Palladium-copper nanoparticle loaded polydopamine modified flaky cobalt metal organic framework material as well as preparation method and application thereof
By loading palladium-copper nanoparticles on cobalt metal organic framework materials and using polydopamine modification to improve catalytic activity and stability, the problem of high temperature and slow kinetics of hydrogen production from ammonia borane hydrolysis was solved, and efficient photocatalysis and cycle stability were achieved. , overcoming the limitations of the instability of metal organic framework compounds and the large amount of precious metals in the existing technology.
Patent Information
- Application Number
- CN202410871635.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-18
AI Technical Summary
In the existing technology, the pyrolysis and alcoholysis hydrogen production reactions of ammonia borane have the problems of high temperature conditions and slow kinetics, and non-noble metal catalysts have poor activity in catalyzing hydrogen production from ammonia borane, and metal organic framework compounds have weak It is unstable under alkaline conditions and affects the activity and recyclability of the catalyst.
By coating polydopamine on the surface of cobalt metal-organic framework materials and loading palladium-doped copper nanoparticles using an impregnation method, a palladium-copper nanoparticle-loaded polydopamine-modified sheet cobalt metal-organic framework material was constructed for photocatalytic hydrogen production from ammonia borane. , improve catalytic activity and cycle stability.
It achieves efficient catalytic hydrolysis of ammonia borane to produce hydrogen under light irradiation, with a catalytic conversion frequency TOF as high as 56.9mol H2 (mol Cu)-1min-1, and improves the structural stability and photoresponsiveness of the catalyst, overcoming the challenges of a single metal-organic framework. The compound is unstable under weakly alkaline conditions and has limitations in the large amount of precious metals used.
Smart Images

Figure CN118788397A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic-organic hybrid materials, and specifically relates to a palladium-copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material, and a preparation method and application thereof. Background Art
[0002] Hydrogen energy is a secondary energy source that is abundant in source, green, low-carbon and widely used. It is an important carrier for the low-carbon transformation of energy and has broad application prospects in the hydrogen economy.
[0003] Hydrogen has a high energy density and its only product is water, so it is considered an ideal green energy source. However, under normal conditions, flammable and explosive hydrogen is difficult to be compressed efficiently. Therefore, the efficiency of hydrogen storage and preparation is the key to developing a hydrogen economy. The use of chemical hydrogen storage materials, including aluminum borohydride, amino aluminum borohydride, hydrazine borane and ammonia borane, is a feasible alternative. Among them, ammonia borane NH3BH3 has attracted widespread attention due to its high hydrogen storage mass density (19.6wt%) and high stability.
[0004] Hydrogen is generally prepared from ammonia borane through pyrolysis, hydrolysis, alcoholysis and other pathways. The pyrolysis of ammonia borane usually requires high temperature conditions, and the reaction is difficult to control; the alcoholysis of ammonia borane to produce hydrogen usually exhibits slow kinetics in the presence of organic solvents, and the rate of hydrogen release is slow. Relatively speaking, adding an appropriate catalyst to the aqueous solution can promote the hydrolysis of ammonia borane at room temperature to produce three equivalents of molecular hydrogen. In addition, the hydrolysis of ammonia borane to produce hydrogen can be further accelerated under light conditions.
[0005] At present, some metal catalysts are often used to catalyze the production of hydrogen from ammonia borane. For example, precious metal catalysts such as Pd, Pt, Rh and Ru can efficiently catalyze the production of hydrogen from ammonia borane. However, their high cost limits their practical application. Non-precious metal catalysts such as Co, Ni and Fe-based catalysts are relatively poor in catalyzing the production of hydrogen from ammonia borane. Therefore, binary metal nanocatalysts are constructed to combine non-precious metals with precious metals, and their catalytic activity can be improved by regulating the electronic structure of non-precious metals through precious metals. However, nano-sized catalysts are prone to aggregation of active components, which affects the activity and recyclability of the catalyst.
