Tungsten and sulfation co-modified iron-based sulfur-resistant denitration catalyst and construction method thereof

By replacing tungsten atoms on the surface of α-ferric oxide catalyst and introducing sulfate ions, combined with density functional theory to optimize the catalyst structure, the problems of reduced activity and poor sulfur resistance of existing catalysts at high temperatures have been solved, achieving high efficiency and environmental protection. denitrification effect.

CN118788366APending Publication Date: 2024-10-18SHANGHAI INST OF TECH

Patent Information

Application Number
CN202410775664.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing vanadium pentoxide-tungsten trioxide/titanium dioxide catalyst has problems such as narrow temperature window, poor sulfur resistance, and reduced activity at high temperatures. Traditional denitrification catalyst research relies on experiments and rules of thumb, which is costly and has limited understanding of the catalytic reaction mechanism.

Method used

By replacing iron atoms with tungsten atoms on the surface of α-ferric oxide (001), and placing sulfate ions on the surface, density functional theory is used to perform DFT calculations to optimize the catalyst structure and performance, and improve the sulfur tolerance and denitrification activity of the catalyst. .

Benefits of technology

It significantly improves the medium-high temperature activity and sulfur resistance of the catalyst, reduces experimental costs and time, and provides a more environmentally friendly and efficient catalyst preparation method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788366A_ABST
    Figure CN118788366A_ABST
Patent Text Reader

Abstract

The invention relates to a tungsten and sulfation co-modified iron-based sulfur-resistant denitration catalyst and a construction method thereof. The method comprises the following steps: carrying out supercellular treatment on an initial alpha-ferric oxide crystal structure model; the method comprises the following steps: carrying out spin polarization DFT (Discrete Fourier Transform) calculation on a titanium-doped alpha-ferric oxide crystal structure by using a Pedew-Burke-Ernzerhof function and a projector augmented wave method, and further optimizing the titanium-doped alpha-ferric oxide crystal structure; performing section supercell on the optimized titanium-doped alpha-ferric oxide crystal structure, and further optimizing; selecting a tungsten atom to replace an iron atom of the surface structure of the titanium-doped alpha-ferric oxide (001), and vertically placing sulfate ions above the surface of the titanium-doped and tungsten-doped alpha-ferric oxide (001); the tungsten and sulfation co-modified iron-based sulfur-tolerant denitration catalyst is subjected to optimization and DFT + U calculation. Compared with the prior art, the sulfur-tolerant denitration performance of the catalyst is improved, and the experiment time is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical fields of material science, catalytic science and computational chemistry, and relates to a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst and a construction method thereof. Background Art

[0002] Since the 20th century, with the rapid development of industry, the use of fossil fuels has increased, and nitrogen oxides (NO x ) is one of the main pollutants in the air. Vanadium pentoxide-tungsten trioxide / titanium dioxide (V2O5-WO3 / TiO2, VW / T) catalysts have been widely studied as industrial selective catalytic reduction (SCR) denitrification catalysts in the temperature range of 300-400℃. Higher active temperatures will lead to excessive production of nitrous oxide (N2O), making sulfur dioxide (SO2) more easily oxidized to sulfur trioxide (SO3). In addition, the toxicity of vanadium (V) will also increase the post-treatment cost of deactivated catalysts. Therefore, there is an urgent need to develop low-temperature and high-efficiency denitrification catalysts.

[0003] At the same time, vanadium pentoxide-tungsten trioxide (molybdenum trioxide) / titanium dioxide (V2O5-WO3(MoO3) / TiO2) catalyst is currently the most widely used catalyst in industry, but it still has problems such as narrow temperature window, poor sulfur resistance, and poor high temperature selectivity. In addition, the carrier titanium dioxide (TiO2) has poor thermal stability, is prone to sintering at high temperatures, and transforms from anatase phase to inactive rutile phase, and V and tungsten (W) species are prone to segregation. These problems hinder its promotion in the field of denitrification. Therefore, vanadium pentoxide (V2O5) or TiO2 carriers are usually optimized by modification and doping.

[0004] In recent years, iron-based catalysts have been favored by many researchers because of their wide sources, no pollution, low cost, and high structural selectivity. Iron-based catalysts are catalysts with good denitrification performance, which have attracted more and more researchers in recent years. γ-Fe2O3 shows good denitrification effect in the temperature range of 200-290℃, and the efficiency can reach up to 90% at 250℃. However, when the temperature is higher than 300℃, γ-Fe2O3 will be transformed into α-Fe2O3, which will lead to a decrease in efficiency.

[0005] The research on traditional denitrification catalysts (such as ammonia SCR catalysts) mainly relies on experiments and empirical rules. However, this method has certain limitations, such as high cost, time consumption, complexity of material screening, and limited understanding of the catalytic reaction mechanism.

