Manufacturing method of bimetal composite plate with X65-level composite layer made of nickel-based alloy
By adopting the bimetallic composite plate manufacturing method of X65 grade clad with nickel-based alloy in the transportation of offshore oil and gas resources, the problem of difficulty in matching the performance of nickel-based alloys and traditional pipeline steel in highly corrosive environments has been solved, and efficient corrosion resistance has been achieved. The combination of physical properties and mechanical properties makes it suitable for the transportation of oil and gas resources rich in corrosive media such as H2S, CO2, and Cl-.
Patent Information
- Application Number
- CN202410772376.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
AI Technical Summary
It is difficult for the existing technology to effectively match the corrosion resistance of nickel-based alloys and the mechanical properties of traditional pipeline steel in the transportation of marine oil and gas resources, making it difficult to use in corrosive medium environments such as high concentrations of H2S, CO2, and Cl-.
The manufacturing method of bimetallic composite panels with X65 grade cladding as nickel-based alloy is adopted. Through reasonable component design and preparation process optimization, including composite billet rolling, post-rolling heat treatment and tempering treatment, the yield strength and corrosion resistance of the composite panels are ensured. Sex meets the requirements.
Producing oil and gas transmission line pipes with a yield strength no less than
Smart Images

Figure BDA0004894547690000061 
Figure BDA0004894547690000062 
Figure BDA0004894547690000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-strength corrosion-resistant structural steel manufacturing, and in particular to a method for manufacturing a bimetallic composite plate whose X65-grade composite layer is a nickel-based alloy. Background Art
[0002] Oil and natural gas are the energy pillars of social development. my country is in a period of rapid development. The increase in energy demand and price increases have led to an increase in oil and natural gas exploration and production activities. Marine oil and gas resources have become a new growth pole for my country's oil and gas resources. In recent years, 80% of my country's new oil and gas has come from the ocean. Marine oil and gas resources contain a large amount of H2S, CO2, Cl - Conventional pipeline steel can no longer meet the safety requirements for transportation of corrosive media such as H2S, CO2, and Cl. Due to the limitation of offshore operation space, the corrosive medium removal device cannot be installed in sufficient quantity, resulting in the corrosive medium content not being able to reach the permitted range of existing pipeline steel. Therefore, the current solution to this problem is to use H2S, CO2, and Cl - The pipeline is made of materials with good corrosion resistance to corrosive media such as stainless steel, titanium alloy, and nickel-based alloy. - In corrosive media environments, nickel-based alloys have unique advantages.
[0003] Nickel-based alloys contain a large amount of Ni and are expensive. In addition, they also contain a large amount of Cr, Mo, Nb and other elements. In order to ensure uniform composition and cleanliness, vacuum smelting, vacuum smelting + electroslag remelting and other methods are required for production. Due to both composition and process reasons, nickel-based alloys are expensive. It is difficult to directly use nickel-based alloys to prepare conveying pipes to replace traditional pipeline pipes, and traditional pipeline pipes have insufficient corrosion resistance. In response to this problem, people have proposed a bimetallic composite solution, that is, using traditional pipeline steel as the base material to ensure mechanical properties and weldability, and using corrosion-resistant alloys as composite materials to ensure corrosion resistance. In order to produce pipeline steel and nickel-based alloy composite plates, the main problem is that the deformation coordination of dissimilar metals is difficult to solve, and it is difficult to achieve a comprehensive match of mechanical properties and corrosion resistance using the same production process.
[0004] Application document CN201710453074.4 announced "a method for preparing a large-size, thin-layer nickel-based alloy / pipeline steel composite plate". This technical solution uses explosive welding to prepare composite billets, and then asynchronous rolling with a speed ratio of 1.05 to 1.30 overcomes the deformation incompatibility between the two metals to obtain the desired composite plate. In addition to the higher billet assembly efficiency than welding billet assembly, the explosive method for preparing composite billets has defects such as high noise, low composite billet bonding quality, and a narrow billet size range.
