Method for recycling non-finished aluminum alloy powder

Through inert gas protection and isostatic mold pressing technology, the problems of oxidative combustion and composition instability in the reuse of aluminum alloy powder are solved, achieving infinite recycling and quality assurance of aluminum alloy powder.

CN118788980APending Publication Date: 2024-10-18AVIMETAL POWDER METALLURGY TECH (XUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410835184.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

It is difficult to effectively utilize the idle powder of aluminum alloy powder for 3D printing with the existing technology, and it is easy to cause oxidative combustion and composition instability during the reuse process, affecting product quality.

Method used

A mixer with inert gas protection is used to uniformly mix the aluminum alloy powder, and an isostatic pressing mold is used for multiple times of pressure and pressure holding to form an aluminum alloy rod with high density, and then vacuum air atomization is used to make the powder. Ensure recyclability of powder.

Benefits of technology

It realizes the infinite recycling of aluminum alloy powder, ensures the stability and quality of powder components, reduces 3D printing costs, and avoids the problems of oxidative combustion and unstable components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118788980A_ABST
    Figure CN118788980A_ABST
Patent Text Reader

Abstract

The invention relates to a method for recycling non-finished aluminum alloy powder, and belongs to the technical field of additive manufacturing, the method comprises the following steps: S1, collecting aluminum alloy powder with different granularities, and carrying out homogenization mixing treatment on the aluminum alloy powder by using a mixing machine with inert gas protection; s2, the mixed metal powder is put into an isostatic pressing die, and the loose ratio of the powder in the die is larger than or equal to 55% of the alloy density; s3, after powder filling is completed, an upper plug of a sealing mold is installed, the packaged mold is put into cold isostatic pressing equipment, pressurization and pressure maintaining pressing are conducted, and pressurization and pressure maintaining are conducted for multiple times; s4, after pressing is completed, the pressed bar is taken out; and S5, the qualified pressed bar is re-smelted into an alloy ingot needed by vacuum gas atomization powder making equipment, powder making is conducted again, the oxygen content of the prepared aluminum alloy powder is not obviously increased compared with that of original powder, the smoke generation phenomenon does not exist in the powder making process, and under the condition that the product quality is not affected, the production cost is reduced. And repeated utilization of the non-finished aluminum alloy powder is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of additive manufacturing, and in particular to a method for recycling unfinished aluminum alloy powder. Background Art

[0002] In the process of preparing aluminum alloy powder for 3D printing by vacuum gas atomization, the particle size of the powder produced by VIGA gas atomization powder making is 0-300 micron powder, while the particle size of aluminum alloy products for 3D printing is mostly 15-53 micron or 20-60 micron powder. The remaining particle size powders after classification cannot be used and are idle and accumulated. How to deal with these powders has become a problem. If they can be used as raw materials for secondary smelting and powder making or re-smelted into aluminum alloy ingot raw materials for secondary powder making, it will be the best way to use these powders. However, the characteristics of aluminum alloy powders make it impossible to directly melt aluminum alloy powders.

[0003] Aluminum alloy powder has a light density and a large specific surface area. When VIGA vacuum powder making equipment is used for direct melting, the aluminum alloy powder is extracted from the crucible during vacuuming and directly sucked into the vacuum system along with the air in the vacuum equipment, resulting in abnormal powder accumulation in the vacuum pump group. If the powder is used as raw material and melted into VIGA powder making alloy ingots using non-vacuum equipment, during the melting process, the powder oxidizes and burns during the melting and heating process, and there is even a slight explosion phenomenon when the powder is added for the second time, so the test is stopped. Considering its powder characteristics, it is decided to press the powder into a high-density alloy block before using it for powder making or melting it into alloy ingots.

[0004] First, we considered using a four-beam four-column mechanical hydraulic press for pressing, but we encountered two problems during the pressing process of the hydraulic press: first, demolding was difficult, the mold was damaged quickly, and the pressing efficiency was low; second, the density of the pressed product was low (<96%) and the density was uneven, and the upper and lower corners were easy to loosen and fall off.

[0005] The pressed powder was tried to be directly melted and powdered using VIGA vacuum powder making equipment. However, the gaps in the powder pressed products still contained air which was difficult to extract. The crucible smoked rapidly during melting (the lower the density of the pressed product, the more smoke was generated), making it impossible to observe the melting conditions in the vacuum equipment. The mechanical hydraulic press pressed products had a high air content due to density issues. During melting, some elements such as aluminum and magnesium were easily oxidized, which would lead to unstable composition of the alloy products.