[0006] Patent CN117095769A discloses a doped iron-based catalyst based on density functional theory and a research method thereof, comprising the following steps: supercelling on the basis of an existing model; optimizing the γ-Fe2O3 crystal structure using the PBE function and the projector augmented wave method; further optimizing to obtain a model of the γ-Fe2O3 (001) surface; replacing an iron (Fe) atom of the γ-Fe2O3 (001) surface structure with the rare earth element praseodymium (Pr) and further optimizing; introducing ammonia (NH3) molecule adsorption into the obtained model, and calculating the gas adsorption energy E ads ; Post-processing and analysis of the data were performed to obtain a PDOS diagram. However, the description of the metal substitution method in this patent is not detailed enough. The patent only mentions the use of the rare earth element Pr to replace an Fe atom in the surface structure of γ-Fe2O3 (001), but does not explain the reason for selecting Pr, the basis for selecting the substitution position, the stability of the structure after substitution, etc.; and the patent mentions post-processing and analysis of the data to obtain a partial wave density of states (PDOS) diagram, but does not explain the specific meaning and analysis results of the PDOS diagram; at the same time, after doping with the rare earth element Pr, the low-temperature activity of the catalyst is not significantly improved, and the acidity is not increased, and the adsorption performance of nitric oxide (NO) and NH3 is not significantly improved. Summary of the invention

[0007] The purpose of the present invention is to overcome at least one defect of the above-mentioned prior art, such as the imperfect research method of the metal-doped iron-based catalyst, and to provide a tungsten and sulfate co-modified iron-based sulfur-resistant denitrification catalyst and a construction method thereof. The present invention improves the sulfur-resistant denitrification performance of the iron-based catalyst and saves experimental time.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] One of the technical solutions of the present invention is to provide a tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst, in which an iron (Fe) atom on the surface of titanium (Ti)-doped α-iron trioxide (α-Fe2O3) (001) is replaced by a tungsten (W) atom, and a sulfate (SO4) is placed above the surface of the titanium and tungsten-doped α-iron trioxide (001). 2- )ion.

[0010] Previous experiments have found that doping with metal elements can change the physical and chemical properties of the catalyst surface and improve the denitrification activity of the catalyst. Studies have reported that tungsten (W) is a doping aid for selective catalytic reduction (SCR) catalysts that improves the dispersibility of active components, increases acidity, helps adsorb ammonia (NH3), regulates the redox ability of active components, increases the active oxygen content, and improves the adsorption and oxidation of nitric oxide (NO). The special properties of the W element give it unique advantages in these aspects, so it has a significant effect in improving NH3 adsorption performance.

[0011] At the same time, experimental studies have shown that metal sulfates have higher catalytic activity and good resistance to sulfur dioxide (SO2) and water vapor (H2O) at high temperatures (300-350°C). The metal oxide catalysts modified by sulfation have more Acidic sites can effectively increase the adsorption of NH3 and significantly improve the activity of the catalyst at medium and high temperatures.

[0012] W doping and sulfation co-modification have a significant impact on the performance of Fe2O3 catalysts, but accurately mastering these parameters remains a challenge. In addition, the adsorption properties of the doped catalyst surface to the reaction gas molecules remain to be studied.

[0013] With the rapid development of computer technology, density functional theory (DFT) has provided new possibilities for the study and design of catalysts.

[0014] One of the technical solutions of the present invention is to provide a method for constructing the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst, which comprises the following steps:

[0015] S1, obtaining an initial α-iron sesquioxide crystal structure model, supercelling the initial α-iron sesquioxide crystal structure model, and selecting a titanium atom to replace an iron atom on the surface of the α-iron sesquioxide to obtain a titanium-doped α-iron sesquioxide crystal structure;

[0016] S2. The spin-polarized DFT (density functional theory) calculation of the titanium-doped α-iron sesquioxide crystal structure is performed by using the Perdew-Burke-Ernzerhof (PBE) function and the projector augmented wave (PAW) method, and further optimized to obtain the optimized titanium-doped α-iron sesquioxide crystal structure;

[0017] S3. Since the 001 surface of α-iron sesquioxide has the strongest reactivity, the 001 surface is selected as the reaction surface, and the optimized titanium-doped α-iron sesquioxide crystal structure is cut into supercells, and further optimized to obtain the titanium-doped α-iron sesquioxide (001) surface structure;

[0018] S4. Since the surface of α-iron sesquioxide (001) has four octahedral iron cations as the main active sites participating in the selective catalytic reduction (SCR) process, a tungsten atom is selected to replace an iron atom on the surface structure of titanium-doped α-iron sesquioxide (001), and sulfate ions are placed vertically above the surface of titanium- and tungsten-doped α-iron sesquioxide (001), thereby obtaining a tungsten and sulfate-modified iron-based sulfur-resistant denitrification catalyst;

[0019] S5. Optimizing and performing DFT+U calculation on the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst to obtain an optimized tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst;

[0020] S6. Introducing ammonia (NH3) molecules, nitric oxide (NO) molecules and sulfur dioxide (SO2) molecules into the optimized tungsten and sulfated co-modified iron-based sulfur-resistant denitration catalyst for adsorption, respectively, to obtain a tungsten and sulfated co-modified iron-based sulfur-resistant denitration catalyst after gas adsorption;

[0021] S7. Post-processing and analysis of the data of the simulated adsorption test of the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst after gas adsorption. The gas adsorption energy E of the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst was calculated based on various energy parameters obtained from the simulated adsorption test. ads , determine the better catalyst;

[0022] S8. Post-process and analyze the data of partial wave density of states (PDOS) calculation of tungsten after gas adsorption and sulfation co-modified iron-based sulfur-resistant denitrification catalyst to obtain a partial wave density of states diagram and determine the better catalyst.