[0005] Application document CN201610487980.1 announced "A X80 grade thick specification pipeline steel composite plate and its manufacturing method". This technical solution uses homogeneous steel billets to prepare composite plates, and the focus is on the thickness of the composite plates. For heterogeneous composite plates prepared from pipeline steel billets and Inconel625 metal plates, there is no technical help in the comprehensive matching of the mechanical properties and corrosion resistance of the composite plates.
[0006] Application document CN201610052976.2 announced "a nickel-based alloy composite steel plate for pipelines and its manufacturing method". The nickel-based composite layer selected in this technical solution contains 22-28% iron, which is closer to the chemical properties of the carbon steel layer of the base layer; after rolling, the composite plate is treated by air cooling, water cooling, solid solution treatment (900-1150℃; 2-100℃ / s cooled to below 650℃; 400-650℃×1mm / min×plate thickness). Application document CN201710983305.2 announced "a 825 / X70 / 825 double-sided composite plate and its production method", and application document CN201710983510.9 announced "a 825 / X70 nickel-based alloy composite plate and its production method". The corrosion-resistant layer of these two technical solutions is 825 alloy, which contains no less than 22% of iron elements. The chemical properties are closer to the matrix, which makes it easier to solve the deformation incoordination. In terms of technology, the final rolling temperature is 760-830°C. In the above-mentioned prior art, in order to solve the problem of deformation incoordination, some nickel-based alloys with higher Fe content are used to reduce the property differences between dissimilar metals, and some are asynchronous rolling technology. Asynchronous rolling technology has strict requirements on the capacity of the rolling mill. If the Fe content is increased, the excellent corrosion resistance of Inconel 625 alloy will not be fully utilized. In order to solve these problems, the components of X65 and Inconel 625 can be comprehensively optimized and then matched with appropriate rolling and heat treatment processes. Summary of the invention
[0007] The purpose of the present invention is to provide a method for manufacturing a bimetallic composite plate with an X65 grade composite layer of a nickel-based alloy, to produce a bimetallic composite plate for oil and gas pipelines with a yield strength not lower than X65 and excellent corrosion resistance, to overcome the shortcomings of the prior art through reasonable component design and optimized matching of the preparation process, and to provide a bimetallic composite plate for oil and gas pipelines rich in H2S, CO2, Cl - It provides a new technical solution for the selection of pipelines for transporting oil and gas resources in corrosive media.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for manufacturing a bimetallic composite plate with an X65 grade composite layer being a nickel-based alloy comprises the following steps:
[0010] 1) Composite billet rolling: The composite billet with a thickness of H after the billet assembly welding is reheated to 1200-1250℃ (T1), kept at this temperature for 2-4 hours (t1), and then rolled to the target thickness t after being removed from the furnace and descaled. c The final rolling temperature is not less than 1000℃ (T2), and the steel is immediately water-cooled to 300~600℃ (T3) after rolling, with a cooling rate of not less than 5℃ / s (R c ), air-cooled to room temperature; during rolling, in order to ensure the composite effect, H / t c ≥5.
[0011] 2) Heat treatment after rolling: The composite plate is tempered at a tempering temperature of 500-600°C (T4). The tempering time t2 is calculated according to t2=t×(1-3)min / mm+15min, where t is the thickness of the composite plate during heat treatment, in mm.
[0012] The base material of the composite plate is X65 iron-based alloy, and the composite material is Inconel 625 nickel-based alloy.
[0013] The combined welding method of the composite blank comprises:
[0014] 1) Prepare raw materials: The base material X65 uses continuous casting billets, and the composite material Inconel 625 uses metal plates. The thickness of the raw materials is designed according to the thickness ratio required by the dissimilar metals in the finished composite plate; Inconel 625 is required to be in a solid solution state, and its matrix phase γ phase content v γ Not less than 95%.
[0015] 2) Symmetrical billet assembly: Each composite billet consists of two X65 continuous casting billets of the same size and two Inconel 625 metal plates.
[0016] 3) Raw material cleaning: Use mechanical methods to remove all oxide layers from the original surface of the raw material parallel to the rolling surface to expose fresh metal.
