A method for integrated molding of multi-stage disk-shaft structure

By using vacuum powder calcining technology combined with ceramic cover and gasket assembly in the preparation of multi-stage disc shaft structure, combined with oscillation pressure sintering and solid solution treatment, the problems of large material removal, long processing time and unstable accuracy are solved. It realizes efficient and low-cost multi-stage disc shaft structure preparation, improving the mechanical properties and machining accuracy of the product.

CN118788967BActive Publication Date: 2024-11-19HUNAN SHENGHANG POWER TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411288730.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-19
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

There are problems such as large amount of material removal, long processing time and unavailable processing accuracy during the preparation of existing multi-stage disc shaft structures.

Method used

By using the integrated molding method of multi-stage disc shaft structure, the raw material powder is filled in the ceramic cover, the multi-layer annular groove structure arranged in parallel is set and the gasket assembly is filled, vacuum powder calcination and oscillation pressure sintering is carried out, and solid solution treatment is combined with and aging treatment, forming an integrated multi-stage disc shaft structure.

Benefits of technology

It reduces waste of raw materials, shortens processing cycles, improves processing accuracy and performance stability, reduces preparation costs, and avoids cracking problems of special-shaped parts during the molding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788967B_ABST
    Figure CN118788967B_ABST
Patent Text Reader

Abstract

The integrated forming method of the multi-stage disc-shaft structure described in the present invention comprises the following steps: loading raw material powder into a ceramic sleeve, the ceramic sleeve is provided with a parallel multi-layer annular groove structure, the annular groove structure is filled with a gasket assembly, and the gasket assembly is filled in the annular groove to form a cylindrical structure with the ceramic sleeve; placing the cylindrical structure in a matching sintering mold, the top and bottom of the sintering mold have piston-type pressure heads; placing the sintering mold in a vacuum powder calcining device for calcining treatment; continuing to carry out solid solution treatment and aging treatment in the vacuum powder forging equipment, and then cooling and taking out of the furnace to obtain an integrated multi-stage disc-shaft structure. The present invention has a small amount of material removal when processing the multi-stage disc-shaft structure, avoids the waste of raw materials, has a short processing cycle, and has low cost, and solves the problem that the special-shaped parts are prone to uneven force during the molding process, resulting in cracking and poor mechanical properties, and the performance is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of disk-shaft manufacturing, and in particular to a method for integrated molding of a multi-stage disk-shaft structure. Background Art

[0002] By reducing the number of parts, small and medium-sized aircraft engines can effectively reduce engine weight and manufacturing costs. As the most heavily loaded engine components, the compressor and turbine disk-shaft systems are often critical for reliable engine operation. Existing compressor and turbine disks typically have separate disk-shaft structures, connected by gears or flanges. This results in numerous and expensive components, and reliability needs to be improved urgently. In recent years, during the development of advanced small and medium-sized aircraft engines, researchers have discovered that combining the multi-stage compressor and turbine disk-shaft systems into a single component can effectively reduce the number of parts, improve lifespan, and enhance reliability. However, currently, these components are typically manufactured by machining from rods with sufficient diameter tolerances. This method has the following disadvantages: excessive material removal between the disks during rod machining results in significant waste of raw material. This excessive material removal also prolongs the processing time, exponentially increasing the production cycle. Furthermore, improper control of the material removal process can lead to unstable processing accuracy, impacting product performance, and thus urgently needs improvement. Summary of the Invention

[0003] The technical problem solved by the present invention is to provide a method for integrated molding of a multi-stage disc-shaft structure, so as to solve the technical problems in the prior art of large material removal, long processing time and unguaranteed processing accuracy in the preparation process of the multi-stage disc-shaft structure.

[0004] The technical problem solved by the present invention is achieved by adopting the following technical solutions:

[0005] A method for integrally forming a multi-stage disk-shaft structure comprises the following steps:

[0006] (1) The raw material powder is loaded into a ceramic sleeve, which is provided with a multi-layer annular groove structure arranged in parallel, and a gasket assembly is filled in the annular groove structure. After the gasket assembly is filled in the annular groove, it forms a cylindrical structure together with the ceramic sleeve;

[0007] (2) placing the cylindrical structure in a matching sintering mold, wherein the top and bottom of the sintering mold have piston-type pressure heads; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to a median pressure and then applying an oscillating pressure load, wherein the median pressure is 10 to 90 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 to 5 Hz, and the amplitude range is 0 to 10 MPa; the vacuum degree during the sintering process is less than or equal to 1×10 -5 Pa; cooling after sintering is completed;

[0008] (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment, and then the product is cooled and taken out of the furnace to obtain an integrated multi-stage disc-shaft structure.