[0023] As a preferred technical solution, in step S1, the initial α-ferric oxide crystal structure model is downloaded from the database of the Materials project official website, and the initial α-ferric oxide crystal structure model is supercelled using Materials Studio software. At the same time, a titanium atom is selected from the metal library of the Materials Studio software to replace an iron atom on the surface of the α-ferric oxide.

[0024] As a preferred technical solution, the CIF file code of the initial α-iron sesquioxide crystal structure model in step S1 is 890596, the space group number is R-3c (167), and the lattice constant of α-iron sesquioxide is and That is, the actual calculated model is 5.037×5.037×13.771, titanium is a close-packed hexagonal crystal (HCP), the space group of titanium is P6 / mmm, and a POSCAR file is generated to record the lattice information of the titanium-doped α-ferric oxide crystal structure.

[0025] As a preferred technical solution, in step S2, VASP software is used to perform spin-polarized DFT calculations on the titanium-doped α-Fe2O3 crystal structure using the Perdew-Burke-Ernzerhof function and the projector augmented wave method, and VASP software is used for further optimization until the calculation results meet the convergence conditions.

[0026] As a preferred technical solution, in step S2, according to the POSCAR file, the VASPKIT post-processing tool 101 function is used to generate an INCAR file, 102 function is used to generate a KPOINTS file, and 103 function is used to generate a POTCAR file to record the lattice information of the titanium-doped α-iron sesquioxide crystal structure during spin-polarized DFT calculations.

[0027] Furthermore, during optimization in step S2, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1.

[0028] As a preferred technical solution, in step S2, the optimized data is observed, and the changes in the total energy and force of each ion action are less than 10 -6 -10 -4 eV and 10 -4 -10 -2 eV·A -1 , indicating that the calculation is reliable and the optimized titanium-doped α-Fe2O3 crystal structure is obtained.

[0029] As a preferred technical solution, in step S3, the optimized titanium-doped α-ferric oxide crystal structure is sectioned and supercelled using Materials Studio software, and further optimized using the Constraints function of the Modify option of Materials Studio software.

[0030] Furthermore, in step S3, a 2×2 or 3×3 plate model is set when the slice supercell is formed. Vacuum layer, select four to six layers of atoms, of which the bottom two layers are fixed to relax other atoms;

[0031] Since the model after sectioning supercell is too large to be conducive to calculation, Monkhorst-pack 1×1×1, 2×2×1 or 3×3×1 points were set during optimization to obtain the titanium-doped α-Fe2O3 (001) surface structure.

[0032] As a preferred technical solution, in step S4, a tungsten atom is selected from the metal library of the Materials Studio software to replace an iron atom on the surface structure of the titanium-doped α-iron sesquioxide (001), and at the same time, the sulfate ions are placed vertically above the titanium- and tungsten-doped α-iron sesquioxide (001) surface using the Materials Studio software.

[0033] As a preferred technical solution, in step S4, tungsten is body-centered cubic (BCC) and the space group of tungsten is

[0036] Furthermore, in step S4, the ions are optimized before being placed, and the optimization includes the following steps:

[0037] S4.1. Obtaining an initial sulfate ion model;

[0038] S4.2. Optimize the initial sulfate ion model.

[0039] As a preferred technical solution, in step S4.1, the initial sulfate ion model is downloaded from the database of the Materials project official website.

[0040] As a preferred technical solution, in step S4.2, the initial sulfate ion model is optimized using VASP software until the calculation results reach a convergence condition.

[0041] Furthermore, during optimization in step S4.2, the cutoff energy is set to 400-540 eV, the K point is set to 1×1×1, 2×2×1 or 3×3×1, and the ion step NSW is set to 200-300, and the U value of the sulfur (S) atom and the oxygen (O) atom is not set.

[0042] As a preferred technical solution, after observing the optimized data in step S4.2, the changes in the total energy and force of each ion action are less than 10 -6 -10 -4 eV and 10 -4 -10 -2 eV·A -1 , indicating that the calculation is reliable and the optimized ionic structure is obtained.

[0043] Further, the distance between the optimized sulfate ion and the surface of the titanium- and tungsten-doped α-iron trioxide (001) in step S4 is

[0044] As a preferred technical solution, in step S5, VASP software is used to optimize and perform DFT+U calculation on the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst until the calculation results reach the convergence condition, indicating that the sulfate ions are successfully adsorbed on the surface.