[0006] Chinese patent CN110125384B discloses a method for preparing metal powder for 3D printing using non-target particle size metal powder. However, the following problems exist in the whole process: (1) Adding other non-metallic substances will increase the inclusion of the alloy and reduce the purity of the alloy and the re-atomized powder; (2) Even if the powder compact is pressed into shape, there will still be air in the gaps between the powders in the compact that cannot be completely discharged during the pressing process. The lower the density of the compact, the greater the amount of air contained. The direct sintering and atomization powder making process will increase the oxygen content of the alloy and the burn-off amount of the alloy components. In particular, active metals with large active components (such as magnesium, aluminum, titanium and other components) will oxidize under high temperature conditions, affecting the quality of the finished product and making it impossible to recycle; or in the case of recycling, the product quality cannot be guaranteed.

[0007] In summary, there is an urgent need to develop a processing method for the recycling of finished aluminum alloy powder prepared by vacuum atomization, which can achieve the repeated recycling of idle powder while ensuring product quality. Summary of the invention

[0008] The purpose of the present invention is to provide a method for recycling unfinished aluminum alloy powder, which has the characteristics of simple method and low cost, and the recycled aluminum alloy rods can be re-smelted into qualified aluminum alloy ingots for preparing aluminum alloy powder for 3D printing again, thereby realizing the repeated recycling of idle powders such as aluminum alloy powder and coarse powder prepared by vacuum air atomization.

[0009] The present invention solves the technical problem by adopting the following technical solutions.

[0010] The present invention provides a method for recycling unfinished aluminum alloy powder, comprising the following steps:

[0011] Step S1: collecting aluminum alloy powders of different particle sizes, wherein the mass percentage of aluminum alloy powders of 0-20 μm is 17-22%, the mass percentage of aluminum alloy powders of 53-150 μm is 58-68%, and the mass percentage of aluminum alloy powders of 150 μm and above is 15-20%; using a mixer with inert gas protection to homogenize and mix the above aluminum alloy powders;

[0012] Step S2: loading the mixed metal powder into an isostatic pressing mold, wherein the powder bulk ratio in the mold is ≥55% of the alloy density;

[0013] Step S3: After the powder is filled, a plug is installed on the sealing mold, and the mold after encapsulation is placed in a cold isostatic pressing device for pressurization and pressure holding, and the pressurization and pressure holding are performed for multiple times;

[0014] Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out;

[0015] Step S5: The qualified pressed bars are loaded into a resistance furnace or a medium frequency furnace as raw materials for smelting, and the pressed bars are re-smelted into alloy ingots required by the vacuum air atomization powder making equipment according to the steps of refining aluminum alloy ingots in the smelting furnace, and then powdered again.

[0016] Furthermore, in step S1, the mass percentage of the aluminum alloy powder of 0-20 μm is 20%, the mass percentage of 53-150 μm is 65%; and the mass percentage of above 150 μm is 15%.

[0017] Furthermore, in step S1, using a mixer to homogenize the powder includes:

[0018] S11: Add aluminum alloy powder to the mixer and start vacuuming after closing it. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer. When the vacuum degree is lower than -0.08MPa, stop vacuuming.

[0019] S12: After the vacuum is completed, fill with inert gas;

[0020] S13: Mix the powders, mixing time ≥ 30 minutes.

[0021] Furthermore, in step S12, after the inert gas is filled, the absolute value of the pressure difference between the mixer and the atmospheric pressure is ≤3 KPa.

[0022] Furthermore, in step S2, the mold radius r is 30-40 mm, the length h≤700 mm, and the wall thickness is 3-5 mm.

[0023] Furthermore, in step S2, the mold is made of polymer polyurethane material or silicone material.

[0024] Furthermore, in step S2, after the powder is loaded into the mold, the mold is placed on a vibration platform, and the vibration frequency is set to 30 Hz and the vibration time is ≥ 120 s.

[0025] Furthermore, in step S3, the cold isostatic pressing equipment is oil isostatic pressing or water isostatic pressing.

[0026] Furthermore, the pressurization and pressure-holding process in step S3 is divided into 5 stages: initial pressurization P1, the pressure-holding time is 5-15min; secondary pressurization P2, the pressure-holding time is 5-15min; tertiary pressurization P3, the pressure-holding time is 5-15min; quaternary pressurization P3, the pressure-holding time is 5-15min; fifth pressurization P5, the pressure-holding time is 5-15min; and P1≥20Mpa, P5>P4>P3>P2>P1, 200Mpa≤P5≤250Mpa.

[0027] Furthermore, the holding time is 50Mpa≥P2-P1≥p3-p2≥p4-p3≥p5-p4≥20Mpa.

