Hierarchical pore catalyst for synthesizing ammonia through plasma and preparation method of hierarchical pore catalyst
By designing a hierarchical porous catalyst for plasma ammonia synthesis, using the colloidal crystal template method to prepare an oxide carrier with a macroporous-mesoporous-microporous structure and loading active components and additives, the high-temperature and high-pressure problems of the traditional ammonia synthesis process are solved. , achieving high-efficiency ammonia synthesis and low energy consumption at room temperature, and is suitable for small-scale regional ammonia synthesis industry.
Patent Information
- Application Number
- CN202410790902.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-18
AI Technical Summary
The high temperature and high pressure conditions of the traditional Haber-Bosch process for ammonia synthesis lead to high energy consumption and serious environmental pollution. The catalyst is prone to sintering and deactivation, and there is a large room for improvement in the ammonia yield of plasma catalyzed ammonia synthesis.
Design a hierarchical porous catalyst for plasma ammonia synthesis. An oxide carrier with a macroporous-mesoporous-microporous structure is prepared through a colloidal template method that combines hard templates and soft templates, and the active components are loaded through an impregnation method. and auxiliaries to form a catalyst of xM*yA*(100-x-y)C, optimizing its catalytic performance at room temperature.
It achieves efficient synthesis of ammonia at normal pressure and room temperature, improves ammonia conversion rate, reduces energy consumption, and maintains the stability and high selectivity of the catalyst. It is suitable for small-scale regional ammonia synthesis industry.
Smart Images

Figure CN118788352A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts and preparation thereof, in particular to a multi-level porous catalyst for plasma synthesis of ammonia and a preparation method thereof. Background Art
[0002] Ammonia is one of the most important raw materials in the synthesis process of chemical products and fertilizers. In recent years, it has also shown broad application prospects as an energy carrier in the field of hydrogen storage. However, the high temperature and high pressure (400-500°C, 150-250 bar) reaction conditions required by the traditional industrial ammonia synthesis industry using the Haber-Bosch process have led to a large amount of energy consumption (accounting for 2% of the world's total energy consumption) and serious environmental pollution (accounting for 1.5-2% of the world's total carbon emissions). At the same time, its harsh reaction conditions are prone to cause catalyst sintering and deactivation.
[0003] Non-thermal plasma (NTP) synergistic catalysis is an advanced technology that can activate inert molecules with strong chemical bonds under normal pressure and room temperature. This technology provides a new idea for synthesizing ammonia under mild conditions. The high-energy electrons in NTP can eliminate the equilibrium barrier shown in traditional thermal catalysis. At the same time, the combination of plasma and catalyst can effectively vibrate and excite highly stable N≡N bonds, thereby realizing the synthesis of ammonia using N2 and H2 under normal pressure and room temperature. In addition, the plasma catalytic process can achieve an instant start-stop mode, which provides greater possibilities for the small-scale regional ammonia synthesis industry coupled with intermittent renewable energy. Although the plasma catalytic ammonia synthesis process has broad prospects, there is still a lot of room for improvement in the yield of ammonia in this reaction. Summary of the invention
[0004] The purpose of the present invention is to provide a multi-level porous catalyst for plasma synthesis of ammonia and a preparation method thereof, to design a high-efficiency catalyst adapted to the plasma environment, to achieve a true combination of the significant advantages of plasma (high energy) and catalyst (high selectivity), and thus to obtain the best ammonia synthesis effect.
[0005] To achieve the above object, the present invention provides a multi-level porous catalyst for plasma synthesis of ammonia, the general formula of the multi-level porous catalyst is: xM*yA*(100-xy)C,
[0006] Wherein, M is the active component, A is the active auxiliary agent, C is the carrier, x and y represent the mass percentages of M and A respectively, and 0.1≤x≤60, 0.1≤y≤60.
[0007] Preferably, the mass percentage of the active component to the active auxiliary agent is: 20≤x≤40, 0.1≤y≤5.
[0008] Preferably, the active component M includes one or more metals and / or metal oxides selected from the group consisting of Rh, Ru, Pt, Pd, Au, Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mo and Ce, and the active auxiliary agent A includes one or more metals and / or metal oxides selected from the group consisting of Na, Mg, K, Ba and La.
[0009] Preferably, the carrier C comprises one or more of Al2O3, TiO2, CaO, ZrO2 and BaTiO3, and the micropore size of the oxide carrier in the carrier is distributed in the range of 0.5 to 2 nm, the mesopore size is distributed in the range of 4.5 to 50 nm, and the macropore size is distributed in the range of 50 to 1500 nm. The specific surface area of the oxide carrier is 100 to 500 m 2 g -1 .
