the SCR reaction tube and pass 16mL min -1 NH3, ensuring the experimental space velocity is 2,000 mL·h -1 ·g cat -1 The experimental examples were pre-treated at 550°C.

[0057] Furthermore, the pretreatment duration is 1 hour.

[0058] The results of recording the NH3 decomposition rate of the catalyst at temperatures of 250°C, 300°C, 350°C, 400°C, 450°C, 500°C and 550°C are shown in Table 1.

[0059] Table 1 Activity evaluation results of examples and comparative examples

[0060]

[0061] The activity test results of samples in Examples 1, 2 and 3 of the present invention are as follows Figure 1 As shown in the figure, different types of alkali metal modification have different effects on the catalytic ammonia decomposition activity of Ru-based catalysts with the same content, among which the improvement effect is: Cs>K>Na, which is far better than the unmodified comparative example 2. This shows that the stronger the alkalinity, the stronger the promoting effect of the alkali metal on the catalyst. Cs has a stronger effect on Ru / Pr6O 11 As for catalysts, alkali metal additives have the best promoting effect.

[0062] Figure 2 The activity test curves of Examples 3, 4, and 5 obtained from different Ru precursors under Cs modification are shown. As shown in the figure, the activities of the examples obtained from different Ru precursors are different, among which the optimization effect is: Ru3(CO) 12 >Ru(OH)3>RuCl3, which is consistent with the results shown in Comparative Examples 1, 2, and 3. The strong attraction of Cl ions to electrons and the electron donation of carbonyl ligands adjust the electronic structure of Ru, which is believed to be the reason for this result.

[0063] Combining Table 1 and Figure 2 It can be seen that the Ru3(CO) prepared by the present invention 12 / Cs / Pr6O 11 The sample has a higher catalytic ammonia decomposition activity than other examples, with an NH3 decomposition rate of 74.3% at 350°C and 93.0% at 400°C, showing broad prospects for industrial application.

[0064] The above description is only a preferred embodiment of the present invention. Any equivalent changes and modifications made by any technician familiar with the profession within the scope of the patent application of the present invention also belong to the scope covered by the claims attached to the present invention.

Claims

1. A low-temperature, high-activity ammonia decomposition hydrogen production catalyst, comprising an active component, a carrier and a promoter, characterized in that The active component is Ru, and the carrier is rare earth metal oxide Pr6O 11 , the co-catalyst is an alkali metal.

2. The low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 1, characterized in that The promoter is one of K, Na and Cs.

3. The low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 1 or 2, characterized in that The particle size of the catalyst is 40-60 mesh.

4. A method for preparing a low-temperature, high-activity ammonia decomposition hydrogen production catalyst as claimed in any one of claims 1 to 3, characterized in that The following steps are involved: S1: Evenly dissolving the Ru precursor in a certain amount of solvent to prepare a Ru solution of a specified concentration; S2: Take a certain amount of Pr6O 11 The powder was placed in deionized water and ultrasonically stirred at room temperature to obtain a uniformly dispersed Pr6O 11 A carrier solution is prepared, and a certain amount of an alkali metal solution is added dropwise to the carrier solution, followed by stirring, drying, and calcining to obtain a modified carrier; S3: placing the modified support in a certain amount of deionized water, stirring until uniformly dispersed, adding a certain volume of Ru solution, continuing to stir for a period of time and sequentially performing separation, washing, drying, calcining, tableting, grinding, and sieving operations to obtain a low-temperature and high-activity ammonia decomposition hydrogen production catalyst.

5. The method for preparing a low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 4, characterized in that In step S1, the Ru precursor is RuCl3, Ru(OH)3, Ru3(CO) 12 One of them.

6. The method for preparing a low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 5, characterized in that When the Ru precursor is Ru3(CO) 12 In step S1, a Ru precursor is uniformly dissolved in tetrahydrofuran; in step S3, a specified amount of Ru solution is added dropwise to the modified carrier, and stirring, rotary evaporation, drying, calcination, tableting, grinding, and sieving are performed in sequence to obtain a low-temperature and high-activity ammonia decomposition hydrogen production catalyst.

7. The method for preparing a low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 4, characterized in that In step S2, the molar ratio of the added amount of the alkali metal to the active component Ru is 1:1; the stirring treatment time after adding the alkali metal solution is 48 hours; the temperature of the drying treatment is 80°C and the time is 48 hours; the gas environment of the calcination treatment is Ar; the temperature of the calcination treatment is 300°C; and the calcination treatment time is 1 hour.

8. The method for preparing a low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 4, characterized in that In step S3, the mass fraction of the active component Ru is 5wt% with the mass of the modified carrier as the reference standard; the stirring time is 48 hours; the number of washing times with deionized water is not less than three times; the drying temperature is 80°C; the calcination operation temperature is 300°C and the time is 1 hour.

9. Use of a catalyst as claimed in any one of claims 1 to 3 or a catalyst prepared by the method as claimed in any one of claims 4 to 8, characterized in that The catalyst is used for decomposing ammonia to produce hydrogen.

10. Use of the catalyst according to claim 9, characterized in that The catalyst is loaded into a quartz tube of an ammonia decomposition hydrogen production reaction device, and is reduced at high temperature in an NH3 atmosphere before undergoing an ammonia decomposition hydrogen production reaction.

Citation Information

Patent Citations

  • Titanium-based multi-metal oxide catalyst for removing diesel engine NOx by NH3-SCR in wide temperature window

    CN101898136A

  • Rare earth metal oxide supported ruthenium catalyst for ammonia decomposition to produce hydrogen and preparation and application

    CN109954493A

  • Oxidative decomposition catalyst of ammonia, hydrogen production method, and hydrogen production apparatus

    JP2014111517A

  • Ammonia decomposition catalyst, method for producing ammonia decomposition catalyst, method for producing hydrogen and apparatus for producing hydrogen

    JP2016198720A