Phospholipid-encapsulated gold nanoparticle array as well as preparation method and application thereof
The development of phospholipid-encapsulated gold nanoparticle arrays through combinatorial chemical methods solves the problem of unclear targeted drug delivery and cellular uptake mechanisms of liposome drugs, achieves targeted drug delivery and improves immunity, and provides a targeted carrier. and diagnostic applications.
Patent Information
- Application Number
- CN202410764432.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
AI Technical Summary
Existing liposome drugs are difficult to meet the needs of precise drug delivery in terms of targeted drug delivery, controlled drug release and organ cell selection, and the targeting and cellular uptake mechanism of a single phospholipid in vivo is not yet clear.
A combinatorial chemical approach was used to develop phospholipid-encapsulated gold nanoparticle arrays. 12 phospholipids with different hydrophilic head groups and hydrophobic chain lengths were combined with gold nanoparticles, and dual quantitative technologies of fluorescent dyes and ICP-MS were used to achieve more accurate targets. Study on the mechanism of tropism and cellular uptake.
It enables accurate exploration of targeted drug delivery and cellular uptake mechanisms in organisms, improves immunity and the number of immune cells, and provides targeted carriers for drug delivery and disease diagnosis.
Smart Images

Figure CN118788974A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of development and application modification of combinatorial chemical nanomaterial library, and specifically relates to a phospholipid-encapsulated gold nanoparticle array and a preparation method and application thereof. Background Art
[0002] Liposomes are composed of phospholipids / phospholipid-like substances. They are bilayer microvesicles that simulate the structure of biological membranes, with a hydrophilic outer layer and a hydrophobic inner layer. In recent years, liposomes have been widely used in drug encapsulation and delivery to achieve long-term drug circulation in the body, improve targeting effects, and control drug release. Compared with non-liposomal encapsulated drugs, liposomal drug delivery can effectively improve the utilization efficiency and stability of drugs.
[0003] Liposomes are constructed with phospholipid molecules as carrier materials, have good biocompatibility, and can be naturally degraded in the body. Liposomes use a double-layer membrane structure to protect the internal drugs from degradation by the body to improve drug utilization. Its main technology can achieve specific recognition of organs and tissues to achieve targeted drug delivery by changing the proportion of components. At present, studies have shown that modifying the surface of liposomes and changing the type / proportion of phospholipids can regulate the targeted distribution of liposomes in the body. However, as a drug prescription, the targeting effect and cell uptake mechanism regulation of different phospholipids in liposomes have not yet been elucidated. Therefore, it is urgent to develop a combinatorial chemical nanomaterial library that can be used to explore the targeting and uptake mechanisms of liposome prescriptions with different phospholipid compositions.
[0004] At present, although existing liposome drugs can achieve a preliminary long circulation time and passively enhance organ targeting in vivo, their targeted drug delivery, controlled drug release and organ cell selection still cannot meet the needs of precise drug delivery. In particular, it is difficult to clarify the effects and mechanisms of targeting and uptake of a single phospholipid in a prescription in vivo / intracellular. The present invention uses a variety of single phospholipids with different physicochemical properties during preparation, and by adding fluorescent dyes for tracing, it can achieve fluorescence localization in cells and organ tissues of organisms, explore the physicochemical properties of a certain phospholipid on organ / cell targeting, and the role of uptake, while the combinatorial chemical nanomaterial library uses gold nanoparticles as the core, and by encapsulating a phospholipid molecular layer doped with fluorescent dyes, a material library that can be used for dual quantitative inductively coupled plasma mass spectrometry (ICP-MS) and fluorescence can be successfully developed, which can more accurately quantify the material distribution of phospholipid layers in different organs and cells.
[0005] According to the design concept of combinatorial chemistry, the present invention provides 12 kinds of phospholipids with different hydrophilic head groups and hydrophobic chain lengths. The biological activity experiment proves that at the dosage used in the present invention, neither mice nor cells show toxic effects. The results of in vivo targeting and in vitro cell uptake confirm that phosphatidylserine with different hydrophobic chain lengths has excellent in vivo immune organ targeting effect (liver and spleen) and the effect of promoting the proliferation of mouse macrophages (RAW264.7), which can be used to increase the number of immune cells in an organism, thereby improving the immunity of the organism.