[0006] To solve the above problems, a simple and effective method is to find a suitable carrier for the nanocatalyst so that it can be evenly dispersed on the carrier material. However, the structure of some metal organic framework compounds is prone to collapse under weak alkaline conditions, and its stability needs to be further improved. In addition, the catalytic performance of metal organic framework compound-based materials needs to be further improved. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a palladium-copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material and a preparation method thereof. The polydopamine is wrapped on the outer surface of the cobalt metal organic framework material, and palladium-doped copper nanoparticles are loaded by an impregnation method to construct a palladium-copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material. The preparation method has simple steps, mild and controllable conditions, and is environmentally friendly.
[0008] The present invention also provides the use of polydopamine modified flaky cobalt metal organic framework materials loaded with palladium copper nanoparticles in photocatalytic hydrogen production from ammonia borane. The material can efficiently catalyze the decomposition of ammonia borane to produce hydrogen under light irradiation and exhibits high catalytic cycle stability.
[0009] The technical solution adopted by the present invention is as follows:
[0010] A method for preparing a palladium-copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material, the preparation method comprising the following steps:
[0011] (1) Using the surfactant polyvinyl pyrrolidone to induce the preparation of sheet-like cobalt metal organic framework materials;
[0012] (2) dispersing the flaky cobalt metal organic framework material in a tris (hydroxymethyl) aminomethane Tris-buffered solution, slowly adding a Tris buffer solution containing dopamine hydrochloride thereto, stirring for reaction, and separating and drying the product after the reaction is completed to obtain a polydopamine-modified flaky cobalt metal organic framework material;
[0013] (3) dispersing the polydopamine modified cobalt metal organic framework material in methanol, slowly adding an aqueous solution containing palladium salt and copper salt thereto, stirring evenly, and adding a reducing agent for reduction to obtain a polydopamine modified cobalt metal organic framework material loaded with palladium copper nanoparticles.
[0014] The step (1) specifically comprises: adding a cobalt salt aqueous solution to a mixed solution of DMF containing terephthalic acid and anhydrous ethanol, adding polyvinyl pyrrolidone thereto, mixing evenly, performing a hydrothermal reaction at 140 to 160° C. for 9 to 11 hours, and obtaining a flaky cobalt metal organic framework material through centrifugation, washing, and drying.
[0015] Furthermore, the mass ratio of cobalt salt, terephthalic acid and polyvinyl pyrrolidone is 1:0.05-0.10:1.3-2.0; the cobalt salt is any one of cobalt chloride, cobalt nitrate and cobalt sulfate.
[0016] In step (2), the mass ratio of the sheet-like cobalt metal organic framework material to dopamine hydrochloride is 1:1 to 1.2.
[0017] In step (2), the pH of the Tris-buffer solution is 8-9.
[0018] In step (2), the concentration of the sheet-like cobalt metal organic framework material in the Tris-buffered solution is 1 to 5 mg / mL.
[0019] In step (2), the concentration of dopamine hydrochloride in the Tris buffer solution containing dopamine hydrochloride is 20 to 30 mg / mL.
[0020] In step (2), the stirring reaction conditions are: stirring the reaction at room temperature for 4 to 6 hours.
[0021] In step (3), the mass ratio of polydopamine modified sheet cobalt metal organic framework material, palladium salt, copper salt and reducing agent is 1: 0.001-0.002: 0.05-0.30: 1-1.2, preferably 1: 0.001-0.002: 0.15-0.25: 1-1.2.
[0022] In step (3), the palladium salt is any one of palladium chloride and palladium nitrate; the copper salt is any one of copper nitrate and copper chloride, and the reducing agent is sodium tetrahydroborate.
[0023] In step (3), the concentration of the polydopamine modified sheet-like cobalt metal organic framework material in methanol is 1 to 5 mg / mL.
[0024] In step (3), the reduction reaction is carried out at room temperature for 1.5 to 2.5 hours.