[0010] The present invention provides a method for preparing a multi-level porous catalyst for plasma synthesis of ammonia, comprising the following steps:
[0011] Step 1: by combining a hard template and a soft template, an oxide support having a macroporous-mesoporous-microporous multi-level pore structure is prepared using a colloidal crystal template method;
[0012] Step 2: Load the active component M and the active auxiliary agent A on the oxide carrier by an impregnation method, and the impregnated oxide is dried and calcined to obtain a catalyst.
[0013] Preferably, the specific operation of the impregnation method is: impregnating the oxide support with the active metal precursor solution, and then obtaining the catalyst by drying and calcining, wherein the drying conditions are: rotary evaporation at 60-85°C, and then drying in an oven at 85-100°C for 7-13h, and the calcination conditions are: calcining at 400-600°C for 4-6h to obtain the catalyst.
[0014] Preferably, the method for preparing the oxide carrier comprises the following steps:
[0015] S1, using monodisperse microspheres as macroporous templates, and arranging the monodisperse microspheres into an ordered colloidal crystal template by self-assembly or sintering;
[0016] S2, mixing surfactant A, surfactant B, butyl titanate, hydrochloric acid, acetic acid and ethanol, and heating and stirring to obtain a uniform and transparent precursor sol;
[0017] S3, adding the precursor sol in S2 dropwise to the colloidal crystal template prepared in S1, and removing the microsphere colloidal crystal template by drying, calcining or solution dissolution to obtain the oxide carrier having a multi-level pore structure of macropores-mesopores-micropores.
[0018] Preferably, the macroporous template is monodisperse polystyrene microspheres, polymethyl methacrylate microspheres or silica microspheres with a particle size of 100 to 1500 nm, wherein the monodisperse microspheres are silica microspheres.
[0019] Preferably, the surfactant A is a combination of one or more of P123, F127, F123, SDS and PE, and the surfactant B is fatty alcohol polyoxyethylene ether, wherein the molar ratio of butyl titanate, ethanol, acetic acid, hydrochloric acid, water, surfactant A and surfactant B is (2-4): (24-40): (1-2.5): (17-31): (5-12): (2.94-4.16): (1.96-4.08).
[0020] Preferably, the heating conditions in S2 include a temperature of 25-80°C and a time of 35-80 hours; the sintering conditions in S3 include a temperature of 700-950°C and a time of 10-15 hours; and the roasting conditions include a temperature of 350°C for 1-3.5 hours and a temperature of 650°C for 3-9 hours.
[0021] Therefore, the present invention adopts the above-mentioned multi-level porous catalyst for plasma ammonia synthesis and its preparation method, and develops a multi-level porous ammonia synthesis catalyst with macropores, mesopores and micropores based on the research goal of improving the conversion rate of synthetic ammonia and reducing energy consumption by combining the advantages and disadvantages of synthetic ammonia catalysts with macropores, mesopores and micropores, so that the catalyst can efficiently catalyze the synthesis of ammonia in a plasma environment under room temperature conditions, and has broad application prospects.
[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a test result diagram of ammonia synthesis reaction of a multi-level porous catalyst for plasma ammonia synthesis and an embodiment of the preparation method thereof according to the present invention. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.
[0025] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.
[0026] Example
[0027] The present invention provides a multi-level porous catalyst for plasma synthesis of ammonia. The general formula of the multi-level porous catalyst is: xM*yA*(100-xy)C,
[0028] Wherein, M is the active component, A is the active auxiliary agent, C is the carrier, x and y represent the mass percentages of M and A respectively, and 0.1≤x≤60, 0.1≤y≤60.
[0029] The preferred mass percentage of the active component to the active auxiliary is: 20≤x≤40, 0.1≤y≤5.
[0030] The active component M includes one or more metals and / or metal oxides selected from the group consisting of Rh, Ru, Pt, Pd, Au, Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mo and Ce; the active auxiliary agent A includes one or more metals and / or metal oxides selected from the group consisting of Na, Mg, K, Ba and La; the carrier C includes one or more selected from the group consisting of Al2O3, TiO2, CaO, ZrO2 and BaTiO3; the micropore size of the oxide carrier in the carrier is distributed in the range of 0.5 to 2 nm, the mesopore size is distributed in the range of 4.5 to 50 nm, the macropore size is distributed in the range of 50 to 1500 nm, and the specific surface area of the oxide carrier is 100 to 500 m 2 g -1 .
