Ru-based catalyst for hydrogen production through ammonia decomposition as well as preparation method and application of Ru-based catalyst
By using MgO carrier and alkali metal-assisted Ru-based catalyst in the ammonia decomposition hydrogen production catalyst, the problem of insufficient low-temperature catalytic activity and high cost is solved, efficient ammonia conversion rate is achieved, and the industrial application of ammonia hydrogen-carrying technology is promoted.
Patent Information
- Application Number
- CN202410995993.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-18
AI Technical Summary
Existing ammonia decomposition hydrogen production catalysts have insufficient catalytic activity at low temperatures and are expensive, which limits the industrial-scale application of ammonia hydrogen-carrying technology.
MgO is used as the carrier, and alkali metal compounds (such as sodium hydroxide, potassium hydroxide, cesium hydroxide) are used to assist the Ru-based catalyst. Ru is evenly loaded through the deposition method and the amount of alkali metal ions is adjusted to improve the dispersion of the catalyst. and activity.
The high ammonia conversion rate reaches 72.15% at 350°C and 93.85% at 400°C, which reduces the cost of the catalyst and improves the dispersion and activity of the metal, and has good industrial application prospects.
Smart Images

Figure CN118788338A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst in the technical field of thermal catalytic ammonia decomposition to produce hydrogen, in particular to a Ru-based catalyst with good metal dispersion and high catalytic activity for ammonia decomposition to produce hydrogen, and a preparation method and application thereof. Background Art
[0002] Green hydrogen produced from renewable energy and nuclear energy is considered to be the ultimate solution to the increasingly scarce and expensive fossil fuels. To solve the problems of low hydrogen density, high storage cost and low transportation efficiency, and to give full play to its advantages of high energy density and pollution-free products, it is urgent to develop efficient and safe hydrogen storage materials in order to clear the bottlenecks in the hydrogen energy industry chain and promote the large-scale and industrialized utilization of hydrogen energy, but this is also the main technical obstacle at present. In order to achieve large-scale storage and transportation, researchers have proposed the "Power-to-X" process, which is the process of using renewable energy to electrolyze water to produce green hydrogen, and then further converting green hydrogen into liquid fuels (such as methanol, methane, ammonia, etc.).
[0003] Among them, ammonia has been used as fertilizer and refrigerant gas for more than 100 years, and the infrastructure for ammonia production, storage and transportation has been improved. Compared with other hydrogen storage carriers, ammonia has unique advantages such as high hydrogen storage density, high volume energy density, and low comprehensive cost of the whole process from source to tank, and has broad application prospects. The key to the application and promotion of ammonia hydrogen-carrying technology lies in solving the problem of ammonia decomposition hydrogen production catalyst, especially the low catalytic activity and high cost under mild conditions. A large number of research results show that Ru has the best performance among existing catalysts, but the disadvantages of high cost and low reserves of precious metal Ru still restrict the large-scale application of ruthenium-based catalysts. Transition metals Ni, Fe, etc. are currently commonly used catalysts for industrial ammonia decomposition hydrogen production, but their operating temperature needs to be above 800°C to achieve the desired ammonia conversion rate and hydrogen production. The huge consumption and waste of energy, as well as the strict quality requirements and high manufacturing costs for production equipment are still very difficult problems.
[0004] The carrier helps to fix the active components and improve the dispersion of the metal through the interaction with the metal. By adjusting the size and morphology of the loaded metal particles, the number of active sites exposed by the metal particles can be changed. Chinese patent CN116139859A uses carbon-encapsulated silicon dioxide SiO2@C as a catalyst carrier. The prepared catalyst achieves an ammonia conversion rate of 94.5% at 550°C, but its preparation method is still relatively complicated.