[0006] This invention utilizes a single phospholipid-encapsulated combinatorial chemically modified gold nanoparticle array and preparation method, which can be widely developed and applied to the efficacy verification of single components in liposome formulations (including targeting and uptake regulation effects), among which phosphatidylserine-coated gold nanoparticles with different hydrophobic chain lengths can be used to enhance immune cell proliferation and enhance the immunity of the organism. Summary of the invention
[0007] Based on the above problems, one of the purposes of the present invention is to provide a study on the interaction between single phospholipid-coated gold core nanoparticles and cells. Based on the fact that traditional liposome fluorescence quantification is prone to fluorescence leakage and other problems, it is difficult to accurately quantify the delivery efficiency. The present invention uses fluorescence and inductively coupled plasma mass spectrometry (ICP-MS) dual quantification, and the results are more accurate.
[0008] In order to explore the mechanism of organ distribution and cellular uptake of key phospholipid components in liposomes with different formulations after administration, another object of the present invention is to provide a gold nanoparticle array that can be used to simulate the exploration of organ targeting and cellular uptake mechanisms in vivo after liposome administration.
[0009] The gold nanoparticle array for simulating the interaction between liposomes and cells of the present invention utilizes combinatorial chemistry methods, uses gold nanoparticles as matrix models, selects 12 kinds of phospholipids with different polar parts (head groups) and different non-polar parts (alkyl chain lengths), and encapsulates the surface of gold nanoparticles. The liposomes encapsulated on the surface of each gold nanoparticle have similar basic structures, but different phospholipid compositions, and the surface properties of liposome-encapsulated gold nanoparticles are jointly affected by the alkyl chain length and head groups of phospholipids. The inner layer of the gold nanoparticles is connected to alkylthiols through gold-sulfur bonds. The phospholipid molecules are connected to alkylthiols through hydrophobic forces. The gold nanoparticle array is composed of 12 kinds of nanoparticles, wherein the nanoparticles are round gold nanoparticles of about 15 nanometers, represented by GNP1-GNP12 respectively.
[0010] To achieve the above object, the present invention provides the following technical solutions.
[0011] One aspect of the present invention provides a method for preparing a phospholipid-encapsulated gold nanoparticle array, the method comprising the following steps:
[0012] S1: adding sodium citrate solution into ultrapure water, heating to 96°C while stirring, then adding chloroauric acid solution and stirring to react, to obtain gold nanoparticles;
[0013] S2: The obtained gold nanoparticles are concentrated by centrifugation and dissolved in an isopropanol solution, and an isopropanol solution of alkylthiol is added, and stirred at room temperature for three days. The obtained solution is then subjected to ultrasound, centrifugal separation, and vacuum drying in sequence to obtain alkylthiol-modified gold nanoparticles;
[0014] S3: dissolving phospholipid molecules in a chloroform / methanol mixed solution to obtain a mixed solution I, dissolving alkylthiol-modified gold nanoparticles in chloroform to obtain a mixed solution II, and mixing the obtained mixed solution I and mixed solution II uniformly and vacuum drying to obtain a solid product;
[0015] The obtained solid product is added into ultrapure water and ultrasonically treated until the solution is clear, the obtained solution is centrifuged and the supernatant is taken to obtain the phospholipid-encapsulated gold nanoparticle array.
[0016] Preferably, in step S1, the sodium citrate aqueous solution, ultrapure water and chloroauric acid solution are added in a volume ratio of 6.125:117.5:2.5, the concentration of the sodium citrate solution is 68 mM, and the concentration of the chloroauric acid solution is 50 mM.
[0017] Preferably, the stirring reaction conditions in step S1 are: rotation speed 600-1000 rpm; time 25 min.
[0018] Preferably, the concentration of alkyl thiol in the isopropanol solution of alkyl thiol in step S2 is 0.01 mmol / mL, the alkyl thiol and the nano-gold particles are added in a mass ratio of 1.2:1, and the alkyl thiol is selected from thiols with a carbon chain length of C8 to C18.
[0019] Preferably, the alkyl mercaptan is selected from at least one of octyl mercaptan, dodecanethiol and octadecyl mercaptan.
[0020] Preferably, the ultrasonic time in step S2 is 2-3 min, and the centrifugal separation conditions are: speed 9000 r / min, time 30 min.
[0021] Preferably, the chemical structural formula of the phospholipid molecule in step S3 is as follows:
[0022]
[0023] Among them, the polar part difference group is marked as R, which are four structures of a, b, c, and d, as shown below:
[0024]
[0025] The length of the alkyl chain in the non-polar part is marked as N, where N is e, f, and g, respectively, as shown below:
[0026]
[0027] The above phospholipid array for encapsulating gold nanoparticles is shown below:
[0028]
[0029] Preferably, in step S3, the phospholipid molecules and the chloroform / methanol mixed solution are added at a material-liquid ratio of 5 mg:1 mL.