[0045] Furthermore, during optimization in step S5, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1;

[0046] Since some metal-doped iron-based catalysts are strongly electron-correlated systems, the addition of Hubbard U should be considered in the DFT calculation. When calculating with DFT+U, the d-orbital U value of the iron atom is set to 3.5-5, the d-orbital U value of the tungsten atom is set to 3.5-5, and the d-orbital U value of the titanium atom is set to 2.5-4. No U value is set for the sulfur atom and the oxygen atom.

[0047] As a preferred technical solution, in step S5, the optimized data is observed, and the changes in the total energy and force of each ion action are less than 10 -6 -10 -4 eV and 10 -4 -10 -2 eV·A -1 , indicating that the calculation is reliable.

[0048] As a preferred technical solution, in step S6, Materials Studio software is used to introduce ammonia molecules, nitric oxide molecules and sulfur dioxide molecules into the optimized tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst for adsorption.

[0049] Furthermore, in step S6, before the molecular adsorption, the gas molecules are placed in the single cell for optimization, and the optimization includes the following steps:

[0050] S6.1. Obtaining initial structural models of ammonia molecules, nitric oxide molecules and sulfur dioxide molecules;

[0051] S6.2. Optimize the molecular structure.

[0052] As a preferred technical solution, in step S6.1, the initial ammonia molecule, nitric oxide molecule and sulfur dioxide molecule structure models are downloaded respectively from the database of the Materials project official website.

[0053] As a preferred technical solution, in step S6.2, VASP software is used to optimize the molecular structure until the calculation results reach the convergence condition.

[0054] Furthermore, the size of the single unit cell is

[0055] During optimization in step S6.2, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1.

[0056] As a preferred technical solution, after observing the optimized data in step S6.2, the changes in the total energy and force of each ion action are less than 10 -6 -10 -4 eV and 10 -4 -10 -2 eV·A -1 , indicating that the calculation is reliable and the optimized molecular structure is obtained.

[0057] As a preferred technical solution, in step S7, VASP software is used to perform post-processing analysis on the data of the simulated adsorption test of the tungsten and sulfation-modified iron-based sulfur-resistant denitrification catalyst after gas adsorption.

[0058] As a preferred technical solution, the gas adsorption energy E in step S7 ads The calculation formula is as follows:

[0059] E ads =E gas+surface -(E gas +E surface );

[0060] Among them, E gas+surface is the energy of the gas adsorption configuration and the relaxed surface, E gas is the energy of a single gas before adsorption, E surface is the energy after relaxing the surface.

[0061] As a preferred technical solution, in step S8, the VASPKIT post-processing tool is used to perform data post-processing analysis on the partial wave density of states calculation of the tungsten after gas adsorption and the sulfation co-modified iron-based sulfur-resistant denitrification catalyst.

[0062] As a preferred technical solution, when calculating the partial wave density of states in step S8, the INCAR file settings are added with parameters such as LORBIT and NEDOS, the number of K points is increased when the ISMEAR value is modified to -5, and the 115 function of the VASPKIT post-processing tool is used to analyze the partial wave density of states of ammonia gas molecules, nitric oxide gas molecules and sulfur dioxide gas molecules adsorbed on the surface of α-ferric oxide before and after doping.

[0063] One of the technical solutions of the present invention is to provide a construction device for a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst, comprising a memory, a processor, and a computer program stored in the memory, wherein the processor executes the computer program to implement the steps of the described method.

[0064] One of the technical solutions of the present invention is to provide a computer-readable storage medium on which a computer program is stored, and when the computer program is executed by a processor, the steps of the method described are implemented.

[0065] One of the technical solutions of the present invention is to provide a computer program product, including a computer program, which implements the steps of the method when executed by a processor.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] (1) The present invention solves the shortcomings of the traditional "trial and error" method of preparing catalysts, saves time and resources, determines the initial crystal structure based on density functional theory, and analyzes the performance through theoretical calculation;

[0068] (2) The present invention does not involve the implementation and experiment of chemical products in the whole process, does not produce chemical pollution, conforms to the concept of environmental protection and green, and has low cost, convenient operation, easy implementation, and is suitable for application and promotion;

[0069] (3) The present invention can predict the performance of the catalyst in advance through calculation results before the experiment, and at the same time explore the effects of tungsten doping and the introduction of sulfate ions on the adsorption of ammonia, nitric oxide, sulfur dioxide and other gases by the iron-titanium catalyst, promote the adsorption of ammonia and nitric oxide by the catalyst, enhance the denitration effect of the catalyst, inhibit the adsorption of sulfur dioxide by the catalyst, enhance the sulfur resistance of the catalyst, select suitable samples in advance, and save experimental time;

[0070] (4) The present invention reduces the calculation time and avoids wasting computer time by reasonably setting the calculation parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 This is a model diagram of the iron-based sulfur-resistant denitration catalyst co-modified by tungsten and sulfation in an embodiment of the present invention;