[0005] Alkali metals are a common type of co-catalyst, and have been proven to be effective promoters of supported Ru catalysts due to their electron-donating effect. By increasing the density of basic sites on the Ru surface, nitrogen atoms are more easily associated and desorbed, thereby greatly enhancing the NH3 decomposition activity. Patent CN 114471553 A discloses the preparation and application of a rare earth modified catalyst for hydrogen production from ammonia decomposition. The method uses rare earth element yttrium and alkali metal potassium as co-agents to prepare a Ru-based catalyst, which effectively inhibits H2 poisoning on Ru. The NH3 conversion rate can reach 95.4% at 430°C. It has good low-temperature catalytic activity and a simple preparation method, but the addition of rare earth metals makes the cost issue more prominent.
[0006] In summary, Ru-based catalysts have excellent performance that other catalysts cannot match, and selecting a suitable combination of carrier and co-catalyst is an effective way to further enhance the catalytic activity of Ru, improve dispersion, and reduce costs. Therefore, the development of a Ru-based catalyst for hydrogen production from ammonia decomposition is of great practical significance. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention proposes a Ru-based catalyst for hydrogen production by decomposing ammonia, a preparation method and an application thereof. MgO with economical advantages is used as a carrier, and the Ru-based catalyst is modified with an alkali metal to solve the problems of insufficient activity at low temperatures and high costs in the prior art, and promote industrial-scale applications.
[0008] The present invention is achieved through the following technical solutions:
[0009] The invention provides a Ru-based catalyst for hydrogen production by decomposing ammonia, comprising an active component, a carrier and a co-catalyst, wherein the active component is Ru, the carrier is MgO, and the co-catalyst is an alkali metal compound.
[0010] Furthermore, in the present invention, one of sodium hydroxide, potassium hydroxide and cesium hydroxide.
[0011] Furthermore, in the present invention, compared with the molar mass of Ru, the amount of the co-catalyst added is 1-20 times that of Ru.
[0012] Furthermore, in the present invention, the particle size of the catalyst is 40-60 mesh.
[0013] The present invention also provides a method for preparing a Ru-based catalyst for hydrogen production by decomposing ammonia, comprising the following steps:
[0014] S1: Evenly mix the Ru precursor solution with a certain amount of HNO3, then take a certain amount of MgO powder and deionized water, dilute and stir;
[0015] S2: taking a certain amount of urea and placing it in the solution of S1, and then stirring, aging, filtering, washing, and drying in sequence to obtain an initial product;
[0016] S3: Take a certain amount of the initial product described in S2, add it into a certain amount of alkali metal solution under stirring, and then perform stirring, drying and calcination operations in sequence to obtain a Ru-based catalyst for hydrogen production by decomposing ammonia.
[0017] Furthermore, in the above step S1, the precursor solution is a RuCl3·xH2O aqueous solution prepared with a certain amount of RuCl3 powder, and the stirring is to put the diluted suspension into a magnetic stirrer at room temperature for 1 hour.
[0018] Furthermore, in the above step S2, taking the mass of the carrier as a reference standard, the mass fraction of the active component Ru is 5wt%, and the molar amount of the added precipitant urea should be 200 times the molar amount of the active component Ru; the stirring treatment time is 8 hours, and the reaction temperature is 80°C; the aging treatment is carried out at room temperature for 12 hours; the washing treatment uses deionized water for washing for no less than three times; and the drying treatment temperature is 80°C.
[0019] Furthermore, in the above step S3, the molar ratio of the added amount of alkali metal to the active component Ru is 1 to 20; the stirring treatment time after adding the alkali metal solution is 48 hours; the temperature of the drying treatment is 80°C and the time is 24 hours; the gas environment of the calcination treatment is Ar; the temperature of the calcination treatment is 300°C; and the calcination treatment time is 2 hours.
[0020] The present invention also provides an application of the above catalyst, wherein the catalyst is used for decomposing ammonia to prepare a CO-free x (x=1 or 2) of hydrogen.