[0030] Preferably, in step S3, the alkylthiol-modified gold nanoparticles and chloroform are added at a solid-liquid ratio of 5 mg:1 mL.
[0031] Preferably, the centrifugal conditions in step S3 are: rotation speed 15000 r / min, time 30-60 min.
[0032] Another aspect of the present invention also provides a use of the phospholipid-encapsulated gold nanoparticle array obtained according to the above preparation method in the preparation of a product that promotes the proliferation of immune cells and enhances the immunity of an organism.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention discloses a method for stably fixing phospholipids on the surface of nanoparticles by utilizing the covalent structure of thiol and gold through the hydrophobic interaction between long-chain thiol and phospholipids, which is applicable to almost all phospholipids.
[0035] (2) The gold nanoparticle array of the present invention provides relevant research on the interaction between single phospholipid-coated gold core nanoparticles and cells. Traditional liposome fluorescence quantification is prone to fluorescence leakage and other problems, making it difficult to accurately quantify the delivery efficiency. The dual quantification of fluorescence and ICP-MS adopted in the present invention has more accurate results.
[0036] (3) The gold nanoparticle array prepared by the present invention for simulating the interaction between liposomes and cells is composed of 12 kinds of nanoparticles. Since the surface chemical environments of these nanoparticles are different, they show different effects when interacting with cells. The present invention realizes the uptake efficiency of gold cores inside cells through ICP-MS, and the delivery efficiency of liposomes is quantified by fluorescence imaging and fluorescence intensity, so as to realize the study of the mechanism of action between liposomes and cells. The single phospholipid / dual quantification of the present invention can also guide the design of carriers used in biomedical fields such as targeted drug delivery, biological imaging, disease diagnosis and gene therapy. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a perspective electron microscope photo of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention;
[0038] Figure 2 This is a perspective electron microscope photo of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention;
[0039] Figure 3 Dynamic light scattering particle size analysis of gold nanoparticle arrays No. 1-12 obtained according to Example 2 of the present invention;
[0040] Figure 4 Surface Zeta potential analysis of gold nanoparticle arrays No. 1-12 obtained according to Example 2 of the present invention;
[0041] Figure 5 Raman spectroscopy analysis of gold nanoparticle arrays No. 3, 7, 9-12 obtained according to Example 2 of the present invention;
[0042] Figure 6 This is an SDS-Page image of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention after incubation with 10% FBS;
[0043] Figure 7 This is a quantitative analysis of protein adsorption after incubation of gold nanoparticle arrays No. 2, 6, 9-12 obtained in Example 2 of the present invention with 10% FBS;
[0044] Figure 8 This is the ICP-MS quantitative analysis of the uptake effect of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the human liver cancer cell line HepG2;
[0045] Fig. 9 The flow cytometry fluorescence intensity analysis of the uptake effect of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the human liver cancer cell line HepG2;
[0046] Fig.10This is a fluorescence photograph of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention taken in the human liver cancer cell line HepG2;
[0047] Fig.11 This is the quantitative analysis of the uptake of gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the mouse macrophage cell line Raw264.7 by ICP-MS;
[0048] Fig.12 This is a fluorescence photograph of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention taken up in the mouse macrophage cell line Raw264.7;
[0049] Fig.13 Analysis of the endocytosis mechanism of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the human liver cancer cell line HepG2;
[0050] Fig.14 Analysis of the endocytosis mechanism of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the mouse macrophage cell line Raw264.7;
[0051] Fig.15 Cell viability analysis of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention in the human liver cancer cell line HepG2;
[0052] Fig.16 Cell viability analysis of gold nanoparticle arrays No. 1-12 obtained according to Example 2 of the present invention in the mouse macrophage cell line Raw264.7;
[0053] Fig.17 Analysis of the proliferation effect of the gold nanoparticle array No. 10 obtained according to Example 2 of the present invention on the mouse macrophage cell line Raw264.7;
[0054] Fig.18 Analysis of the immune effects of the No. 2, 6, 9-12 gold nanoparticle arrays obtained in Example 2 of the present invention on the secretion of inflammatory factors in the mouse macrophage cell line Raw264.7;
[0055] Fig.19 This is the ICP-MS quantitative analysis of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in different organs of ICR mice;
[0056] Fig. 20 This is a perspective electron microscope photograph of the gold nanoparticle array obtained according to Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0057] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0058] Example 1: Optimization of the preparation method of phospholipid-encapsulated gold nanoparticle arrays
[0059] The present invention has obtained the best preparation method of phospholipid-encapsulated gold nanoparticle array through multiple tests and optimization of various condition parameters in the preparation method, which specifically includes the following steps:
[0060] (1) Preparation of gold nanoparticles modified with alkylthiol: 6.125 mL of 68 mM sodium citrate aqueous solution was added to 117.5 mL of ultrapure water, and the resulting mixture was heated to 96°C with stirring at a speed of 800 rpm, and then 2.5 mL of 50 mM chloroauric acid solution was added and stirred for 25 min to obtain a gold nanoparticle solution. The resulting gold nanoparticle solution was centrifuged and concentrated, dissolved in 60 mL of isopropanol solution, and 10 mL of an isopropanol solution of 0.1 mmol of octadecyl mercaptan was added, and stirred at room temperature for three days to obtain an octadecyl mercaptan-modified gold nanoparticle solution. The resulting octadecyl mercaptan-modified gold nanoparticle solution was ultrasonicated for 5 minutes, separated and purified using a centrifuge tube, with a speed of 9000 r / min and a centrifugation time of 3 min, and then placed in a vacuum drying oven overnight to remove the organic solvent.