[0025] The present invention also provides a polydopamine-modified flaky cobalt metal organic framework material loaded with palladium copper nanoparticles prepared by the preparation method, wherein the structure is an organic-inorganic hybrid material obtained by loading a trace amount of precious metal Pd doped with non-precious metal Cu nanoparticles on the polydopamine-modified flaky cobalt metal organic framework material, the polydopamine-modified metal organic framework material plays a dispersing and stabilizing role on the palladium copper nanoparticles, and the palladium copper nanoparticles with uniform and fine particle sizes in the structure are uniformly loaded in the polydopamine-modified metal organic framework material with a high specific surface area. When applied to a photocatalyst for hydrogen production by hydrolysis of ammonia borane, the substrate ammonia borane can fully contact the catalyst, and the polydopamine can enhance its light responsiveness, thereby improving its photocatalytic performance.
[0026] The present invention also provides the use of the polydopamine-modified sheet-shaped cobalt metal organic framework material loaded with palladium copper nanoparticles in the photocatalytic production of hydrogen from ammonia borane. When the photocatalytic hydrolysis of ammonia borane produces hydrogen, the conversion frequency TOF is as high as 56.9 mol H2 (mol Cu) -1 min -1When the hybrid material of polydopamine-modified sheet-like cobalt metal organic framework compound loaded with bimetallic nanoparticles is photocatalytically hydrolyzed by ammonia borane, trace amounts of palladium regulate the electronic structure of copper nanoparticles and synergistically induce the heterolytic cleavage of the boron-nitrogen coordination bond of ammonia borane, and then generate hydrogen and corresponding ammonium salts under the action of photogenerated holes and electrons, respectively, thereby improving its photocatalytic activity.
[0027] The method for photocatalytic hydrolysis of ammonia borane by polydopamine modified flaky cobalt metal organic framework material loaded with palladium copper nanoparticles is as follows: adding the polydopamine modified flaky cobalt metal organic framework material loaded with palladium copper nanoparticles to an aqueous solution of ammonia borane and performing a photocatalytic decomposition reaction under closed conditions.
[0028] In the preparation method of the polydopamine-modified flaky cobalt metal organic framework material loaded with palladium copper nanoparticles provided by the present invention, a flaky cobalt metal organic framework compound is firstly prepared, and then polydopamine is modified on the surface of the flaky cobalt metal organic framework material by a surface polymerization method, and then the palladium copper bimetallic nanoparticles are loaded in the polydopamine-modified flaky cobalt metal organic framework compound by means of impregnation, reduction and the like.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention overcomes the limitations of the prior art, such as the instability of single metal organic framework compounds under weakly alkaline conditions, the easy agglomeration of metal nanoparticles, and the large amount of precious metals used, and provides a way to develop polydopamine-modified sheet metal organic framework compounds loaded with ultrafine trace precious metal-doped non-precious metal nanoparticles.
[0031] The palladium-copper nanoparticle-loaded polydopamine-modified sheet-shaped cobalt metal organic framework material provided by the present invention is an inorganic-organic hybrid material formed by ultrafine trace precious metal Pd doped non-precious metal Cu bimetallic nanoparticles loaded with sheet-shaped polydopamine-modified cobalt metal organic framework, such as Fig. 9 As shown, the photocatalytic performance of the hydrogen production by hydrolysis of ammonia borane was tested, and the conversion frequency TOF of the hydrogen production by the hydrolysis of ammonia borane was as high as 56.9 mol H2 (mol Cu) -1 min -1 . BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A synthetic route for polydopamine-modified sheet-like cobalt metal-organic frameworks supported on palladium-copper nanoparticles;