[0017] 4) Spraying the isolation agent: Evenly spray a metal oxide with a thickness of 1 to 2 mm on the non-cleaned surface of the composite Inconel 625 metal plate. The metal oxide is MgO or Al2O3, and is dispersed into a toothpaste-like state with water. After the water evaporates naturally, the blanks are assembled. The composite can also be placed in a drying furnace with a temperature T5 not higher than 200°C for drying. The isolation agent after drying is not allowed to have defects such as cracks and holes to prevent the two composite metals from sticking together during the rolling process.
[0018] 5) Assembly welding: stack the four layers of metal in sequence, from top to bottom, X65-Inconel 625-isolator-isolator-Inconel 625-X65, to form a composite billet with a thickness of H; when dissimilar metals come into contact, the cleaned surfaces without oxide layer are in direct contact; the stacked raw materials are formed into a composite billet through the outer edge of the welding contact surface, and a vacuum channel is left to reduce the internal pressure P of the combined billet to no more than 5Pa before completing the final welding.
[0019] The composite plate splitting method comprises: cutting off the four sides of the composite plate with welds, separating the composite plate along the isolation agent layer, and obtaining two composite plate sub-plates, the sub-plates having a thickness of t c / 2.
[0020] The order of plate separation and post-rolling heat treatment of composite plates can be adjusted according to the actual situation. When calculating the tempering time t2, the t in the formula is calculated according to the actual thickness t of the heat-treated workpiece. c or c / 2 can be calculated.
[0021] The composite plate is prepared by the manufacturing method of the bimetallic composite plate whose X65 grade composite layer is a nickel-based alloy, and the chemical composition of the base material is as follows by weight percentage: C 0.02%-0.08%, Si 0.15%-0.25%, Mn 0.65%-1.95%, Cr 0.05%-0.35%, Mo 0.05%-0.35%, V0.02%-0.06%, Nb≤0.05%, Al≤0.05%, Ti≤0.05%, and the balance is Fe and unavoidable impurity elements;
[0022] The chemical composition of the composite material is calculated by weight percentage as follows: C≤0.08%, Si≤0.5%, Mn≤0.5%, Cr20.0%-23.0%, Mo 8.0%-10.0%, Nb 3.15%-4.15%, Fe≤5.0%, Al≤0.05%, Ti≤0.05%, and the balance is Ni and unavoidable impurity elements.
[0023] Composite plate yield strength R t0.5 ≥450MPa, tensile strength R m ≥540MPa, elongation A≥15%, -20℃ transverse Charpy impact Akv≥220J, -20℃ transverse DWTT shear area SA≥90%, composite plate interface bonding strength R S ≥400MPa, composite layer pitting corrosion rate v pit ≤3.5g / m 2 (ASTM G48 A method), composite layer intergranular corrosion rate v ig ≤0.8mm / a (ASTM G28 A method).
[0024] The main component design ideas of the present invention are as follows:
[0025] The base material X65 is an iron-based alloy, which contains the easily diffusible alloy element C; the composite material Inconel 625 is a nickel-based alloy, in which C may or may not be added. The main form of C in the composite material is to form carbides with the strengthening elements Nb, Mo, and Cr, among which NbC can appear in the liquid phase and is a primary carbide. In order to avoid the formation of carbides such as NbC due to the diffusion of C at the X65 / Inconel 625 interface, which affects the bonding strength of the interface, the present invention adopts a low C component design, the carbon content in X65 ranges from 0.02% to 0.08%, and the C content in Inconel 625 does not exceed 0.08%. It is recommended that the C content in Inconel 625 is lower than that in X65.