[0028] The beneficial effects of the method for recycling unfinished aluminum alloy powder according to the embodiment of the present invention include:

[0029] (1) The aluminum alloy rod pressed by the pressing method of the present invention can be used as a raw material for re-smelting to make qualified aluminum alloy ingots by slight adjustment according to the difference between the pressed rod powder composition and the designed composition, and used for preparing aluminum alloy powder for 3D printing again, thereby realizing the repeated recycling of unqualified powder, coarse powder and other idle powders;

[0030] (2) The composition of the re-produced aluminum alloy powder is stable, and its oxygen content is not significantly higher than that of the original powder; the unfinished aluminum alloy powder in the re-produced aluminum alloy powder can be recycled and repeated using the method of the present invention to achieve unlimited recycling without affecting the quality of the final aluminum alloy powder.

[0031] (3) By limiting the mixing ratio of powders of different particle sizes, the powder density in the mold, the mold material and size, and the pressurization method of the present invention, the air content of the aluminum alloy loaded into the mold is low, which does not affect the subsequent smelting of the aluminum alloy rod. The density of the aluminum alloy rod after pressing is as high as 2.6g / cm 3 , which solves the problem of smoke generation during the smelting process, and the oxygen increment of the aluminum alloy powder obtained after powder making is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 This is a scanning electron microscope image of the powder before pressing of Example 1 of the present invention;

[0034] Figure 2 This is a scanning electron microscope image of the aluminum alloy powder after atomization and powdering again according to Example 1 of the present invention;

[0035] Figure 3 for Figure 2 A zoomed in picture:

[0036] Figure 4 This is a picture of the aluminum alloy bar after being pressed according to Example 1 of the present invention;

[0037] Figure 5 This is a picture of the comparative example 1 of the present invention after pressing. DETAILED DESCRIPTION

[0038] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiment in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiment, it is carried out according to the conditions recommended by the normal conditions or the manufacturers. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0039] The present invention provides a method for recycling unfinished aluminum alloy powder, comprising the following steps:

[0040] Step S1: collecting aluminum alloy powders of different particle sizes, wherein the mass percentage of aluminum alloy powders of 0-20 μm is 17-22%, the mass percentage of aluminum alloy powders of 53-150 μm is 58-68%, and the mass percentage of aluminum alloy powders of 150 μm and above is 15-20%; using a mixer with inert gas protection to homogenize and mix the above aluminum alloy powders;

[0041] Step S2: loading the mixed metal powder into an isostatic pressing mold, wherein the powder bulk ratio in the mold is ≥55% of the alloy density;

[0042] Step S3: After the powder is filled, a plug is installed on the sealing mold, and the mold after encapsulation is placed in a cold isostatic pressing device for pressurization and pressure holding, and the pressurization and pressure holding are performed for multiple times;

[0043] Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out;

[0044] Step S5: The qualified pressed bars are loaded into a resistance furnace or a medium frequency furnace as raw materials for smelting, and the pressed bars are re-smelted into alloy ingots required by the vacuum air atomization powder making equipment according to the steps of refining aluminum alloy ingots in the smelting furnace, and then powdered again.

[0045] It should be noted that the inert gas in step S1 is preferably argon or nitrogen, which has low cost and is not easy to react chemically with aluminum alloys. The aluminum alloy described in the present invention includes various aluminum alloys, such as aluminum-iron alloy, aluminum-zirconium alloy, aluminum-silicon alloy, aluminum-manganese alloy, aluminum-scandium alloy, etc., and also includes pure aluminum or pure magnesium with properties similar to those of aluminum alloys.

[0046] The aluminum alloy rod pressed by the pressing method of the present invention can be used as a raw material for re-smelting to make a qualified aluminum alloy ingot by slight adjustment according to the difference between the pressed rod powder composition and the designed composition, and used for preparing aluminum alloy powder for 3D printing again, thereby realizing the repeated recycling of unqualified powder, coarse powder and other idle powders;

[0047] The composition of the re-produced aluminum alloy powder is stable, and its oxygen content is not higher than that of the original powder; the unfinished aluminum alloy powder in the re-produced aluminum alloy powder can be recycled and repeated using the method of the present invention to achieve wireless recycling without affecting the quality of the final aluminum alloy powder.

[0048] By limiting the mixing ratio of powders of different particle sizes, the powder density in the mold, the mold material and size, and the pressurization method of the present invention, the air content of the aluminum alloy loaded into the mold is low, which does not affect the quality of the aluminum alloy powder obtained after subsequent smelting and powdering of the aluminum alloy rod.