[0033] Figure 2 SEM images of the materials, (a) Co-MOF prepared in Example 1; (b) Co-MOF-PDA prepared in Example 1; (c) Pd1Cu prepared in Example 1 150NPs@Co-MOF-PDA; (d) Pd1Cu prepared in Example 1 150 After the photocatalytic hydrolysis of ammonia borane by NPs@Co-MOF-PDA;
[0034] Figure 3 TEM images of the materials, (a) and (b) are Pd1Cu prepared in Example 1 150 TEM images of NPs@Co-MOF-PDA at different scales; (c) (d) Pd1Cu 150 HRTEM image of NPs@Co-MOF-PDA;
[0035] Figure 4 Pd1Cu prepared in Example 1 150 SEM mapping of NPs@Co-MOF-PDA;
[0036] Figure 5 Pd1Cu prepared in Example 1 150 XPS graph of NPs@Co-MOF-PDA;
[0037] Figure 6 The XRD patterns of the products prepared in each step of Example 1;
[0038] Figure 7 The solid UV images of the products prepared in each step of Example 1 and the products prepared in Comparative Example 4;
[0039] Figure 8 Pd1Cu 150 NPs@Co-MOF-PDA, Pd1Cu 150 Transient photocurrent response curves (a) and current impedance diagrams (b) of NPs@Co-MOF, Pd NPs@Co-MOF-PDA, and CuNPs@Co-MOF-PDA;
[0040] Fig. 9 (a) is Pd1Cu 150 Kinetic curves of NPs@Co-MOF-PDA catalyzing hydrogen production from ammonia borane under 300-watt xenon lamp irradiation at 25°C and in the dark; (b) Pd1Cu 150 NPs@Co-MOF-PDA, Pd1Cu 150 Kinetic curves of photocatalytic hydrogen production from ammonia borane by NPs@Co-MOF, Pd NPs@Co-MOF-PDA, and Cu NPs@Co-MOF-PDA under 300-W xenon lamp irradiation at 25°C. The catalytic conditions are 50 mM ammonia borane when the catalyst mass is 12 mg.
[0041] Fig.10 The different palladium-copper ratio materials Pd prepared in Example 1-2 x Cu y Kinetic curve (a) and XRD diagram (b) of photocatalytic hydrogen production from ammonia borane by NPs@Co-MOF-PDA at 25°C. The catalytic conditions are 50 mM ammonia borane when the catalyst mass is 12 mg.
[0042] Fig.11 Pd1M of different non-precious metals prepared in Comparative Example 1 150 Kinetic curve of photocatalytic hydrogen production from ammonia borane by NPs@Co-MOF-PDA at 25°C (a) and its XRD (b). The catalytic conditions are 50 mM ammonia borane when the catalyst mass is 12 mg.
[0043] Fig.12 Pd1M prepared in Example 1 150 The kinetic curves of photocatalytic hydrogen production from ammonia borane by NPs@Co-MOF-PDA at different temperatures (a) and the Arrhenius equation fitting diagram (b). The catalytic conditions are that the catalyst mass is 12 mg and the ammonia borane is 50 mM.
[0044] Fig.13 Pd1M prepared in Example 1 150 Kinetic curves of hydrogen production from ammonia borane with different concentrations photocatalyzed by NPs@Co-MOF-PDA (a) and rate equation fitting diagram (b), the catalyst mass is 12 mg, the temperature is 25 °C;
[0045] Fig.14 Pd1M of different masses prepared in Example 1 150 Kinetic curve of NPs@Co-MOF-PDA photocatalytic hydrogen production from ammonia borane (a) and its rate equation fitting diagram (b), ammonia borane is 50mM, temperature is 25℃;
[0046] Fig.15 Pd1M prepared in Example 1 150 The cyclic experimental diagram of NPs@Co-MOF-PDA photocatalytic hydrogen production from ammonia borane (a) and the XRD after the cycle (b). The catalytic conditions are catalyst mass 12 mg, temperature 25°C, and ammonia borane 50 mM.
[0047] Fig.16 Pd1M prepared in Example 1 150 NPs@Co-MOF-PDA photocatalyzes the production of hydrogen from ammonia borane in the presence of 0.1 mmol NaHCO3 or isopropanol and other quenchers. The catalytic conditions are 12 mg catalyst mass, 25 °C temperature, and 50 mM ammonia borane.
[0048] Fig.17 This is a diagram of the experimental setup for photocatalytic hydrogen production from ammonia borane, where a-25 ml jacketed reactor, b-constant temperature circulating water bath interlayer, c-magnetic stirrer, d-pressure dividing funnel, e-rubber tube, f-gradient tube, g-stopcock, h-level mark bottle, i-stirring magnet, j-300W xenon lamp light source. DETAILED DESCRIPTION
[0049] The present invention is described in detail below with reference to the embodiments.