[0072] Figure 2 It is the adsorption configuration diagram of ammonia (NH3) molecules on the Fe-Ti surface in Comparative Example 1 of the present invention;

[0073] Figure 3 In the embodiment of the present invention, NH3 molecules are in W-Fe-Ti-SO4 2- Adsorption configuration diagram of the surface;

[0074] Figure 4 This is the adsorption configuration diagram of nitric oxide (NO) molecules on the Fe-Ti surface in Comparative Example 1 of the present invention;

[0075] Figure 5 In the embodiment of the present invention, NO molecules are in W-Fe-Ti-SO4 2-Adsorption configuration diagram of the surface;

[0076] Figure 6 It is the adsorption configuration diagram of sulfur dioxide (SO2) molecules on the Fe-Ti surface in Comparative Example 1 of the present invention;

[0077] Figure 7 In the embodiment of the present invention, SO2 molecules are in W-Fe-Ti-SO4 2- Adsorption configuration diagram of the surface;

[0078] Figure 8 It is a partial wave density of states (PDOS) diagram of NO molecules adsorbed on the Fe-Ti surface in the comparative example 1 of the present invention;

[0079] Fig. 9 It is a detailed enlarged view of the PDOS of the NO molecule adsorbed on the Fe-site configuration on the Fe-Ti surface in Comparative Example 1 of the present invention;

[0080] Fig.10 In the embodiment of the present invention, NO molecules are in W-Fe-Ti-SO4 2- PDOS diagram of the adsorption configuration at the Fe site;

[0081] Fig.11 In the embodiment of the present invention, NO molecules are in W-Fe-Ti-SO4 2- A detailed enlarged image of PDOS adsorbed on the Fe site;

[0082] Fig.12 The NH3 molecule in Fe-Ti-SO4 in Comparative Example 3 of the present invention 2- PDOS diagram of the surface adsorbed on the Fe site;

[0083] Fig.13 The NH3 molecule in Fe-Ti-SO4 in Comparative Example 3 of the present invention 2- A detailed enlarged image of PDOS adsorbed on the Fe site;

[0084] Fig.14 In the embodiment of the present invention, NH3 molecules are in W-Fe-Ti-SO4 2- PDOS diagram of the adsorption configuration at the Fe site;

[0085] Fig.15 In the embodiment of the present invention, NH3 molecules are in W-Fe-Ti-SO4 2- Detailed enlargement of PDOS adsorbed on the Fe site. DETAILED DESCRIPTION

[0086] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0087] Example:

[0088] A tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst, such as Figure 1 As shown, an iron (Fe) atom on the surface of titanium (Ti)-doped α-iron trioxide (α-Fe2O3) (001) is replaced by a tungsten (W) atom, and a sulfate (SO4) is placed above the surface of Ti- and W-doped α-Fe2O3 (001). 2- )ion.

[0089] The method for constructing the above-mentioned tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst has the following specific steps:

[0090] S1. Download the initial α-Fe2O3 crystal structure model from the database of the Materials project official website, use Materials Studio software to supercell the initial α-Fe2O3 crystal structure model, and select a Ti atom from the metal library of Materials Studio software to replace an Fe atom on the surface of α-Fe2O3 to obtain a Ti-doped α-Fe2O3 crystal structure;

[0091] The CIF file code of the initial α-Fe2O3 crystal structure model is 890596, the space group number is R-3c(167), and the lattice constant of α-Fe2O3 is and That is, the actual calculated model is 5.037×5.037×13.771, Ti is a close-packed hexagonal crystal (HCP), the space group of Ti is P6 / mmm, and the POSCAR file is generated to record the lattice information of the Ti-doped α-Fe2O3 crystal structure;

[0092] S2. Use VASP software to perform spin-polarized DFT (density functional theory) calculations on the Ti-doped α-Fe2O3 crystal structure using the Perdew-Burke-Ernzerhof (PBE) function and the projector augmented wave (PAW) method, and use VASP software to further optimize until the calculation results reach the convergence condition to obtain the optimized Ti-doped α-Fe2O3 crystal structure;

[0093] According to the POSCAR file, the VASPKIT post-processing tool 101 function is used to generate the INCAR file, 102 function is used to generate the KPOINTS file, and 103 function is used to generate the POTCAR file to record the lattice information of the Ti-doped α-Fe2O3 crystal structure during spin-polarized DFT calculations;

[0094] During optimization, the cutoff energy was set to 520 eV and the K point was 1 × 1 × 1;

[0095] After optimizing, the changes of total energy and force of each ion interaction are less than 10 -5 eV and 10 - 3 eV·A -1 , indicating that the calculation is reliable, and the optimized Ti-doped α-Fe2O3 crystal structure is obtained;

[0096] S3. Since the 001 surface of α-Fe2O3 has the strongest reactivity, the 001 surface is selected as the reaction surface, and the optimized Ti-doped α-Fe2O3 crystal structure is cut into supercells using Materials Studio software, and further optimized using the Constraints function of the Modify option of Materials Studio software to obtain the Ti-doped α-Fe2O3 (001) surface structure;