[0031] The active component M can improve the plasma discharge activity, and at the same time enhance the catalyst's ability to adsorb N2 and desorb NH3, thereby promoting the synthesis of NH3. The active additive A can enhance the dispersion of the active component on the carrier, thereby optimizing the overall performance of the catalyst and achieving the goal of high conversion rate of synthetic NH3 under mild conditions. The carrier C can provide a stable carrier material with a multi-level pore structure for the plasma catalytic synthesis of NH3.
[0032] The present invention provides a method for preparing a multi-level porous catalyst for plasma synthesis of ammonia, comprising the following steps:
[0033] Step 1: by combining a hard template and a soft template, an oxide support having a macroporous-mesoporous-microporous multi-level pore structure is prepared using a colloidal crystal template method;
[0034] Step 2: Load the active component M and the active auxiliary agent A on the oxide carrier by impregnation method, and the impregnated oxide is dried and calcined to obtain a catalyst.
[0035] The specific operation of the impregnation method is: impregnate the oxide support with the active metal precursor solution, and then obtain the catalyst by drying and calcining. The drying conditions are: rotary evaporation at 60-85°C, and then drying in an oven at 85-100°C for 7-13h. The calcination conditions are: calcining at 400-600°C for 4-6h to obtain the catalyst.
[0036] The method for preparing the oxide carrier comprises the following steps:
[0037] S1. Using monodisperse microspheres as macroporous templates, the monodisperse microspheres are arranged into ordered colloidal crystal templates by self-assembly or sintering; the macroporous templates are monodisperse polystyrene microspheres, polymethyl methacrylate microspheres or silica microspheres, with a particle size of 100 to 1500 nm, wherein the monodisperse microspheres are silica microspheres.
[0038] S2, mixing surfactant A, surfactant B, butyl titanate, hydrochloric acid, acetic acid and ethanol, and heating and stirring to obtain a uniform and transparent precursor sol;
[0039] Surfactant A is a combination of one or more of P123, F127, F123, SDS and PE, and surfactant B is fatty alcohol polyoxyethylene ether, wherein the molar ratio of butyl titanate, ethanol, acetic acid, hydrochloric acid, water, surfactant A and surfactant B is (2-4):(24-40):(1-2.5):(17-31):(5-12):(2.94-4.16):(1.96-4.08).
[0040] S3. Add the precursor sol in S2 dropwise to the colloidal crystal template prepared in S1, and remove the microsphere colloidal crystal template by drying, calcining or solution dissolution to obtain an oxide carrier with a multi-level pore structure of macropores-mesopores-micropores.
[0041] The heating conditions include a temperature of 25 to 80° C. and a time of 35 to 80 hours; the sintering conditions include a temperature of 700 to 950° C. and a time of 10 to 15 hours; and the roasting conditions include a temperature of 350° C. for 1 to 3.5 hours and a temperature of 650° C. for 3 to 9 hours.
[0042] Example 1
[0043] A method for preparing a multi-level porous catalyst for plasma catalytic synthesis of ammonia, comprising the following steps:
[0044] SiO2 monodisperse microspheres are sintered to obtain a colloidal crystal template, and then oxide, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B and deionized water are mixed in proportion to prepare an oxide sol, and then the sol is evenly dropped into the prepared colloidal crystal template. After filtration and drying, the SiO2 colloidal crystal template is dissolved and removed using a NaOH solution to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores. Finally, the active component salt M and the active auxiliary agent salt A are loaded on the oxide carrier by an impregnation method, and then dried and reduced to the target catalyst.
[0045] In this embodiment, the diameter of SiO2 monodisperse microspheres is 500nm, surfactants A and B are F127 and fatty alcohol polyoxyethylene ether, respectively, and the concentration of NaOH solution is 2mol·L -1The active component salt M and the active auxiliary salt A are both nitrates, namely, cobalt nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively. 8g of SiO2 monodisperse microspheres with a diameter of 500nm, 76.6g of butyl titanate, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B, and deionized water are mixed in a molar ratio of 2:24:1:17:2.94:1.96:5 to prepare a transparent oxide sol. At a flow rate of 100mL·min -1 In air, at 2℃·min -1 The temperature was raised to 850℃ at a speed of 100 °C and kept constant for 10 h to enhance the mechanical properties of the SiO2 template and obtain a SiO2 colloidal crystal template.