[0050] Example 1
[0051] A method for preparing a palladium copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material comprises the following steps:
[0052] (1) Synthesis of Co-MOF: 20 mL of 1.6 g Co(NO3)2 . The aqueous solution of 6H2O was slowly added to 30mL of N, N'-dimethylformamide / anhydrous ethanol mixed solution containing 0.48g of terephthalic acid, wherein the volume of N, N'-dimethylformamide and anhydrous ethanol were both 20mL, the addition time was 5 minutes, and stirring was continued at room temperature for 10 minutes; then 2.4g of polyvinyl pyrrolidone was slowly added thereto in batches, stirred for 30 minutes, and the mixture was placed in a 100mL polytetrafluoroethylene stainless steel reactor, reacted at 150°C for 10h, after the reaction was completed, the reactor was cooled to room temperature, the pink powder product was collected, and it was repeatedly washed and centrifuged with deionized water and anhydrous ethanol for 6 times, and the product was finally dried in a vacuum oven at 70°C overnight to obtain a flaky cobalt metal organic framework material (Co-MOF).
[0053] (2) Preparation of Co-MOF-PDA: 120 mg of dried Co-MOF was ultrasonically dispersed in 55 mL of Tris buffer solution with a pH of 8.5. Under stirring, 5 mL of Tris buffer solution containing 120 mg of dopamine hydrochloride was added dropwise. The mixture was stirred for 5 h. The brown solid was separated by centrifugation, washed twice with deionized water and anhydrous ethanol, respectively, and then dried in a vacuum drying oven at 70 °C overnight to obtain a polydopamine-modified flaky cobalt metal organic framework material (Co-MOF-PDA).
[0054] (3)Pd1Cu 150Preparation of NPs@Co-MOF-PDA: 100 mg Co-MOF-PDA was ultrasonically dispersed in 45 mL methanol. Under stirring, 78 μL of an aqueous solution containing 0.138 mg PdCl2 and 20 mg CuCl2·2H2O was slowly added, and stirred at room temperature for 10 h. Then, 5 mL of an aqueous solution containing 100 mg NaBH4 was added dropwise, and stirred at room temperature for 2 h. The obtained black solid was centrifuged at 12,000 rpm, washed with methanol three times, and then placed in a vacuum drying oven at 70 °C for overnight vacuum drying to obtain a polydopamine-modified cobalt metal organic framework material (Pd1Cu 150 NPs@Co-MOF-PDA). Its SEM, TEM, HRTEM and mapping images are shown in Figure 1. Figure 2 , 3 , 4; From these figures, it can be seen that the metal palladium copper nanoparticles are uniformly loaded on the surface of Co-MOF-PDA, indicating that Co-MOF-PDA can effectively disperse metal nanoparticles. Figure 3 As can be seen from Figure (d), the interplanar spacing of the metal nanoparticles is 0.211 nm, which is between the lattice fringes of the Pd
[111] crystal plane (0.227 nm) and the lattice fringes of the Cu
[111] crystal plane (0.208 nm), indicating the existence of palladium-copper alloying effect.
[0055] Its XPS chart is as follows Figure 5 As shown in the figure, it can be seen that there are a large number of cobalt, palladium and copper. The peaks at 932.8 and 952.8 eV indicate the presence of zero-valent copper, indicating that divalent copper is reduced to copper nanoparticles; the two peaks at 935.8 and 955.6 eV indicate the presence of divalent copper, which is due to the fact that high-energy X-rays partially oxidize the surface of some copper nanoparticles during the XPS test. It should be pointed out that the XPS peak of the palladium element is very weak, because the amount of palladium added during the synthesis is very small, so that the content is small and the signal detected by XPS is weak. However, the ICP-MS data of the product obtained from step (3) are shown in Table 1. The results show that the molar ratio of palladium to copper in the product is 1:153, which is very close to the feed ratio of 1:150 during the synthesis.