[0097] When cutting the supercell, set the 2×2 plate model and For the vacuum layer, five layers of atoms are selected, of which the bottom two layers are fixed to relax the other atoms;

[0098] Since the model after the section supercell is too large to be useful for calculation, the Monkhorst-pack 1×1×1 point was set during optimization to obtain the Ti-doped α-Fe2O3 (001) surface structure;

[0099] S4, since there are four octahedral Fe cations on the surface of α-Fe2O3(001) as the main active sites participating in the selective catalytic reduction (SCR) process, W atoms were selected from the metal library of Materials Studio software to replace one Fe atom on the surface structure of Ti-doped α-Fe2O3(001). At the same time, SO4 2- The ions were placed vertically above the Ti- and W-doped α-Fe2O3 (001) surface, resulting in a tungsten- and sulfate-co-modified iron-based sulfur-resistant denitrification catalyst;

[0100] W is a body-centered cubic (BCC) crystal, and the space group of W is

[0101] The ions are optimized before placement. The specific steps of optimization are as follows:

[0102] S4.1. Download the initial SO4 from the database on the Materials project website 2- Ionic model;

[0103] S4.2. Use VASP software to analyze the initial SO4 2- The ion model is optimized until the calculation results reach the convergence condition;

[0104] During optimization, the cutoff energy was set to 520 eV and the K point was 1 × 1 × 1, while the ion step NSW was set to 200, and the U value of sulfur (S) atoms and oxygen (O) atoms was not set;

[0105] S4.3. Observe the optimized data. The changes of total energy and force of each ion are less than 10 -5 eV and 10 -3 eV·A -1 , indicating that the calculation is reliable and the optimized ionic structure is obtained;

[0106] Optimized SO4 2- The distance between the ions and the Ti- and W-doped α-Fe2O3(001) surface is

[0107] S5. Use VASP software to optimize and perform DFT+U calculation on the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst until the calculation results reach the convergence condition, indicating that SO4 2- The ions were successfully adsorbed on the surface, and the optimized tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst was obtained. Figure 1 ;

[0108] During optimization, the cutoff energy was set to 520 eV and the K point was 1 × 1 × 1;

[0109] After optimizing, the changes of total energy and force of each ion interaction are less than 10 -5 eV and 10 - 3 eV·A -1 , indicating that the calculation is reliable;

[0110] Since some metal-doped iron-based catalysts are strongly electron-correlated systems, Hubbard U should be considered in DFT calculations. When calculating with DFT+U, the d-orbital U value of Fe atoms is set to 4.0, the d-orbital U value of W atoms is set to 4.0, and the d-orbital U value of Ti atoms is set to 3.0. The U values ​​of S atoms and O atoms are not set.

[0111] S6. Using Materials Studio software, ammonia (NH3), nitric oxide (NO) and sulfur dioxide (SO2) molecules were introduced into the optimized tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst for adsorption, respectively, to obtain the tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst after gas adsorption, see Figures 2 to 7 ;

[0112] Before molecular adsorption, the gas molecules are placed in a single unit cell for optimization. The size of the single unit cell is The specific steps of optimization are as follows:

[0113] S6.1. Download the initial NH3 molecule, NO molecule and SO2 molecule structure models from the database of Materials project official website;

[0114] S6.2. Use VASP software to optimize the molecular structure until the calculation results reach the convergence condition;

[0115] During optimization, the cutoff energy was set to 520 eV and the K point was 1 × 1 × 1;

[0116] S6.3. Observe the optimized data. The changes of total energy and force of each ion interaction are less than 10 -5 eV and 10 -3 eV·A -1 , indicating that the calculation is reliable and the optimized molecular structure is obtained;

[0117] S7. Use VASP software to perform post-processing analysis on the data of the simulated adsorption test of the tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst after gas adsorption. Calculate the gas adsorption energy E of the tungsten and sulfated co-modified iron-based sulfur-resistant denitrification catalyst through various energy parameters obtained from the simulated adsorption test. ads , to determine the optimal catalyst, gas adsorption energy E ads The calculation formula is as follows:

[0118] E ads =E gas+surface -(E gas +E surface );

[0119] Among them, E gas+surface is the energy of the gas adsorption configuration and the relaxed surface, E gas is the energy of a single gas before adsorption, E surface is the energy after relaxing the surface;

[0120] S8. Use VASPKIT post-processing tool to perform partial wave density of states (PDOS) calculation on the gas adsorbed tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst to obtain the PDOS diagram, see Figures 8 to 15 , determine the better catalyst;

[0121] When calculating PDOS, the INCAR file settings are added with parameters such as LORBIT and NEDOS. The number of K points is increased when the ISMEAR value is changed to -5. The 115 function of the VASPKIT post-processing tool is used to analyze the PDOS results of NH3 gas molecules, NO gas molecules and SO2 gas molecules adsorbed on the α-Fe2O3 surface before and after doping.