[0046] The oxide sol was slowly and evenly dripped onto the SiO2 colloidal crystal template and allowed to stand for 48 h to complete the impregnation. The mixture was then placed in a drying oven and dried at 70 °C for 20 h. The dried sample was then dried at a flow rate of 100 mL min -1 In air, at 2℃·min -1 The temperature was raised to 650℃ at a rate of 4 h to remove the surfactant and nitrate. After the sample cooled to room temperature, it was placed in a 2 mol·L -1 The obtained product was dissolved in a NaOH solution at 75 °C for 5 h to remove the SiO2 colloidal template, washed until the pH value of the washing water was 7, and then placed in a vacuum drying oven and dried at 70 °C for 6 h to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores.
[0047] Example 2
[0048] A method for preparing a multi-level porous catalyst for plasma catalytic synthesis of ammonia, comprising the following steps:
[0049] SiO2 monodisperse microspheres are sintered to obtain a gel crystal template, and then oxide, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B and deionized water are mixed in proportion to prepare an oxide sol. The gel is then evenly dropped into the prepared gel crystal template, filtered and dried, and then the SiO2 gel crystal template is dissolved and removed using a NaOH solution to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores. Finally, the active component salt M and the active auxiliary agent salt A are loaded on the oxide carrier by an impregnation method, and then dried and reduced to the target catalyst.
[0050] In this embodiment, the diameter of SiO2 monodisperse microspheres is 1000nm, surfactants A and B are F127 and fatty alcohol polyoxyethylene ether, respectively, and the concentration of NaOH solution is 2mol·L -1The active component salt M and the active auxiliary salt A are both nitrates, namely, cobalt nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively. 8g of SiO2 monodisperse microspheres with a diameter of 1000nm, 76.6g of butyl titanate, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B, and deionized water are mixed in a molar ratio of 2:24:1:17:2.94:1.96:5 to prepare a transparent oxide sol. At a flow rate of 100mL·min -1 In air, at 2℃·min -1 The temperature was raised to 850℃ at a speed of 100 °C and kept constant for 10 h to enhance the mechanical properties of the SiO2 template and obtain a SiO2 colloidal crystal template.
[0051] The oxide sol was slowly and evenly dripped onto the SiO2 colloidal crystal template and allowed to stand for 48 h to complete the impregnation. The mixture was then placed in a drying oven and dried at 70 °C for 20 h. The dried sample was then dried at a flow rate of 100 mL min -1 In air, at 2℃·min -1 The temperature was raised to 650℃ at a rate of 4 h to remove the surfactant and nitrate. After the sample cooled to room temperature, it was placed in a 2 mol·L -1 The obtained product was dissolved in a NaOH solution at 75 °C for 5 h to remove the SiO2 colloidal template, washed until the pH value of the washing water was 7, and then placed in a vacuum drying oven and dried at 70 °C for 6 h to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores.
[0052] Example 3
[0053] A method for preparing a multi-level porous catalyst for plasma catalytic synthesis of ammonia, comprising the following steps:
[0054] SiO2 monodisperse microspheres are sintered to obtain a colloidal crystal template, and then oxide, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B and deionized water are mixed in proportion to prepare an oxide sol, and then the sol is evenly dropped into the prepared colloidal crystal template. After filtration and drying, the SiO2 colloidal crystal template is dissolved and removed using a NaOH solution to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores. Finally, the active component salt M and the active auxiliary agent salt A are loaded on the oxide carrier by an impregnation method, and then dried and reduced to the target catalyst.
[0055] In this embodiment, the diameter of SiO2 monodisperse microspheres is 1500nm, surfactants A and B are F127 and fatty alcohol polyoxyethylene ether, respectively, and the concentration of NaOH solution is 2mol·L -1The active component salt M and the active auxiliary salt A are both nitrates, namely, cobalt nitrate hexahydrate and lanthanum nitrate hexahydrate, respectively. 8g of SiO2 monodisperse microspheres with a diameter of 1500nm, 76.6g of butyl titanate, ethanol, acetic acid, hydrochloric acid, surfactant A, surfactant B, and deionized water are mixed in a molar ratio of 2:24:1:17:2.94:1.96:5 to prepare a transparent oxide sol. At a flow rate of 100mL·min -1 In air, at 2℃·min -1 The temperature was raised to 850℃ at a speed of 100 °C and kept constant for 10 h to enhance the mechanical properties of the SiO2 template and obtain a SiO2 colloidal crystal template.