[0061] (2) Preparation of gold nanoparticle array: 5 mg of phospholipid molecules were dissolved in 1 mL of chloroform / methanol (9:1) mixed solution to obtain mixed solution I; then 5 mg of octadecylthiol-modified gold nanoparticles were dissolved in 1 mL of chloroform to obtain mixed solution II, and then mixed solution I and mixed solution II were mixed and dried in a vacuum drying oven to remove all organic solvents. 2 mL of ultrapure water was added, and ultrasonication was performed above the phase transition temperature of the phospholipid molecules until the aqueous solution was clarified. The obtained gold nanoparticle solution was purified by centrifugation in a centrifuge tube at a speed of 15000 r / min, and the supernatant was taken to obtain the phospholipid-encapsulated gold nanoparticle array.
[0062] Example 2: Preparation of phospholipid-encapsulated gold nanoparticle arrays
[0063] The preparation method provided in Example 1 was used, and phospholipid-encapsulated gold nanoparticle arrays were prepared according to the 12 phospholipid molecules provided in Table 1 below, corresponding to GNP1 to GNP12, respectively. According to the different types of phospholipid molecules, a total of 12 phospholipid-encapsulated gold nanoparticle array materials were obtained, numbered 1 to 12, respectively.
[0064] Table 1 Details of the types of phospholipid molecules
[0065]
[0066] Application Example 1: Physicochemical Property Detection of Phospholipid-Encapsulated Gold Nanoparticle Arrays
[0067] 1. Morphology and surface properties analysis of gold nanoparticle arrays
[0068] The gold nanoparticle array material solutions No. 1 to 12 obtained in Example 2 were respectively placed in an ultrasonic crusher for 5 minutes, 50 μL of the solution was taken out and added to a clean small tube, diluted to 1 mL with ultrapure water, and ultrasonicated again for 5 minutes to disperse the material evenly. 8 μL of the material was carefully dropped onto a copper grid with a 10 μL pipette and negatively stained with phosphotungstic acid, and dried under an infrared lamp for at least 30 minutes. The morphology of the gold nanoparticles was observed using a Tecnai G2 20 transmission electron microscope at 120 KV. Figure 1 This is a perspective electron microscope photograph of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention. The figure mainly shows that the organic layer thickness of phospholipids with different chain lengths is different. The numbers 1-12 in the figure correspond to the gold nanoparticle array materials No. 1-12 obtained in Example 2, and their corresponding organic layer thicknesses are 2.5nm, 3.3nm, 3.3nm, 3.4nm, 4.3nm, 4.5nm, 4.5nm, 4.3nm, 6.3nm, 5.5nm, 6.2nm, and 6.4nm, respectively; it can be seen that the organic layer thickness range of the numbered 1-4 is 2.5-4nm, the organic layer thickness range of the numbered 5-8 is 4-5.5nm, and the organic layer thickness range of the numbered 9-12 is 5.5-7nm, that is, the organic layer thickness is related to the chain length of the phospholipid molecules. Figure 1 As shown, the obtained gold nanoparticles are approximately round, with an average particle size of 14.5 nm, good dispersion and uniform particle size. Figure 2 The following is a perspective electron microscope photo of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention. Figure 2 It can be seen that the particle sizes of the 12 nanoparticles obtained in Example 2 are all between 13-15 nm, and the obtained nanoparticles are uniformly coated and have good monodispersity.