[0056] Table 1
[0057]
[0058] The XRD patterns of the products prepared in each step of this embodiment are as follows: Figure 6 shown.
[0059] The solid UV images of the products prepared in each step of this embodiment are as follows: Figure 7As shown. It shows that after the hybrid material is modified with polydopamine PDA, its absorption of 200-800nm ultraviolet visible light is greatly enhanced, which is due to the π-π long-range conjugation effect of polydopamine. In particular, the absorption intensity of the hybrid material in the visible absorption region increases sharply, which is beneficial to improve the photocatalytic performance of the material.
[0060] Example 2
[0061] The rest is the same as in Example 1, except that the CuCl2 in step (2) is replaced by . The amount of 2H2O added was adjusted to 6.7 mg, 13.3 mg, and 26.7 mg, respectively, to prepare Pd1Cu 50 NPs@Co-MOF-PDA, Pd1Cu 100 NPs@Co-MOF-PDA, Pd1Cu 200 NPs@Co-MOF-PDA, their XRD patterns are as follows Fig.10 As shown in Figure (b).
[0062] Comparative Example 1
[0063] The rest is the same as in Example 1, except that the CuCl2 in step (2) is replaced by . 2H2O is replaced by an equal amount of NiCl2 . 6H2O、CoCl2 . 6H2O, FeCl3 . 6H2O.
[0064] Then Pd1Ni 150 NPs@Co-MOF-PD, Pd1Co 150 NPs@Co-MOF-PDA, Pd1Fe 150 NPs@Co-MOF-PDA, their XRD patterns are shown in Fig.11 As shown in Figure (b).
[0065] Comparative Example 2
[0066] The rest is the same as Example 1, except that the addition of CuCl2·2H2O in step (3) is omitted, and the obtained material is Pd NPs@Co-MOF-PDA.
[0067] Comparative Example 3
[0068] The rest is the same as in Example 1, except that the addition of PdCl2 in step (3) is omitted, and the obtained material is Cu NPs@Co-MOF-PDA.
[0069] Comparative Example 4
[0070] The rest is the same as in Example 1, except that step (2) is omitted, and the obtained material is Pd1Cu 150 NPs@Co-MOF.
[0071] Application Example 1
[0072] The materials prepared in the above examples and comparative examples were used in the photocatalytic hydrolysis experiment of ammonia borane to evaluate the catalytic effect of each material.
[0073] The basic principle is:
[0074] The specific steps are as follows: the activity of the prepared catalyst in the photocatalytic ammonia borane hydrolysis hydrogen production reaction is measured in a typical gas burette system filled with water, the light source used is a 300-watt Perfill xenon lamp, and the reaction temperature is controlled by constant temperature circulating water. The gas burette system is as follows: Fig.17 As shown. 5 ml of aqueous solution containing 12 mg of materials prepared in each embodiment and comparative example was added to a 25 ml double-layer jacketed reactor. The circulating water in the interlayer was connected to the water in the fully automatic thermostat. One neck was used to add the aqueous solution of ammonia borane, and the other neck was connected to the gas measuring tube system filled with water through a vacuum head and a hose. Dissolve ammonia borane in 5 ml of distilled water, quickly inject it from the constant pressure reactor, immediately unscrew the piston, press the stopwatch, and record the scale of the water surface in the gas measuring tube system. When no bubbles emerge, the reaction is over. In order to measure the activation energy of catalytic hydrolysis of ammonia borane, adjust the circulating water temperature of the fully automatic thermostat to 25, 30, 35, 40, and 45°C, respectively. Repeat the above experiment.
[0075] The kinetic curves of the hydrolysis of ammonia borane catalyzed by the products in Examples 1-2 and Comparative Examples 1 to 4 are shown in Figures 8-10. It can be seen from the figure that Pd1Cu 150 NPs@Co-MOF-PDA has the fastest time for catalyzing ammonia borane to produce hydrogen. The Co-MOF-PDA carrier is better than Co-MOF. The palladium-copper ratio of 1:150 has the best catalytic effect. The catalytic effect of non-precious metal copper doped with palladium is better than that of nickel, cobalt, iron and zinc doped with palladium.