[0056] The oxide sol was slowly and evenly dripped onto the SiO2 colloidal crystal template and allowed to stand for 48 h to complete the impregnation. The mixture was then placed in a drying oven and dried at 70 °C for 20 h. The dried sample was then dried at a flow rate of 100 mL min -1 In air, at 2℃·min -1 The temperature was raised to 650℃ at a rate of 4 h to remove the surfactant and nitrate. After the sample cooled to room temperature, it was placed in a 2 mol·L -1 The obtained product was dissolved in a NaOH solution at 75 °C for 5 h to remove the SiO2 colloidal template, washed until the pH value of the washing water was 7, and then placed in a vacuum drying oven and dried at 70 °C for 6 h to obtain an oxide carrier with a multi-level pore structure of macropores, mesopores and micropores.
[0057] In order to load 10 wt% of the active component Co and 0.5 wt% of the active auxiliary La, 8.89 g of cobalt nitrate hexahydrate and 0.24 g of lanthanum nitrate hexahydrate were dissolved in 30 mL of deionized water to obtain an impregnation solution, and the impregnation solution was loaded on 17.98 g of the multi-level porous structure oxide support prepared in Examples 1, 2 and 3 at a temperature of 80° C. using an equal volume impregnation method;
[0058] The obtained sample was placed in a vacuum drying oven and dried at 110 °C for 14 h. It was then calcined in a tube furnace at 2 °C min -1 The temperature was raised to 550°C at a rate of 10000 nm and kept constant for 4 hours to obtain the target catalyst with a macroporous-mesoporous-microporous multi-level pore structure: 10wt% Co / 0.5wt% La / oxide. In order to clearly describe the measurement and test results, the three prepared catalysts are respectively recorded as: Example 1-500nm, Example 2-1000nm and Example 3-1500nm.
[0059] Characterization results
[0060] The results of the samples obtained by N2 adsorption, SEM and mercury intrusion porosimetry are as follows:
[0061] Table 1 Characterization results
[0062]
[0063] Test Results
[0064] In order to test the effect of the prepared multi-level porous structure catalyst, the synthetic ammonia reaction was tested in a plasma environment, with the main reference being the concentration of ammonia produced. The prepared catalyst was filled into a quartz tube with an outer diameter of 12 mm, an inner diameter of 10 mm, and a length of 400 mm. It was fixed with quartz wool, and a tungsten needle was used as the inner electrode to connect to the high voltage pole of the power supply. The copper mesh was used as the outer electrode to connect to the low voltage pole of the power supply. In this experiment, the discharge power was 15-35 W, the frequency was 9.5 kHz, and the gas flow rate was controlled by a mass flow meter at 50 mL min -1 High-purity hydrogen was introduced at a flow rate of 20 mL min -1 High-purity nitrogen was introduced at a flow rate of 1.5 % and the product was detected by GC at the outlet of the reactor. Under normal temperature and pressure conditions, the reaction results of Examples 1 to 3 were as follows: Figure 1 As shown. Figure 1 It can be seen that the large pore diameter similar to the Debye length can improve the plasma discharge performance. The existence of multi-level pores ensures that the presence of large pores does not reduce the catalytic performance of the catalyst, and a high synthetic NH3 conversion rate can be achieved under mild conditions.
[0065] Therefore, the present invention adopts the above-mentioned multi-level porous catalyst for plasma ammonia synthesis and its preparation method, and develops a multi-level porous ammonia synthesis catalyst with macropores, mesopores and micropores based on the research goal of improving the conversion rate of synthetic ammonia and reducing energy consumption by combining the advantages and disadvantages of synthetic ammonia catalysts with macropores, mesopores and micropores, so that the catalyst can efficiently catalyze the synthesis of ammonia in a plasma environment under room temperature conditions, and has broad application prospects.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A multi-level porous catalyst for plasma synthesis of ammonia, characterized in that: The general formula of the multi-level porous catalyst is: xM*yA*(100-xy)C, Wherein, M is the active component, A is the active auxiliary agent, C is the carrier, x and y represent the mass percentages of M and A respectively, and 0.1≤x≤60, 0.1≤y≤60.
2. The multi-level porous catalyst for plasma synthesis of ammonia according to claim 1, characterized in that: The mass percentage of the active component and the active auxiliary agent is: 20≤x≤40, 0.1≤y≤5.