[0069] 2. Dynamic light scattering particle size analysis of gold nanoparticle arrays
[0070] The gold nanoparticle array material solutions No. 1-12 obtained in Example 2 were diluted with ultrapure water to a gold nanoparticle solution with a concentration of 5 μg / mL, placed in an ultrasonic crusher for 5 minutes, and about 1 mL of the sample solution to be tested was taken using a pipette and injected into the sample cell of the HORIBA Nano particle analyzer. The particle size distribution of the gold nanoparticles to be tested in high-purity water was measured by the dynamic light scattering (DLS) method. The measurement conditions were 25 times, and the average value was taken for three parallel measurements. Figure 3 The dynamic light scattering particle size analysis of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention, wherein (a) represents the dynamic light scattering particle size of the gold nanoparticle array No. 1-12; (b) represents the dynamic light scattering particle size bar graph of the gold nanoparticle array No. 1-12, in which: PA represents phosphatidic acid, PC represents phosphatidylcholine, PS represents phosphatidylserine, PE represents phosphatidylethanolamine, 18PL represents a phospholipid with a hydrophobic chain containing 18 carbons, 12PL represents a phospholipid with a hydrophobic chain containing 12 carbons, and 6PL represents a phospholipid with a hydrophobic chain containing 6 carbons. Figure 3 As shown in (a) and (b), the dynamic hydrated particle sizes of the 12 gold nanoparticle arrays are approximately 40-100 nm, where the hydrated particle size is related to the chain length of the phospholipid molecules: the longer the chain length of the phospholipid molecules, the larger the hydrated particle size.
[0071] 3. Analysis of surface Zeta potential of gold nanoparticle arrays
[0072] The gold nanoparticle array material solutions No. 1-12 obtained in Example 2 were diluted with ultrapure water to a gold nanoparticle solution with a concentration of 5 μg / mL, placed in an ultrasonic crusher for 5 minutes, and the gold nanoparticle array material solution to be tested was drawn using a 1 mL syringe without a needle, and injected into the Zeta potential sample cell of the nanoparticle size analyzer (HORIBA). The injection process should be as slow and careful as possible to avoid bubbles in the sample cell that affect the measurement. The Zeta potential of the gold nanoparticles was detected in turn at 25°C, and the average value was taken for three parallel tests. Figure 4 This is the surface Zeta potential analysis of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention. Figure 4 As shown, the surface of the gold nanoparticle array is negatively charged, with a Zeta potential of about -74.2 to -34.6 mV, and good stability in water.
[0073] 4. Raman spectroscopy analysis of gold nanoparticle arrays
[0074] The gold nanoparticle array material solutions No. 3, 7, 9-12 obtained in Example 2 were diluted with ultrapure water to 50 μg / mL gold nanoparticle solutions, and 10 μL was carefully transferred to the slide wrapped in tin foil with a 10 μL pipette. The dropping process should be as slow and careful as possible to avoid wrinkles in the tin foil that affect the measurement. The slide with the sample was placed in a vacuum drying oven to remove all moisture. The Raman spectrum of the gold nanoparticles was scanned using a micro-Raman spectrometer (Renishaw) with a 785nm laser at a laser intensity of 0.5%. Figure 5 This is the Raman spectrum analysis of the gold nanoparticle arrays No. 3, 7, 9-12 obtained according to Example 2 of the present invention. Figure 5 As shown, by comparing the Raman spectra of the gold nanoparticle arrays No. 3, 7, 9-12 of the present invention with the phospholipid standards, it was determined that the phospholipid ligands had been coated on the gold nanoparticles.
[0075] Application Example 2: Analysis of Surface Adsorbed Proteins on Gold Nanoparticle Arrays
[0076] The gold nanoparticle array material to be tested was diluted with ultrapure water to a 200 μg / mL gold nanoparticle solution, and 100 μL of the gold nanoparticle solution was mixed with 400 μL of 12.5% FBS solution to make the final concentration of FBS 10%. The mixed solution was incubated at 37°C for 2 hours to obtain a protein-coated gold nanoparticle array. Subsequently, SDS-Page was performed at 120V to separate the proteins.