[0122] Comparative Example 1:

[0123] An iron-based catalyst and its preparation method and test are basically the same as the embodiment, except that only steps S1 to S3 are taken to obtain a Ti-doped α-Fe2O3 (001) surface structure.

[0124] Comparative Example 2:

[0125] A tungsten-modified iron-based catalyst and a preparation method and test thereof are basically the same as those in the embodiment, except that only steps S1 to S3 are taken, and in S4, a W atom is selected from the metal library of the Materials Studio software to replace an Fe atom in the Ti-doped α-Fe2O3 (001) surface structure to obtain a Ti- and W-doped α-Fe2O3 (001) surface structure.

[0126] Comparative Example 3:

[0127] A sulfated modified iron-based catalyst and its preparation method and test are basically the same as the embodiment, except that only steps S1 to S3 are taken, and in S4, SO4 is converted into 2- ions are placed vertically above the Ti-doped α-Fe2O3 (001) surface to obtain Ti-doped and SO4-introduced 2- α-Fe2O3(001) surface structure of ions.

[0128] like Figures 2 to 7 As shown in the figure, NO and NH3 are both polar molecules, and their adsorption on the metal surface is mainly achieved through electrostatic interaction and hydrogen bonding interaction. The presence of Ti and W can increase the adsorption energy of NO and NH3 on the catalyst surface, because they can act as mediators between NO and NH3 molecules and the metal surface, increasing the interaction between them. In addition, the electron cloud distribution of Ti and W is different from that of Fe, and their presence can change the electron density distribution on the metal surface, thereby affecting the interaction between NO and NH3 and the metal surface. At the same time, SO4 2- The presence of will reduce the adsorption energy of SO2 on the catalyst surface, because SO4 2-It can compete with SO2 for adsorption sites and reduce the interaction between SO2 and the metal surface. 2- The chemical properties of SO2 are similar to those of SO2, and they will interact with each other, thus affecting the adsorption energy of SO2 on the Fe surface.

[0129] Through DFT calculation, the adsorption of NH3 gas molecules, NO gas molecules and SO2 gas molecules on Fe-Ti surface, W-Fe-Ti surface, Fe-Ti-SO4 2- Surface and W-Fe-Ti-SO4 2- The adsorption conditions at various positions on the surface, this embodiment mainly studies the adsorption of various surface Fe sites. The adsorption energy of SO2, NO and NH3 adsorbed on different surface Fe sites of α-Fe2O3 is calculated, see Table 1.

[0130] Table 1 Adsorption energy of gas molecules adsorbed on different Fe positions on the surface of α-Fe2O3 in the examples and comparative examples

[0131] Example Surface <![CDATA[SO2-E ads (eV)]]> <![CDATA[NO-E ads (eV)]]> <![CDATA[NH3-E ads (eV)]]> Comparative Example 1 Fe-Ti (Fe position) -1.675 -3.084 -0.541 Comparative Example 2 W-Fe-Ti (Fe position) -1.261 -4.122 -1.693 Comparative Example 3 <![CDATA[Fe-Ti-SO4 2- (Fe position)]]> -1.283 -3.941 -1.522 Example <![CDATA[W-Fe-Ti-SO4 2- (Fe position)]]> -1.213 -4.682 -2.343

[0132] From the gas adsorption energy E ads It can be obtained, as shown in Table 1, in Fe-Ti, W-Fe-Ti, Fe-Ti-SO4 2- and W-Fe-Ti-SO4 2- The adsorption energies of SO2 on Fe sites on the four surfaces are -1.675eV, -1.261eV, -1.283eV and -1.213eV, respectively. 2- With the introduction of ions, the adsorption energy of SO2 on the surface of Fe-Ti catalyst is reduced and shows a downward trend, which is beneficial to reduce the sulfidation of Fe-Ti catalyst surface;

[0133] The adsorption energies of NO on Fe sites are −3.084 eV, −4.122 eV, −3.941 eV, and −4.682 eV, respectively, indicating that W doping and / or sulfation promote the adsorption of NO on Fe-Ti catalysts;

[0134] The adsorption energies of NH3 on Fe sites are −0.541 eV, −1.693 eV, −1.522 eV, and −2.343 eV, respectively, indicating that W doping and / or sulfation promote the adsorption of NH3 on Fe-Ti catalysts.

[0135] At the same time, it can be seen from the PDOS diagram that Figures 8 to 11 As shown, compared with the Fe-Ti surface in Comparative Example 1, the adsorption of NO on the SO4 2-After the surface is doped with W, the 2p orbital of N interacts with the 3d orbital of Fe, the 3d orbital of Ti, the 5d orbital of W and S(SO4 2- ) overlaps well at -6-0 eV, supporting the relationship between NO and W-Fe-Ti-SO4 2- Strong interactions between surfaces.