3. The multi-level porous catalyst for plasma synthesis of ammonia according to claim 1, characterized in that: The active component M includes one or more metals and / or metal oxides selected from the group consisting of Rh, Ru, Pt, Pd, Au, Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mo and Ce, and the active auxiliary agent A includes one or more metals and / or metal oxides selected from the group consisting of Na, Mg, K, Ba and La.
4. The multi-level porous catalyst for plasma ammonia synthesis according to claim 1, characterized in that: The carrier C comprises one or more of Al2O3, TiO2, CaO, ZrO2 and BaTiO3, the micropore size of the oxide carrier in the carrier is distributed in the range of 0.5 to 2 nm, the mesopore size is distributed in the range of 4.5 to 50 nm, the macropore size is distributed in the range of 50 to 1500 nm, and the specific surface area of the oxide carrier is 100 to 500 m 2 g -1 .
5. A method for preparing a multi-level porous catalyst for plasma synthesis of ammonia according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: by combining a hard template and a soft template, an oxide support having a macroporous-mesoporous-microporous multi-level pore structure is prepared using a colloidal crystal template method; Step 2: Load the active component M and the active auxiliary agent A on the oxide carrier by an impregnation method, and the impregnated oxide is dried and calcined to obtain a catalyst.
6. The method for preparing a multi-level porous catalyst for plasma ammonia synthesis according to claim 5, characterized in that: The specific operation of the impregnation method is: impregnating the oxide support with an active metal precursor solution, and then obtaining a catalyst by drying and calcining, wherein the drying conditions are: rotary evaporation at 60-85°C, and then drying in an oven at 85-100°C for 7-13h, and the calcination conditions are: calcining at 400-600°C for 4-6h to obtain the catalyst.
7. The method for preparing a multi-level porous catalyst for plasma ammonia synthesis according to claim 5, characterized in that: The preparation method of the oxide carrier comprises the following steps: S1, using monodisperse microspheres as macroporous templates, and arranging the monodisperse microspheres into an ordered colloidal crystal template by self-assembly or sintering; S2, mixing surfactant A, surfactant B, butyl titanate, hydrochloric acid, acetic acid and ethanol, and heating and stirring to obtain a uniform and transparent precursor sol; S3, adding the precursor sol in S2 dropwise to the colloidal crystal template prepared in S1, and removing the microsphere colloidal crystal template by drying, calcining or solution dissolution to obtain the oxide carrier having a multi-level pore structure of macropores-mesopores-micropores.
8. The method for preparing a multi-level porous catalyst for plasma ammonia synthesis according to claim 7, characterized in that: The macroporous template is monodisperse polystyrene microspheres, polymethyl methacrylate microspheres or silicon dioxide microspheres, with a particle size of 100-1500nm, wherein the monodisperse microspheres are silicon dioxide microspheres.
9. The method for preparing a multi-level porous catalyst for plasma ammonia synthesis according to claim 7, characterized in that: The surfactant A is a combination of one or more of P123, F127, F123, SDS and PE, and the surfactant B is fatty alcohol polyoxyethylene ether, wherein the molar ratio of butyl titanate, ethanol, acetic acid, hydrochloric acid, water, surfactant A and surfactant B is (2-4): (24-40): (1-2.5): (17-31): (5-12): (2.94-4.16): (1.96-4.08).
10. The method for preparing a multi-level porous catalyst for plasma ammonia synthesis according to claim 7, characterized in that: The heating conditions in S2 include a temperature of 25 to 80° C. and a time of 35 to 80 hours; the sintering conditions in S3 include a temperature of 700 to 950° C. and a time of 10 to 15 hours; and the roasting conditions include a temperature of 350° C. for 1 to 3.5 hours and a temperature of 650° C. for 3 to 9 hours.
Citation Information
Patent Citations
Catalyst applied to the reaction of synthesizing ammonia gas by plasma technology and preparation method thereof
CN110496646A
Catalyst for non-thermal plasma ammonia preparation and preparation method and application thereof
CN116351418A
Catalyst for synthesizing ammonia through plasma as well as preparation method and application of catalyst
CN117619391A
Catalyst applied to non-thermal plasma to directly synthesize ammonia from nitrogen and water
CN117680123A
Preparation method for synthesizing ammonia by using plasma
CN117923515A
Cited By
Synthetic ammonia catalyst with good stability and preparation method thereof
CN121016825A
Synthetic ammonia catalyst with good stability and preparation method thereof
CN121016825B