[0077] Figure 6 This is an SDS-Page diagram of the gold nanoparticle arrays No. 1-12 obtained in Example 2 of the present invention after incubation with 10% FBS. In the diagram, 18PA represents the gold nanoparticle array No. 9 in Example 2, 12PA represents the gold nanoparticle array No. 5 in Example 2, 6PA represents the gold nanoparticle array No. 1 in Example 2, 18PS represents the gold nanoparticle array No. 10 in Example 2, 12PS A represents the gold nanoparticle array No. 6 in Example 2, 6PS represents the gold nanoparticle array No. 2 in Example 2, 18PC represents the gold nanoparticle array No. 11 in Example 2, 12PC represents the gold nanoparticle array No. 7 in Example 2, 6PC represents the gold nanoparticle array No. 3 in Example 2, 18PE represents the gold nanoparticle array No. 12 in Example 2, 12PE represents the gold nanoparticle array No. 8 in Example 2, 6PE represents the gold nanoparticle array No. 4 in Example 2, and the following all represent the same meaning. Figure 6 As shown, the gold nanoparticle arrays No. 1-12 of the present invention were incubated with 10% FBS, and the differences in surface adsorbed proteins were compared by SDS-Page, indicating that there were differences in adsorbed proteins, which was the main reason for the cell effect.
[0078] Figure 7 The results of measuring the total amount of protein adsorbed on the surface of different nanoparticles by BCA method after incubation of gold nanoparticle arrays No. 2, 6, 9-12 with 10% in Example 2 of the present invention. Figure 7 As shown, the gold nanoparticle arrays No. 2, 6, 9-12 of the present invention were incubated with 10% FBS, and the amount of protein adsorbed on the surface decreased with the increase of the phospholipid chain length, and the amount of protein adsorbed on the surface of the nanoparticles coated with anionic phospholipids was less than the amount of protein adsorbed on the surface of the nanoparticles coated with zwitterionic phospholipids.
[0079] Application Example 3: Analysis of the Uptake Effect of Gold Nanoparticle Arrays in HepG2 and Raw264.7 Cells
[0080] The gold nanoparticle array material solution to be tested was diluted with ultrapure water to a 50 μg / mL gold nanoparticle solution, diluted with DMEM medium to a 2 μg / mL solution, and added to a 24-well plate inoculated with 100,000 HepG2 cells / well or 200,000 Raw264.7 cells / well 24 hours in advance. The cells were collected after incubation in DMEM medium containing 10% FBS or serum-free medium for 4 hours. The samples were washed three times with PBS solution and digested with aqua regia, and quantitatively analyzed using Agilent 8900ICP-MS / MS. The samples were washed three times with PBS solution and resuspended with PBS solution, and fluorescence analysis was performed using the Thermo Attune NxT flow cytometer. The samples were washed three times with PBS solution and fixed with 4% paraformaldehyde, and fluorescence photography was performed using the Thermo EVOSM5000 fluorescence imaging system.
[0081] The gold nanoparticle array material solution to be tested was diluted with ultrapure water to a 50 μg / mL gold nanoparticle solution, diluted with DMEM medium to a 2 μg / mL solution, and added to a 24-well plate inoculated with 100,000 Raw264.7 cells / well 24 hours in advance. The cells were collected after incubation in DMEM medium containing 10% FBS or serum-free medium for 4 hours. The sample was washed three times with PBS solution and digested with aqua regia, and quantitatively analyzed using Agilent 8900ICP-MS / MS. The sample was washed three times with PBS solution and resuspended with PBS solution, and fluorescence analysis was performed using the Thermo Attune NxT flow cytometer. The sample was washed three times with PBS solution and fixed with 4% paraformaldehyde, and fluorescence photography was performed using the Thermo EVOS M5000 fluorescence imaging system.
[0082] Figure 8 This is the ICP-MS quantitative analysis of the uptake effect of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in the human liver cancer cell line HepG2. Fig. 9 For HepG2 cell line flow cytometry fluorescence intensity analysis, Fig.10 Take fluorescent photos of HepG2 cell line. Fig.11 ICP-MS quantitative results analysis for Raw264.7 cell line uptake, Fig.12 Fluorescence images were taken for the Raw264.7 cell line.
[0083] like Figure 8-12 As shown in the figure, the gold nanoparticle array of the present invention was analyzed for cellular uptake effect, incubated in two different cell lines HepG2 and Raw264.7, and the uptake results of HepG2 cells and Raw264.7 cells were analyzed by ICP-MS and flow cytometry. The gold nanoparticle array showed different uptake effects, and the uptake showed a significant correlation with the phospholipid chain length. As the chain length decreased, the uptake decreased. Secondly, phospholipids with different head groups of the same chain length are taken up differently in different cell lines, which can explore the specific targeting of phospholipids.