[0076] Pd1Cu 100 TEM of the catalyst recovered after catalytic hydrogen production from ammonia borane by NPs@Co-MOF-PDA. Figure 2 As shown in Figure (d), it can be seen from the figure that the structure and morphology before and after catalysis remain basically unchanged, indicating that the catalyst has high stability.
[0077] Pd1Cu 150 The XRD pattern of the catalyst recovered after NPs@Co-MOF-PDA catalyzed hydrogen production from ammonia borane is shown in Figure 2. Fig.15As shown in Figure (b), it can be seen from the figure that its structure remains basically unchanged before and after catalysis, indicating that the hybrid material has high stability.
[0078] Pd1Cu 150 The kinetic curves of NPs@Co-MOF-PDA catalyzing hydrogen production from ammonia borane at different temperatures and its Arrhenius equation fitting diagram are shown in Figure 2. Fig.12 As shown in the figure, it can be seen that its activation energy is 43.3 kJ mol, indicating that its activation energy is low and the catalytic rate is fast.
[0079] Pd1Cu 150 The kinetic curves and rate equation fitting diagrams of hydrogen production by NPs@Co-MOF-PDA catalyzed by different concentrations of ammonia borane are shown in Figure 2. Fig.13 As shown in the figure, it can be seen that the change in the concentration of the catalytic substrate does not affect the catalytic rate, indicating that for the substrate, it is a zero-order reaction.
[0080] Pd1Cu of different quality 150 The kinetic curve of hydrogen production from ammonia borane catalyzed by NPs@Co-MOF-PDA and its rate equation fitting diagram are shown in Figure 2. Fig.14 As shown in the figure, it can be seen that the catalyst mass and the catalytic rate are in a linear relationship, indicating that for the catalyst, it is a first-order reaction.
[0081] Application Example 2
[0082] Cyclic stability test of hydrogen production from ammonia borane catalyzed by hybrid materials of porous cobalt-zinc core-shell metal-organic framework compounds and confined noble metal nanoparticles
[0083] 5 ml of Pd1Cu 100 The aqueous dispersion of NPs@Co-MOF-PDA was placed in a reactor, the water bath temperature was 40°C, magnetic stirring was applied for 5 min, and then 5 ml of 31 mg of ammonia borane aqueous solution was injected, and the hydrogen generation rate was recorded. When no gas was emitted, 5 ml of 31 mg of ammonia borane aqueous solution was injected again, and the hydrogen generation rate was recorded. This was repeated 5 times. The results are shown in Fig.15 As shown, from Fig.15 It can be seen that its activity remains basically unchanged after 5 cycles.
[0084] Fig.16 Pd1M prepared in Example 1 150 NPs@Co-MOF-PDA photocatalyzes hydrogen production from ammonia borane in the presence of 0.1mmol NaHCO3 or isopropanol as a quencher. The catalytic conditions are Pd1Cu 100 When the mass of NPs@Co-MOF-PDA catalyst is 12 mg, the temperature is 25 °C, and the ammonia borane is 50 mM.
[0085] Under the conditions of 300W xenon lamp irradiation and circulating water temperature control at 25 degrees Celsius, hole scavenger NaHCO3 and free radical scavenger isopropanol were introduced as hydroxyl groups to study the Pd1Cu 100 Performance of NPs@Co-MOF-PDA in catalyzing the hydrolysis of ammonia borane to produce hydrogen. When 0.1mmol NaHCO3 was added, the rate of photocatalytic hydrogen production from ammonia borane decreased significantly, indicating that the photogenerated vacancies played an important role in the photocatalytic hydrogen production from ammonia borane. When 0.1mmol isopropanol was added, the rate of photocatalytic hydrogen production from ammonia borane decreased slightly, indicating that hydroxyl radicals played a minor role in the photocatalytic reaction of ammonia borane. Therefore, the mechanism of photocatalytic hydrogen production from ammonia borane hydrolysis may be as follows: (1) Pd1Cu 100 NPs@Co-MOF-PDA complexes and adsorbs ammonia borane to activate the substrate; (2) the BN bond of activated ammonia borane breaks to form BH3 δ- and NH3 δ+ Intermediate; (3) The intermediate undergoes the following reaction to produce 3 equivalents of hydrogen:
[0086] NH3 δ+ + e - + H2O→ NH4OH (1);
[0087] BH3 δ- + h + + 2H2O → HBO2 + 3H2 (2).