[0009] Furthermore, in step (1), the raw material powder is a high-temperature alloy powder or a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm.

[0010] Furthermore, in step (1), the material of the ceramic sheath is one or more of Si3N4, ZrO2 or Al2O3, and the thickness of the ceramic sheath is 2-5 mm.

[0011] Furthermore, in step (2), the sintering mold is a hollow cylindrical structure, the sintering mold and the piston-type pressure head are both made of graphite, and the inner diameter of the sintering mold matches the outer diameter of the ceramic sleeve.

[0012] Furthermore, in step (1), the gasket assembly includes a circular gasket, which is composed of at least two independently arranged gasket blocks, and the upper and lower surfaces of the two gasket blocks are both provided with protruding sub-gasket blocks, and the gasket assembly fully fills the annular groove structure. Preferably, the gasket material is one of graphite, Si3N4, ZrO2 and Al2O3 bulk materials.

[0013] Furthermore, in step (2), the sintering temperature is 1100~1300℃, and the sintering time is 1~3h; the heating rate during the sintering process is 5~100℃ / min; after the sintering is completed, forced cooling is performed, and the cooling rate of the forced cooling is 5~10℃ / min.

[0014] Furthermore, in step (3), the solution treatment temperature is 1100-1250°C and the time is 2-6 hours; the aging treatment temperature is 600-800°C and the time is 5-15 hours.

[0015] Furthermore, in step (3), the vacuum degree during the solution treatment and aging treatment is less than or equal to 1×10 -5 Pa.

[0016] Furthermore, in step (2) and step (3), cooling adopts a composite forced cooling method of water circulation and argon gas filling.

[0017] Beneficial effects: The multi-stage disk-shaft structure integrated molding method described in the present invention has a small amount of material removal, which avoids the waste of raw materials. Its multiple processes can be completed in vacuum powder forging equipment, and there is no need to frequently change the processing site, which effectively reduces the process links, shortens the processing cycle, and reduces the pollution caused by the transfer process; the unique design of the ceramic sleeve combined with the gasket assembly solves the problem that the special-shaped parts are prone to uneven force during the molding process, resulting in cracking and poor mechanical properties. In the sintering process, vacuum sintering and constant pressure plus oscillating load sintering processes are adopted to effectively replace forging of powder high-temperature alloys with pressure. During the sintering process, the sample is deformed and strengthened, its grain structure is refined, the density is improved, and the sample organization and performance are guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the structure of the ceramic sleeve in the present invention.

[0019] Figure 2 It is a structural schematic diagram of the cross section of the gasket assembly in the present invention.

[0020] Figure 3 It is a structural schematic diagram of the sintering mold in the present invention.

[0021] Among them: 1. Ceramic sleeve; 2. Annular groove; 3. Gasket assembly; 4. Pad; 5. Sub-pad; 6. Die body; 7. Sintering cavity; 8. Piston pressure head. DETAILED DESCRIPTION

[0022] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is further described below with reference to specific embodiments.

[0023] The ceramic sleeve 1 used in each embodiment of the present invention is as follows Figure 1 and Figure 3 As shown, the ceramic sleeve 1 is provided with parallel multi-layer annular groove 2 structures, and the annular groove 2 structures are filled with gasket components 3; the gasket components used are as shown in FIG. Figure 2 and Figure 3 As shown, the gasket assembly 3 includes a circular gasket, which is composed of at least two independently arranged gasket blocks 4. The upper and lower surfaces of the two gasket blocks 4 are both provided with protruding sub-gasket blocks 5. The gasket assembly 3 fully fills the annular groove 2 structure.

[0024] Sintering mold Figure 3 As shown, the mold body 6 comprises a cylindrical structure with a sintering cavity 7. Piston rams 8 are located at the top and bottom of the sintering cavity 7. Both the mold body 6 and the piston rams 8 are made of graphite. A ceramic can 1 is placed within the sintering cavity 7, and the inner diameter of the sintering cavity 7 matches the outer diameter of the ceramic can 1.