[0084] Application Example 4: Analysis of the Cellular Internalization Mechanism of Gold Nanoparticle Arrays
[0085] The gold nanoparticle array material solution to be tested was diluted with ultrapure water to a 50 μg / mL gold nanoparticle solution, and diluted with DMEM medium to a 2 μg / mL solution, and added to a 24-well plate inoculated with 100,000 HepG2 cells / well or 200,000 Raw264.7 cells / well 24 hours in advance. 50 μM chlorpromazine, 10 μM nystatin, and 10 mM hydroxypropyl-β-cyclodextrin were pre-incubated with the cells for 1 hour to explore the effects of clathrin, caveolin, and macropinocytosis. The cells were cultured at 4 ° C for 1 hour to explore the role of energy. After that, the cells were collected after incubation with the material for 4 hours in DMEM medium containing 10% FBS or serum-free medium. The samples were washed three times with PBS solution and resuspended in PBS solution, and fluorescence analysis was performed using a Thermo Attune NxT flow cytometer. Fig.13 , 14 This is an analysis of the endocytosis mechanism of the gold nanoparticle array No. 1-12 obtained in Example 2 of the present invention in two cell lines. Fig.13 HepG2 cell line, Fig.14 Raw264.7. In the figure, 18PA-coated nanoparticles enter the HepG2 cell line through caveolin-mediated endocytosis, and 18PS / 18PC / 18PE / 12PE enter the HepG2 cell line through clathrin-mediated endocytosis. All types of phospholipid-coated nanoparticles enter the Raw264.7 cell line through clathrin-mediated endocytosis.
[0086] Application Example 5: Cell Viability Analysis Using Gold Nanoparticle Arrays
[0087] The gold nanoparticle array material solution to be tested was diluted with ultrapure water to a 50 μg / mL gold nanoparticle solution, and then diluted with DMEM medium to a 2 μg / mL solution, and added to a 96-well plate inoculated with 10,000 HepG2 cells / well or 20,000 Raw264.7 cells / well 24 hours in advance. After culturing at 37°C for 24 hours, the medium was removed, and 100 μL of DMEM medium containing 10% CCK-8 was added, and incubated at 37°C for 1 hour. The absorbance at 450 nm was detected using a Tecan infinite multifunctional microplate reader to calculate cell viability. Fig.15 , 16 The cell viability analysis of the gold nanoparticle array No. 1-12 obtained according to Example 2 of the present invention in two cell lines showed that the 18PS-coated gold nanoparticles showed a significant proliferation-promoting effect on the Raw264.7 cell line. Fig.17 The cell viability analysis of the Raw264.7 cell line exposed to different concentrations of 18PS-coated gold nanoparticles and the same concentration of 18PS phospholipids shows that only when 18PS is coated on the nanoparticles can the proliferation of Raw264.7 be promoted, while simple phospholipids have no such effect.
[0088] Application Example 6: Analysis of the Immune Effects of Gold Nanoparticle Arrays
[0089] The gold nanoparticle array material solution to be tested was diluted to 50 μg / mL of gold nanoparticle solution, and then diluted to 2 μg / mL of solution with DMEM medium, and added to a 12-well plate inoculated with 200,000 Raw264.7 cells / well 24 hours in advance. After culturing at 37°C for 24 hours, the medium was removed and the concentrations of inflammatory factors IL-1β, IL-6 and TNF-α were determined using an enzyme-linked immunosorbent assay kit. The results are shown in Fig.18 . Fig.18 The immunological effect analysis of the gold nanoparticle arrays No. 2, No. 6, and No. 9-12 obtained according to Example 2 of the present invention shows that only when PS phospholipids are coated on the nanoparticles can Raw264.7 be promoted to produce an inflammatory response, while other phospholipids have no such effect.
[0090] Application Example 7: Tissue Distribution Analysis of Gold Nanoparticle Arrays
[0091] The gold nanoparticle array material solution to be tested was diluted with PBS to a 50μg / mL gold nanoparticle solution, and then injected into 3-8 week old ICR mice through the tail vein. After 24 hours, the heart, liver, spleen, lung, kidney, brain, and muscle of the mice were removed. 100mg of tissue was weighed and added with 8mL of freshly prepared aqua regia. After digestion using Anton Paar microwave digestion instrument, the sample was diluted to 10mL after acid removal at 170℃. After the sample was filtered through a 0.45μm membrane, it was quantitatively analyzed using ICP-MS to calculate the gold content in different organs. Fig.19 This is the ICP-MS quantitative analysis of the distribution of gold nanoparticle arrays No. 1-12 obtained according to Example 2 of the present invention in different organs of ICR mice. It can be seen that all nanoparticles are basically enriched in the liver and spleen, and the content of 18PE and 12PA-coated nanoparticles in the lungs is significantly increased.