[0026] Compared with the two metals. X65 has high content of Fe and Mn elements, while Inconel 625 has high content of Ni, Cr, Mo and Nb elements. Due to the rolling effect, diffusion couples can be formed at the interface, thereby forming a diffusion layer of a certain thickness to achieve metallurgical bonding, which is beneficial to improving the interface strength. Ni, Cr, Mo, and Nb diffuse into the Fe lattice, and Fe and Mn diffuse into the Ni lattice, all of which form substitutional solid solutions or intermetallic compounds. These changes all occur in the solid phase, and the phase change rate is relatively slow, and the effect on the phase structure of the interface is not significant. Therefore, the composition design is mainly to avoid the formation of harmful phases in Inconel 625 that are not conducive to corrosion performance. Because the raw material of the composite is Inconel 625 alloy plate, it must be fully solution treated before assembly, and the γ phase content in the matrix phase is v γ Not less than 95%, especially carbides and carbonitrides are not allowed to be produced on grain boundaries. The control of Inconel 625 phase composition is more through process control rather than composition design restrictions. In order to deal with pitting corrosion, the pitting equivalent PREN of Inconel 625 is required to be not less than 46.4. PREN calculation formula Cr% + 3.3 × Mo% + 16 × N%.
[0027] The reasons for the control range of the main manufacturing process parameters of the present invention are as follows:
[0028] Inconel 625 alloy has a high element content and high deformation resistance. Compared with X65, at the same deformation temperature, the deformation resistance of Inconel625 alloy is higher than that of X65. The lower the temperature, the more significant the deformation resistance between the two. Therefore, when the billet is rolled, the rolling elongation of Inconel 625 alloy will be lower than that of X65, causing the composite plate to bend and the thickness ratio of the composite layer to the base layer to be uncontrollable. In order to avoid the rolling difficulties caused by the uncoordinated deformation of the two, symmetrical billet assembly is adopted, the reheating temperature of the composite billet is increased, and the final rolling temperature of the composite plate is increased. At this time, a deformation of the two metals close to 1:1 in the rolling direction can be obtained. Completing the rolling before 1000°C is the key to the present invention to ensure the coordinated deformation of X65 and Inconel 625. At this time, the difference in rolling resistance between the two does not exceed 100MPa.
[0029] After high-temperature rolling, the Inconel 625 alloy will inevitably go through the sensitization temperature range during the cooling process. In order to avoid the appearance of harmful phases, the cooling rate must be increased to reduce the residence time in the sensitization temperature range. After the cooling rate is increased, due to the difference in the thermophysical parameters of the two metals, a large residual stress will be brought. Therefore, tempering treatment is required after water cooling to avoid damage to the interface bonding quality. Water cooling is used directly after rolling, and the accelerated cooling temperature is significantly higher than the production system of traditional pipeline steel. In addition to ensuring the coordinated deformation of the two metals, in order to make up for the improvement of strength and toughness of the grain refinement of the austenite flattening process in the non-recrystallization zone of X65, high final rolling, high accelerated cooling temperature and tempering heat treatment are used to ensure that the mechanical properties of X65 and the corrosion resistance of Inconel 625 alloy meet the target requirements at the same time.
[0030] The greater the difference in strength, plasticity, thermal expansion coefficient and other indicators between the materials, the greater the residual stress that can be generated at the interface and its vicinity after metallurgical compounding. Therefore, the tempering temperature adopted by the present invention is relatively high, reaching the temperature range of high-temperature tempering required in the conventional quenching and tempering process. Only when the tempering temperature is high and sufficient holding time is combined can the residual stress generated by the coordinated deformation of the interface be fully eliminated. At the same time, the temperature has not yet reached the temperature range where harmful precipitation phases are generated in Inconel 625 and the grains of X65 grow significantly, thereby achieving the structural-functional integration of strength and corrosion resistance.
[0031] Compared with the prior art, the present invention has the following beneficial effects.
[0032] 1) The rolling method can significantly improve production efficiency by producing composite plates. Compared with the explosion method, composite plates can obtain a better plate shape, which is one of the key requirements for subsequent composite plate pipe making.
[0033] 2) Through a post-rolling treatment method similar to "quenching and tempering", the impact on the corrosion-resistant layer of the composite plate during reheating and cooling is reduced, and the large-scale precipitation of harmful phases is avoided, thereby ensuring excellent corrosion resistance; at the same time, the fine austenite recrystallized grains in the rolling stage are retained as much as possible, and the precipitation strengthening brought about by the subsequent tempering process is assisted by fine grain strengthening, which meets the strength and toughness matching requirements of X65.