[0021] Furthermore, in the application of the above catalyst, the catalyst is loaded into a quartz tube of an ammonia decomposition hydrogen production reaction device, and then the ammonia decomposition hydrogen production reaction is carried out after high-temperature reduction under NH3 atmosphere.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] The present invention adopts a deposition precipitation method to uniformly load Ru on a MgO carrier and add alkali metal ions for modification. The prepared Ru-based catalyst exhibits a high ammonia conversion rate of 72.15% at 350°C and 93.85% at 400°C. The interaction between Ru and the MgO carrier can fix the active components and improve the dispersibility of the metal. Furthermore, the addition of alkali metal ions increases the density of alkaline sites, promotes the interaction between the metal and the carrier, and thus further improves the catalytic activity. However, when the alkali metal ions are excessively added, part of the Ru sites will be covered, resulting in a decrease in catalytic activity. Therefore, it is very meaningful to adjust the doping amount of the co-catalyst.
[0024] The preparation method of the present invention is conducive to reducing the concentration of active metal ions, avoiding excessive growth of crystals during the aging process, and the metal particles have high dispersion and narrow particle size distribution, thereby increasing the number of active sites.
[0025] The catalyst provided by the present invention can be applied to the field of hydrogen production by decomposing ammonia and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A curve diagram showing the conversion rate of NH3 in ammonia decomposition hydrogen production reaction using the catalysts prepared in Comparative Example 1 and Experimental Examples 1, 2, 3, and 4 of the present invention;
[0027] Figure 2 A curve diagram showing the conversion rate of NH3 in ammonia decomposition hydrogen production reaction using the catalysts prepared in Comparative Example 1 and Experimental Examples 5, 6, 7, 8, and 9 of the present invention;
[0028] Figure 3 This is a curve chart of the NH3 conversion rate in the ammonia decomposition hydrogen production reaction using the catalysts prepared in Comparative Example 1 and Experimental Examples 10, 11, 12, 13, and 14 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the contents of the present invention easier to understand, the technical scheme of the present invention is further explained below in conjunction with specific embodiments. The examples are only used to illustrate the present invention, but the present invention is not limited to the contents. The operation methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the product instructions. The chemical reagents without specifying the manufacturer are all conventional drugs that comply with national standards and can be purchased on the market.
[0030] Example 1
[0031] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0032] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0033] A certain amount of the obtained product and 50wt% CsOH solution were measured, and the molar ratio of the added amount of alkali metal to the active component Ru was 1:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was pressed, ground, and sieved to finally obtain a 1-Cs / Ru / MgO sample.
[0034] Example 2
[0035] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0036] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0037] A certain amount of the obtained reduction product and 50wt% CsOH solution were measured, and the molar ratio of the amount of alkali metal added to the active component Ru was 2:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was pressed, ground, and sieved to finally obtain a 2-Cs / Ru / MgO sample.
[0038] Example 3
[0039] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0040] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0041] A certain amount of the obtained reduction product and 50wt% CsOH solution were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 3:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 3-Cs / Ru / MgO sample.
[0042] Example 4
[0043] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0044] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0045] A certain amount of the obtained reduction product and 50wt% CsOH solution were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 4:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 4-Cs / Ru / MgO sample.
[0046] Example 5
[0047] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0048] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0049] A certain amount of the obtained reduction product and KOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 1:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was pressed, ground, and sieved to finally obtain a 1-K / Ru / MgO sample.
[0050] Example 6
[0051] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0052] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0053] A certain amount of the obtained reduction product and KOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 3:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was pressed, ground, and sieved to finally obtain a 3-K / Ru / MgO sample.
[0054] Example 7
[0055] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0056] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0057] A certain amount of the obtained reduction product and KOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 8:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 8-K / Ru / MgO sample.
[0058] Example 8
[0059] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0060] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0061] A certain amount of the obtained reduction product and KOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 17:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 17-K / Ru / MgO sample.
[0062] Example 9
[0063] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0064] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0065] A certain amount of the obtained reduction product and KOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 20:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was pressed, ground, and sieved to finally obtain a 20-K / Ru / MgO sample.