[0092] Comparative Example 1
[0093] This example is consistent with Example 1, except that this example does not have the step of modifying the nano-gold particles with octadecanethiol, that is:
[0094] 6.125 mL of 68 mM sodium citrate aqueous solution was added to 117.5 mL of ultrapure water, and the resulting mixture was heated to 96° C. with stirring at 800 rpm, and then 2.5 mL of 50 mM chloroauric acid solution was added and stirred for 25 min to obtain a gold nanoparticle solution.
[0095] 5 mg of phospholipid molecules (corresponding to GNP1) were dissolved in 1 mL of chloroform / methanol (9:1) mixed solution, and then 5 mg of gold nanoparticles were dissolved in 1 mL of chloroform. The two solutions were mixed and dried in a vacuum drying oven to remove all organic solvents. 2 mL of ultrapure water was added, and the aqueous solution was clarified by ultrasound at a temperature above the phase transition temperature of the phospholipid molecules. The resulting gold nanoparticle solution was purified by centrifugation in a centrifuge tube at a speed of 15000 r / min to obtain a gold nanoparticle array.
[0096] Fig. 20 FIG. 1 is a perspective electron microscope photograph of the gold nanoparticle array obtained according to Comparative Example 1 of the present invention. Fig. 20 It can be seen that there is no organic layer coating around the gold nanoparticles. This shows that gold nanoparticles that are not modified with octadecylthiol cannot be encapsulated by phospholipids and cannot produce the corresponding cellular uptake effect.
[0097] The matters not described in detail in the present invention are all known technologies to those skilled in the art.
[0098] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified and replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a phospholipid-encapsulated gold nanoparticle array, characterized in that: The method comprises the following steps: S1: adding sodium citrate solution into ultrapure water, heating to 96°C while stirring, then adding chloroauric acid solution and stirring to react, to obtain gold nanoparticles; S2: The obtained gold nanoparticles are concentrated by centrifugation and dissolved in an isopropanol solution, and an isopropanol solution of alkylthiol is added, and stirred at room temperature for three days. The obtained solution is then subjected to ultrasound, centrifugal separation, and vacuum drying in sequence to obtain alkylthiol-modified gold nanoparticles; S3: dissolving phospholipid molecules in a chloroform / methanol mixed solution to obtain a mixed solution I, dissolving alkylthiol-modified gold nanoparticles in chloroform to obtain a mixed solution II, and mixing the obtained mixed solution I and mixed solution II uniformly and vacuum drying to obtain a solid product; The obtained solid product is added into ultrapure water and ultrasonically treated until the solution is clear, the obtained solution is centrifuged and the supernatant is taken to obtain the phospholipid-encapsulated gold nanoparticle array.
2. The preparation method according to claim 1, characterized in that: In step S1, the sodium citrate solution, ultrapure water and chloroauric acid solution are added in a volume ratio of 6.125:117.5:2.5, the concentration of the sodium citrate solution is 68 mM, and the concentration of the chloroauric acid solution is 50 mM.
3. The preparation method according to claim 1, characterized in that: The stirring reaction conditions in step S1 are: rotation speed 600-1000 rpm, time 25 min.
4. The preparation method according to claim 1, characterized in that: The concentration of alkyl thiol in the isopropanol solution of alkyl thiol in step S2 is 0.01 mmol / mL, the alkyl thiol and the nano-gold particles are added in a mass ratio of 1.2:1, and the alkyl thiol is selected from thiols with a carbon chain length of C8 to C18.
5. The preparation method according to claim 1, characterized in that: The ultrasonic time in step S2 is 2-3 minutes, and the centrifugal separation conditions are: speed 9000r / min, time 30 minutes.
6. The preparation method according to claim 1, characterized in that: The general chemical structure formula of the phospholipid molecule in step S3 is as follows: Among them, the polar part difference group is marked as R, which are four structures of a, b, c, and d, as shown below: The length of the alkyl chain in the non-polar part is marked as N, where N is e, f, and g, respectively, as shown below:
7. The preparation method according to claim 1, characterized in that: The phospholipid molecules and the chloroform / methanol mixed solution in step S3 are added at a material-liquid ratio of 5 mg:1 mL.
8. The preparation method according to claim 1, characterized in that: The alkylthiol-modified gold nanoparticles and chloroform described in step S3 are added at a solid-liquid ratio of 5 mg:1 mL.
9. The preparation method according to claim 1, characterized in that: The centrifugal conditions in step S3 are: rotation speed 15000r / min, time 30-60min.
10. Use of the phospholipid-encapsulated gold nanoparticle array obtained according to the preparation method according to any one of claims 1 to 9 in preparing products that promote the proliferation of immune cells and enhance the immunity of an organism.