[0025] Example 1

[0026] The method for integrally forming a multi-stage disk-shaft structure described in this embodiment includes the following steps:

[0027] (1) Filling a ceramic sheath with raw material powder, wherein the raw material powder is titanium alloy powder, and the raw material powder is a spherical structure with a diameter dispersed between 50 and 250 μm; wherein the material of the ceramic sheath is Si3N4, and the thickness of the ceramic sheath is 5 mm. The ceramic sheath is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket assemblies, and after the gasket assemblies are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sheath;

[0028] (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 30 MPa, the oscillation frequency range of the oscillating pressure load is 0.6 Hz, and the amplitude range is 5 MPa; maintaining the vacuum degree of 1×10 -5 Pa; the heating rate during the sintering process is 50℃ / min, and the temperature is raised from room temperature to 1100℃ and then sintered for 3h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 8℃ / min;

[0029] (3) Continue to carry out solid solution treatment and aging treatment in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5 Pa; the solution treatment temperature is 1100℃ and the time is 6h; the aging treatment temperature is 800℃ and the time is 5h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 8℃ / min; after taking out of the furnace, an integrated multi-stage disk-shaft structure is obtained.

[0030] Example 2

[0031] The method for integrally forming a multi-stage disk-shaft structure described in this embodiment includes the following steps:

[0032] (1) Filling a ceramic sheath with raw material powder, wherein the raw material powder is titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm; wherein the material of the ceramic sheath is Si3N4, and the thickness of the ceramic sheath is 4 mm. The ceramic sheath is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket assemblies, and after the gasket assemblies are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sheath;

[0033] (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 40 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 Hz, and the amplitude range is 10 MPa; maintaining the vacuum degree of 1×10 -5 Pa; the heating rate during the sintering process is 35℃ / min, and the temperature is raised from room temperature to 1200℃ and then sintered for 2h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 10℃ / min;

[0034] (3) Continue to carry out solid solution treatment and aging treatment in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5 Pa; the solution treatment temperature is 1200℃ and the time is 4h; the aging treatment temperature is 650℃ and the time is 6h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 10℃ / min; after taking out of the furnace, an integrated multi-stage disk-shaft structure is obtained.

[0035] Example 3

[0036] The method for integrally forming a multi-stage disk-shaft structure described in this embodiment includes the following steps:

[0037] (1) Filling a ceramic sheath with raw material powder, wherein the raw material powder is titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm; wherein the material of the ceramic sheath is Si3N4, and the thickness of the ceramic sheath is 4 mm. The ceramic sheath is provided with parallel multi-layer annular groove structures, and the annular groove structures are filled with gasket assemblies, and after the gasket assemblies are filled in the annular grooves, they form a solid cylindrical structure with the ceramic sheath;

[0038] (2) placing the cylindrical structure in a matching sintering mold; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to the median pressure and then applying an oscillating pressure load. In this embodiment, the median pressure is 50 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 Hz, and the amplitude range is 4 MPa; maintaining the vacuum degree of 1×10 -5 Pa; the heating rate during the sintering process is 60℃ / min, and the temperature is raised from room temperature to 1300℃ and then sintered for 1h; forced cooling is performed after sintering; the forced cooling adopts a composite cooling method of water circulation and argon filling; the cooling rate of forced cooling is 6℃ / min;

[0039] (3) Continue to carry out solid solution treatment and aging treatment in the vacuum powder forging equipment. The vacuum degree is maintained at 1×10 -5 Pa; the solution treatment temperature is 1250℃ and the time is 2h; the aging treatment temperature is 600℃ and the time is 15h; then it is forced cooled and taken out of the furnace, and the forced cooling adopts a composite cooling method of water circulation and argon filling; the forced cooling cooling rate is 6℃ / min; after taking out of the furnace, an integrated multi-stage disk-shaft structure is obtained.

[0040] Comparative Example 1

[0041] The difference between this comparative example and Example 1 is that in step (2), an oscillating pressure load is not used, but only a constant pressure of 30 MPa is used, and the rest are the same.

[0042] Comparative Example 2

[0043] The difference between this comparative example and comparative example 1 is that in step (2), the vacuum degree is greater than 1×10 -5 Pa, the rest are the same.

[0044] Comparative Example 3

[0045] In this comparative example, the diameter of the raw material powder is dispersed in the range of 300-400 μm, and the rest is the same as in Example 1.