[0066] Example 10
[0067] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0068] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0069] A certain amount of the obtained reduction product and NaOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 1:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 1-Na / Ru / MgO sample.
[0070] Embodiment 11
[0071] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0072] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0073] A certain amount of the obtained reduction product and NaOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 3:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 3-Na / Ru / MgO sample.
[0074] Example 12
[0075] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0076] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0077] A certain amount of the obtained reduction product and NaOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 8:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain the 8-Na / Ru / MgO sample.
[0078] Example 13
[0079] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0080] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0081] A certain amount of the obtained reduction product and NaOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 20:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 20-Na / Ru / MgO sample.
[0082] Embodiment 14
[0083] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0084] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 1000 °C for 8 hours. After being taken out, the mixture was aged at room temperature, and then filtered, washed and dried in sequence to obtain the precipitate in the solution.
[0085] A certain amount of the obtained reduction product and NaOH were measured, and the molar ratio of the addition amount of alkali metal to the active component Ru was 25:1. After adding an appropriate amount of deionized water and stirring for 24 hours, it was dried at 80°C for 48 hours. Subsequently, the temperature was raised to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground, and sieved to finally obtain a 25-Na / Ru / MgO sample.
[0086] Comparative Example 1
[0087] A specified amount of RuCl3 powder was weighed and dissolved in a certain amount of deionized water to prepare a RuCl3·xH2O solution, and a small amount of HNO3 was added, wherein the ratio of the molar amount of HNO3 added to the molar amount of the active component Ru was 1:10. The mixed solution was mixed with a certain amount of MgO powder, and the precipitate was stirred at room temperature for 1 hour to keep it in suspension.
[0088] Weigh urea with a molar ratio of 1:200 to the added RuCl3, and heat the mixed solution at 80°C and 550 r·min -1 The mixture was stirred at a speed of 100°C for 8 hours. After being taken out, it was aged at room temperature, filtered, washed and dried in sequence to obtain the precipitate in the solution. The mixture was then heated to 300°C in a muffle furnace and calcined for 2 hours. The obtained product was tableted, ground and sieved to obtain a Ru / MgO sample.
[0089] Application Example 1
[0090] In order to better illustrate the catalytic effect of the present invention, the catalytic activity of the ammonia decomposition catalysts prepared in Comparative Example 1 and Examples 1-14 was tested in an SCR reaction system. The test process is as follows:
[0091] Take 0.5g of the catalyst (40-60 mesh) in the SCR reaction tube and pass 16mL min -1 100% NH3, ensuring the experimental space velocity is 2,000 mL·h -1 ·g cat -1 The experimental examples were pre-treated at 550°C.
[0092] Furthermore, the pretreatment duration is 1 hour.
[0093] The results of recording the NH3 decomposition rate of the catalyst at temperatures of 250°C, 300°C, 350°C, 400°C, 450°C, 500°C and 550°C are shown in Table 1.
[0094] The activity test results of the samples described in the present invention are as follows Figure 1 , 2 As shown in Figure 3, alkali metals Cs, K, and Na can all improve the catalytic activity of the catalyst, and the optimal ratio of the input amount of alkali metal to Ru is Cs:Ru=2:1, K:Ru=17:1, and Na:Ru=20:1.
[0095] Combining Table 1 and Figure 1 , 23 It can be seen that the 17-K / Ru / MgO sample prepared in the present invention has a higher catalytic ammonia decomposition activity than other embodiments, with an NH3 decomposition rate of 72.15% at 350°C and 93.85% at 400°C, which has broad industrial application prospects.
[0096] Table 1 Activity evaluation results of examples and comparative examples
[0097]
[0098]
[0099] The above description is only a preferred embodiment of the present invention. Any equivalent changes and modifications made by any technician familiar with the profession within the scope of the patent application of the present invention also belong to the scope covered by the claims attached to the present invention.
Claims
1. A Ru-based catalyst for hydrogen production by decomposing ammonia, comprising an active component, a carrier and a promoter, Features The active component is Ru, the carrier is MgO, and the promoter is an alkali metal compound.