[0034] 3) Compared with other composite methods, rolling composite has a certain width of diffusion layer at the interface. When there is no large amount of brittle phase in the diffusion layer, the interface bonding strength is excellent. By consciously reducing the C content, the formation of brittle phase is avoided, and a good interface bonding effect is obtained. The interface bonding strength is not less than 80% of the lower limit of the composite plate strength, meeting the 0.8 coefficient requirement of pipeline design.
[0035] 4) Yield strength R of the composite plate t0.5 ≥450MPa, tensile strength R m ≥540MPa, elongation A≥15%, -20℃ transverse Charpy impact A kv ≥220J, -20℃ transverse DWTT shear area SA ≥90%, composite plate interface bonding strength R S ≥360MPa, composite layer pitting corrosion rate v pit ≤3.5g / m 2 (ASTM G48 A method), composite layer intergranular corrosion rate v ig ≤0.8mm / a (ASTM G28 A method). DETAILED DESCRIPTION
[0036] The following examples are used to describe the technical solutions of the present invention clearly and completely. The following examples are used to specifically illustrate the content of the present invention. These examples are only general descriptions of the content of the present invention and do not limit the content of the present invention.
[0037] The present invention relates to a bimetallic composite plate with a yield strength not less than X65 grade, which is composed of API X65 as a base material and Inconel 625 as a composite material, and a manufacturing method thereof, including steelmaking and refining, casting, rolling, cooling and heat treatment processes, which can meet the material selection requirements in the field of oil and gas pipeline steel that is allowed to be supplied in a heat-treated state, and is suitable for the production of steel rich in H2S, CO2, Cl - The composite material in the present invention can be any nickel-based alloy.
[0038] Table 1 shows the chemical composition of the substrate X65 and the composite Inconel 625 of the embodiment of the present invention; Table 2 shows the rolling and heat treatment process parameters of the composite plate of the embodiment of the present invention; Table 3 shows the mechanical properties and corrosion resistance of the composite plate of the embodiment of the present invention.
[0039] Table 1 Chemical composition of the composite plate of the present invention by weight
[0040]
[0041] Note: * represents residual elements, the sum of which with other elements is 100%; - represents no intentional addition; 625 means Inconel625.
[0042] Table 2 Rolling and heat treatment process parameters of the composite plate of the embodiment of the present invention
[0043]
[0044] Note: RT- stands for natural drying at room temperature.
[0045] Table 3 Mechanical properties and corrosion resistance of the composite plate of the present invention
[0046]
[0047] From the data in Tables 1, 2 and 3, it can be seen that the technical solution adopted by the present invention has a composite plate yield strength ≥450MPa, a tensile strength ≥540MPa, an elongation ≥15%, a -20°C transverse Charpy impact ≥220J, a -20°C transverse DWTT shear area ≥90%, a composite plate interface bonding strength ≥360MPa, and a composite layer pitting corrosion rate ≤3.5g / m 2 , intergranular corrosion rate ≤0.8mm / a, the produced composite plate has a good match of strength, toughness and corrosion resistance.
[0048] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. Manufacturing method of bimetallic composite plate with X65 grade composite layer as nickel-based alloy, It is characterized in that The method comprises the following steps: 1) Composite billet rolling: The composite billet with a thickness of H after the billet assembly is reheated to 1200-1250°C, kept warm for 2-4 hours, and rolled to the target thickness t after being removed from the furnace and descaled. c The final rolling temperature is not less than 1000℃. After rolling, it is immediately water-cooled to 300-600℃, with a cooling rate of not less than 5℃ / s, and air-cooled to room temperature. During rolling, H / t c ≥5; 2) Post-rolling heat treatment: The composite plate is tempered at a temperature of 500-600°C and a tempering time of t 2 According to t 2 =t×(1~3)min / mm+15min, where t is the thickness of the composite plate during heat treatment, in mm.
2. The method for manufacturing the bimetallic composite plate with X65 grade composite layer being a nickel-based alloy according to claim 1, It is characterized in that The base material of the composite plate is X65 iron-based alloy, and the composite material is Inconel 625 nickel-based alloy.