[0046] Comparative Example 4

[0047] In this comparative example, the multi-stage disc-shaft structure is processed by conventional forging cylindrical blank removal processing.

[0048] The multi-stage disk-shaft structures prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were tested and compared, and the structures are shown in Table 1.

[0049] Among them: room temperature tensile test adopts the room temperature test method for tensile test of metal materials recorded in GB / T 228-2010; high temperature tensile test adopts the high temperature tensile test method for metal materials recorded in GB / T 4338-2006; fatigue test adopts the axial constant amplitude low cycle fatigue test method for metal materials recorded in GB / T15248-2008; grain size adopts the metal average grain size determination method recorded in GB / T 6394-2017.

[0050] Table 1

[0051]

[0052] As shown in Table 1, the technical solution of the present invention is compared with the traditional method described in Reference Example 4, and the preparation cycle is shortened by more than 50%, and its raw material utilization rate is as high as 90%, which is far superior to 30% of the traditional method, greatly reducing the preparation cost. There is no obvious difference in grain size, density and mechanical properties between the products prepared by the traditional method and the products prepared by the traditional method. However, in actual operation, among the multiple products produced in the same batch, the yield rate of the method described in the present invention is significantly greater than that of the products prepared by the traditional method, without cracking, and the processing accuracy and performance are more stable. As shown in Reference Examples 1 to 3, the technical solution of the present invention is the result of the combined cooperation of processing steps and parameter control. When the processing steps or parameter control are improper, the effect is unsatisfactory.

[0053] The basic principles, main features, and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the foregoing embodiments. The foregoing embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for integrated molding of a multi-stage disk-shaft structure, characterized in that: The steps include: (1) The raw material powder is loaded into a ceramic sleeve, the ceramic sleeve is provided with a multi-layer annular groove structure arranged in parallel, the annular groove structure is filled with a gasket assembly, and the gasket assembly is filled in the annular groove to form a cylindrical structure with the ceramic sleeve; (2) placing the cylindrical structure in a matching sintering mold, wherein the top and bottom of the sintering mold have piston-type pressure heads; placing the sintering mold in a vacuum powder calcining device for calcining; increasing the pressure applied by the piston-type pressure head to a median pressure and then applying an oscillating pressure load, wherein the median pressure is 10 to 90 MPa, the oscillation frequency range of the oscillating pressure load is 0.5 to 5 Hz, and the amplitude range is 0 to 10 MPa; the vacuum degree during the sintering process is less than or equal to 1×10 -5 Pa; cooling after sintering is completed; (3) Solution treatment and aging treatment are continued in the vacuum powder forging equipment, and then the product is cooled and taken out of the furnace to obtain an integrated multi-stage disc-shaft structure.

2. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (1), the raw material powder is a high temperature alloy powder or a titanium alloy powder, and the raw material powder is a spherical structure with a diameter of 50 to 250 μm.

3. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (1), the material of the ceramic sheath is one or more of Si3N4, ZrO2 or Al2O3, and the thickness of the ceramic sheath is 2-5 mm.

4. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2), the sintering mold is a hollow cylindrical structure, the sintering mold and the piston-type pressure head are both made of graphite, and the inner diameter of the sintering mold matches the outer diameter of the ceramic sleeve.

5. The method for integrated molding of a multi-stage disk-shaft structure according to claim 4, characterized in that: In step (1), the gasket assembly includes a circular gasket, which is composed of at least two independently arranged gasket blocks, and the upper and lower surfaces of the two gasket blocks are both provided with protruding sub-gasket blocks, and the gasket assembly fully fills the annular groove structure; wherein the gasket material is one of graphite, Si3N4, ZrO2 and Al2O3 block materials.

6. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2), the sintering temperature is 1100°C~1300°C, and the sintering time is 1~3h; the heating rate during the sintering process is 5~100°C / min; after the sintering is completed, forced cooling is performed, and the cooling rate of the forced cooling is 5~10°C / min.

7. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (3), the solution treatment temperature is 1100-1250°C and the time is 2-6 hours; the aging treatment temperature is 600-800°C and the time is 5-15 hours.

8. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (3), the vacuum degree during the solution treatment and aging treatment is less than or equal to 1×10 -5 Pa.

9. The method for integrated molding of a multi-stage disk-shaft structure according to claim 1, characterized in that: In step (2) and step (3), cooling adopts a composite forced cooling method of water circulation and argon gas filling.