[0088] The detailed description of a palladium-copper nanoparticle-loaded polydopamine-modified flaky cobalt metal organic framework material and its preparation method and application with reference to the above-mentioned embodiment is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a palladium copper nanoparticle-loaded polydopamine-modified sheet-shaped cobalt metal organic framework material, characterized in that: The preparation method comprises the following steps: (1) Using the surfactant polyvinyl pyrrolidone to induce the preparation of sheet-like cobalt metal organic framework materials; (2) dispersing the flaky cobalt metal organic framework material in a tris(hydroxymethyl)aminomethane Tris-HCl buffer solution, slowly adding a Tris buffer solution containing dopamine hydrochloride thereto, stirring for reaction, and separating and drying the product after the reaction is completed to obtain a polydopamine-modified flaky cobalt metal organic framework material; (3) dispersing the polydopamine modified cobalt metal organic framework material in methanol, slowly adding an aqueous solution containing palladium salt and copper salt thereto, stirring evenly, and adding a reducing agent for reduction to obtain a polydopamine modified cobalt metal organic framework material loaded with palladium copper nanoparticles.
2. The preparation method according to claim 1, characterized in that: The step (1) specifically comprises: adding a cobalt salt aqueous solution to a mixed solution of DMF containing terephthalic acid and anhydrous ethanol, adding polyvinyl pyrrolidone thereto, mixing evenly, performing a hydrothermal reaction at 140 to 160° C. for 9 to 11 hours, and obtaining a flaky cobalt metal organic framework material through centrifugation, washing, and drying.
3. The preparation method according to claim 2, characterized in that: The mass ratio of cobalt salt, terephthalic acid and polyvinyl pyrrolidone is 1:0.05-0.10:1.3-2.0; the cobalt salt is any one of cobalt chloride, cobalt nitrate and cobalt sulfate.
4. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the sheet-like cobalt metal organic framework material to dopamine hydrochloride is 1:1 to 1.
2.
5. The preparation method according to claim 1, characterized in that: In step (2), the pH of the Tris-buffer solution is 8-9.
6. The preparation method according to claim 1, characterized in that: In step (2), the stirring reaction conditions are: stirring the reaction at room temperature for 4 to 6 hours.
7. The preparation method according to claim 1, characterized in that: In step (3), the mass ratio of the polydopamine-modified sheet-like cobalt metal organic framework material, palladium salt, copper salt, and reducing agent is 1: 0.001-0.002: 0.05-0.30: 1-1.
2.
8. The preparation method according to claim 1, characterized in that: In step (3), the palladium salt is any one of palladium chloride and palladium nitrate; the copper salt is any one of copper nitrate and copper chloride, and the reducing agent is sodium tetrahydroborate.
9. A polydopamine-modified flaky cobalt metal organic framework material loaded with palladium copper nanoparticles prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the polydopamine-modified sheet-shaped cobalt metal organic framework material loaded with palladium copper nanoparticles as claimed in claim 9 in photocatalytic hydrogen production from ammonia borane.
Citation Information
Patent Citations
Preparation method of sheet Co-MOF nano material and application thereof in electric catalysis
CN106944141A
Hybrid material of porous cobalt-zinc core-shell metal organic framework compound confinement noble metal nanoparticle, preparation method and application thereof
CN111330639A
Composite material N-Co-MOF@PDA-Ag and preparation method and application thereof
CN113567531A
Composite material as well as preparation method and application thereof
CN114345411A
Catalyst for ammonia borane hydrolysis hydrogen evolution and preparation method thereof
CN115608375A