2. The low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 1, Features The co-catalyst is one of sodium hydroxide, potassium hydroxide and cesium hydroxide.
3. The low-temperature, high-activity ammonia decomposition hydrogen production catalyst according to claim 1 or 2, Features Compared to the molar mass of Ru, the amount of the co-catalyst added is 1-20 times that of Ru.
4. The Ru-based catalyst for hydrogen production by decomposing ammonia according to any one of claims 1 to 3, Features The particle size of the catalyst is 40-60 mesh.
5. A method for preparing a Ru-based catalyst for hydrogen production by decomposing ammonia according to any one of claims 1 to 4, Features The following steps are involved: S1: Mix Ru precursor solution with a certain amount of HNO 3 Mix evenly, then take a certain amount of MgO powder and deionized water, dilute and stir; S2: taking a certain amount of urea and placing it in the solution of S1, and then stirring, aging, filtering, washing, and drying in sequence to obtain an initial product; S3: Take a certain amount of the initial product described in S2, add it into a certain amount of alkali metal solution under stirring, and then perform stirring, drying and calcination operations in sequence to obtain a Ru-based catalyst for hydrogen production by decomposing ammonia.
6. The method for preparing the Ru-based catalyst for hydrogen production by decomposing ammonia according to claim 5, It is characterized in that In step S1, the precursor solution is a certain amount of RuCl 3 RuCl powder 3 ·xH 2 O aqueous solution, wherein the stirring is to place the diluted suspension in a magnetic stirrer at room temperature for 1 hour.
7. The method for preparing the Ru-based catalyst for hydrogen production by decomposing ammonia according to claim 5, It is characterized in that In step S2, taking the mass of the carrier as a reference standard, the mass fraction of the active component Ru is 5wt%, and the molar amount of the added precipitant urea should be 200 times the molar amount of the active component Ru; the stirring treatment time is 8 hours, and the reaction temperature is 80°C; the aging treatment is carried out at room temperature for 12 hours; the washing treatment uses deionized water for washing for no less than three times; the drying treatment temperature is 80°C.
8. The method for preparing the Ru-based catalyst for hydrogen production by decomposing ammonia according to claim 5, It is characterized in that In step S3, the molar ratio of the added amount of alkali metal to the active component Ru is 1 to 20; the stirring treatment time after adding the alkali metal solution is 48 hours; the temperature of the drying treatment is 80°C and the time is 24 hours; the gas environment of the calcination treatment is Ar; the temperature of the calcination treatment is 300°C; and the calcination treatment time is 2 hours.
9. Use of a catalyst as claimed in any one of claims 1 to 4 or a catalyst prepared by the method as claimed in any one of claims 5 to 8, Features The catalyst is used for decomposing ammonia to prepare CO-free x (x=1 or 2) of hydrogen.
10. Use of the catalyst according to claim 9, Features The catalyst is loaded into a quartz tube of an ammonia decomposition hydrogen production reaction device, and 3 After high-temperature reduction under atmosphere, ammonia is decomposed to produce hydrogen.
Citation Information
Patent Citations
Ruthenium-based ammonia synthetic catalyst and preparation thereof
CN101322938A
Magnesium oxide-supported ruthenium catalyst for hydrogen preparation through ammonia decomposition, preparation method and applications thereof
CN108160072A
Preparation method of ruthenium-based catalyst
CN111229213A
Preparation method of supported ruthenium-based catalyst
CN112387274A
Preparation method of ruthenium-base ammonia synthetic catalyst
CN1954910A
Cited By
Binuclear Ru-based ammonia cracking hydrogen production catalyst as well as preparation method and application thereof
CN119327451A
Binuclear Ru-based ammonia cracking hydrogen production catalyst and its preparation method and application
CN119327451B
Monolithic catalyst for hydrogen production through ammonia decomposition as well as preparation method and application of monolithic catalyst