[0136] like Figures 12 to 15 As shown, the results show that compared with the Fe-Ti-SO4 in Comparative Example 3 2- Compared with the surface, NH3 and W-Fe-Ti-SO4 in the embodiment 2- Stronger orbital hybridization occurs between the surfaces, further proving that W modification enhances the Fe-Ti-SO4 2- The acidity supports NH3 and W-Fe-Ti-SO4 2- Strong interactions between surfaces.

[0137] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst, characterized in that: The catalyst replaces an iron atom on the surface of titanium-doped α-iron sesquioxide (001) with a tungsten atom, and places sulfate ions on the surface of titanium-doped and tungsten-doped α-iron sesquioxide (001).

2. A method for constructing the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst as claimed in claim 1, characterized in that: The method comprises the following steps: S1, obtaining an initial α-iron sesquioxide crystal structure model, supercelling the initial α-iron sesquioxide crystal structure model, and selecting a titanium atom to replace an iron atom on the surface of the α-iron sesquioxide to obtain a titanium-doped α-iron sesquioxide crystal structure; S2. The spin-polarized DFT calculation of the titanium-doped α-iron oxide crystal structure is performed by using the Perdew-Burke-Ernzerhof function and the projector augmented wave method, and further optimized to obtain the optimized titanium-doped α-iron oxide crystal structure; S3, cutting the optimized titanium-doped α-iron sesquioxide crystal structure into a supercell, and further optimizing it to obtain a titanium-doped α-iron sesquioxide (001) surface structure; S4, selecting a tungsten atom to replace an iron atom on the surface structure of titanium-doped α-iron trioxide (001), and at the same time vertically placing sulfate ions above the surface of titanium-doped and tungsten-doped α-iron trioxide (001), to obtain a tungsten and sulfate co-modified iron-based sulfur-resistant denitrification catalyst; S5. Optimizing and performing DFT+U calculation on the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst to obtain an optimized tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst; S6. Introducing ammonia molecules, nitric oxide molecules and sulfur dioxide molecules into the optimized tungsten and sulfated co-modified iron-based sulfur-resistant denitration catalyst for adsorption, respectively, to obtain a tungsten and sulfated co-modified iron-based sulfur-resistant denitration catalyst after gas adsorption; S7. Post-processing and analysis of the data of the simulated adsorption test of the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst after gas adsorption. The gas adsorption energy E of the tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst was calculated based on various energy parameters obtained from the simulated adsorption test. ads , determine the better catalyst; S8. Post-process and analyze the data of partial wave state density calculation of tungsten after gas adsorption and sulfation co-modified iron-based sulfur-resistant denitrification catalyst to obtain a partial wave state density map and determine the better catalyst.

3. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: During optimization in step S2, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1.

4. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: In step S3, when cutting the supercell, set a 2×2 or 3×3 plate model and set For the vacuum layer, four to six layers of atoms are selected, of which the bottom two layers are fixed; During optimization, the points of Monkhorst-pack 1×1×1, 2×2×1 or 3×3×1 were set to obtain the titanium-doped α-Fe2O3 (001) surface structure.

5. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: In step S4, the ions are optimized before being placed, and the optimization includes the following steps: S4.

1. Obtaining an initial sulfate ion model; S4.

2. Optimize the initial sulfate ion model.

6. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 5, characterized in that: During optimization in step S4.2, the cutoff energy is set to 400-540 eV, the K point is set to 1×1×1, 2×2×1 or 3×3×1, and the ion step NSW is set to 200-300. The U value of sulfur atoms and oxygen atoms is not set.

7. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: The distance between the optimized sulfate ion and the surface of α-iron trioxide (001) doped with titanium and tungsten in step S4 is 8. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: During optimization in step S5, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1; In DFT+U calculation, the d-orbital U value of iron atoms is set to 3.5-5, the d-orbital U value of tungsten atoms is set to 3.5-5, and the d-orbital U value of titanium atoms is set to 2.5-4. No U value is set for sulfur atoms and oxygen atoms.

9. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 2, characterized in that: In step S6, before the molecular adsorption, the gas molecules are placed in the single cell for optimization, and the optimization includes the following steps: S6.

1. Obtaining initial structural models of ammonia molecules, nitric oxide molecules and sulfur dioxide molecules; S6.

2. Optimize the molecular structure.

10. The method for constructing a tungsten and sulfation co-modified iron-based sulfur-resistant denitrification catalyst according to claim 9, characterized in that: The size of the unit cell is During optimization in step S6.2, the cutoff energy is set to 400-540 eV, and the K point is set to 1×1×1, 2×2×1, or 3×3×1.

Citation Information

Patent Citations

  • High-activity vanadium-free denitration catalyst, preparation method and application thereof

    CN113976094A

  • Sulfating modified iron-tungsten-titanium SCR (selective catalytic reduction) denitration catalyst as well as preparation method and application thereof

    CN114146713A

  • Doped iron-based catalyst based on density functional theory and research method thereof

    CN117095769A

Cited By

  • Doped iron-based catalyst based on density functional theory and research method thereof

    CN117095769A

  • A doped iron-based catalyst based on density functional theory and a method for researching the same

    CN117095769B