3. The method for manufacturing the bimetallic composite plate with X65 grade composite layer being a nickel-based alloy according to claim 1 or 2, It is characterized in that The combined welding method of the composite blank comprises: 1) Symmetrical billet assembly: Each composite billet consists of two X65 continuous casting billets and two Inconel 625 metal plates of the same size; 2) Raw material cleaning: Use mechanical methods to remove all oxide layers from the original surface of the raw material parallel to the rolling surface to reveal fresh metal; 3) Spraying the isolation agent: Evenly spray the metal oxide with a thickness of 1 to 2 mm on the non-cleaned surface of the composite Inconel 625 metal plate; 4) Assembly welding: stack the four layers of metal in sequence, from top to bottom, X65-Inconel 625-isolator-isolator-Inconel 625-X65, to form a composite billet with a thickness of H; reduce the internal pressure of the combined billet to no more than 5Pa before completing the final welding.
4. The method for manufacturing the bimetallic composite plate with X65 grade composite layer being a nickel-based alloy according to claim 3, It is characterized in that The metal oxide is MgO or Al 2 O 3 , dispersed with water into toothpaste.
5. The method for manufacturing the bimetallic composite plate with X65 grade composite layer being a nickel-based alloy according to claim 1 or 2, It is characterized in that The composite plate splitting method comprises: cutting off the four sides of the composite plate with welds, separating the composite plate along the isolation agent layer, and obtaining two composite plate sub-plates, the sub-plates having a thickness of t c / 2.
6. A composite plate prepared by the method for manufacturing a bimetallic composite plate with an X65-grade composite layer of a nickel-based alloy as claimed in any one of claims 1 to 5, It is characterized in that The chemical composition of the substrate is calculated by weight percentage as follows: C 0.02% to 0.08%, Si 0.15% to 0.25%, Mn 0.65% to 1.95%, Cr 0.05% to 0.35%, Mo 0.05% to 0.35%, V 0.02% to 0.06%, Nb ≤ 0.05%, Al ≤ 0.05%, Ti ≤ 0.05%, and the balance is Fe and unavoidable impurity elements; The chemical composition of the composite material is calculated by weight percentage as follows: C≤0.08%, Si≤0.5%, Mn≤0.5%, Cr 20.0%-23.0%, Mo 8.0%-10.0%, Nb 3.15%-4.15%, Fe≤5.0%, Al≤0.05%, Ti≤0.05%, and the balance is Ni and unavoidable impurity elements.
7. A composite plate prepared by the method for manufacturing a bimetallic composite plate with an X65-grade composite layer of a nickel-based alloy according to claim 6, It is characterized in that Composite plate yield strength R t0.5 ≥450MPa, tensile strength R m ≥540MPa, elongation A≥15%, -20℃ transverse Charpy impact A kv ≥220J, -20℃ transverse DWTT shear area SA ≥90%, composite plate interface bonding strength R S ≥360MPa, composite layer pitting corrosion rate v pit ≤3.5g / m 2 , intergranular corrosion rate of composite layer v ig ≤0.8mm / a.
Citation Information
Patent Citations
Nickel base alloy clad steel plates for pipeline and manufacturing method thereof
CN105671424A
Wear-resistant composite steel plate and manufacturing method thereof
CN109835015A
Preparation method of QT-state nickel-based alloy composite plate
CN117816773A
Steel plate for API-X65 grade line pipe guaranteedstress relief and method of manufacturing them
KR1020020027013A
Cited By
Hot rolling composite process for improving strength of low-alloy high-strength steel / nickel-based alloy bimetal composite plate
CN120079697A
Bimetal composite plate with X90-level composite layer made of nickel-based alloy Inconel625 and manufacturing method of bimetal composite plate with X90-level composite layer made of nickel-based alloy Inconel625
CN120697385A
Double-metal composite plate with X70-level composite layer made of nickel-based alloy Inconel 625 and manufacturing method of double-metal composite plate
CN120697386A
Low-stress gradient annealing process for X65 steel / Inconel 625 composite board
CN120758723A
Nickel-based corrosion-resistant alloy-steel composite plate and preparation method thereof
CN122558992A