[0049] When the mass percentage of powders of different particle sizes is not within the scope of the present technical solution, the obtained metal rod has low density and high oxygen content, and the finally obtained aluminum alloy powder is of poor quality and cannot be used or recycled. Because the aluminum alloy powder is fine, there is a risk of dust explosion due to frictional heat or static electricity under high oxygen concentration, and there are safety hazards when mixed in air. Therefore, an inert gas must be used to fill the volume for protection, mainly argon or nitrogen, which are low in cost and not easy to react chemically with aluminum alloy. The protective mixer uniformly mixes the three powders of different particle sizes. During mixing, the effective volume of the mixer shall not exceed 2 / 3 of the rated volume of the mixer, otherwise the powder will not be mixed in the mixer during rotating mixing. Mixing space, cannot be fully mixed evenly; when the mixer is evacuated, there will be filtering devices such as filter elements at the inner end of the vacuum pump pipeline of the mixer, which will not affect the air extraction; after the vacuum degree is lower than -0.08MPa, stop evacuating, control the oxygen content in the mixer to be low, and after filling with inert gas, the pressure in the mixer is slightly negative or slightly positive relative to the atmospheric pressure, and the pressure is equivalent to the atmospheric pressure, ensuring that the powder after mixing is not easy to produce convection with the gas in the air, which is beneficial to the protection of the aluminum alloy powder by the inert gas; the powder loaded into the mold has a higher density, which increases the weight of a single pressing on the one hand, and prevents the powder compression rate from being too high, resulting in large deformation of the mold during the pressing process, and the equipment compression liquid from penetrating into the mold, causing powder contamination in the mold.

[0050] By controlling the pressure of cold isostatic pressing on the powder, the obtained aluminum alloy rod has a higher density and a lower air content, which does not affect the quality of the aluminum alloy powder after secondary powder making. It can achieve unlimited reuse of unfinished aluminum alloy powder, reduce 3D printing costs, and solve the backlog problem of unfinished aluminum alloy powder.

[0051] Preferably, in step S1, the mass percentage of the aluminum alloy powder of 0-20 μm is 20%, the mass percentage of 53-150 μm is 65%; and the mass percentage of above 150 μm is 15%.

[0052] Specifically, in step S1, using a mixer to homogenize the powder includes:

[0053] S11: Add aluminum alloy powder to the mixer and start vacuuming after closing it. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer. When the vacuum degree is lower than -0.08MPa, stop vacuuming.

[0054] S12: After the vacuum is completed, fill with inert gas;

[0055] S13: Mix the powders, mixing time ≥ 30 minutes.

[0056] By improving the aluminum alloy powder mixing process, on the one hand, the risk factor in the aluminum alloy powder mixing process is reduced, and on the other hand, no other impurities are added during the mixing process, and uniform mixing of the powder is achieved, laying the foundation for the density of the powder after being loaded into the mold and the quality of the final aluminum alloy powder.

[0057] Specifically, after the inert gas is filled, the absolute value of the pressure difference between the mixer and the atmospheric pressure is ≤3 KPa.

[0058] By controlling the pressure difference between the pressure in the mixer and the atmospheric pressure, convection between the mixer and the atmospheric pressure can be reduced or avoided, thereby preventing aluminum alloy powder from being ejected outward and air from entering the mixer after the mixer is opened after mixing.

[0059] Specifically, in step S2, the mold radius r is 30-40 mm, the length h≤700 mm, and the wall thickness is 3-5 mm.

[0060] It should be noted that the mold radius r refers to the inner diameter of the mold.

[0061] The best die size is 30-40mm in diameter. A larger diameter will result in higher pressing efficiency, but a higher diameter will lead to lower pressing density. The best maximum length is no more than 700mm. The longer the die, the easier it is for the pressed bar to break.

[0062] Preferably, the mold is made of polymer polyurethane material or silicone material.

[0063] Specifically, in step S2, after the powder is loaded into the mold, the mold is placed on a vibration platform, and the vibration frequency is set to 30 Hz and the vibration time is ≥ 120 s.

[0064] The density of the aluminum alloy powder in the mold is further enhanced by a vibration platform.

[0065] As a preferred solution, the cold isostatic pressing equipment is oil isostatic pressing or water isostatic pressing.

[0066] Specifically, the pressurization and pressure-holding process in step S3 is divided into 5 stages: initial pressurization P1, with a pressure-holding time of 5-15 min; secondary pressurization P2, with a pressure-holding time of 5-15 min; tertiary pressurization P3, with a pressure-holding time of 5-15 min; quaternary pressurization P3, with a pressure-holding time of 5-15 min; fifth pressurization P5, with a pressure-holding time of 5-15 min; and P1≥20Mpa, P5>P4>P3>P2>P1, 200Mpa≤P5≤250Mpa.

[0067] Preferably, 50Mpa≥P2-P1≥p3-p2≥p4-p3≥p5-p4≥20Mpa.

[0068] In order to further illustrate the present invention, a method for recycling unfinished aluminum alloy powder provided by the present invention is described in detail below in combination with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0069] Example 1

[0070] The present embodiment provides a method for recycling unfinished aluminum alloy powder, which comprises the following steps:

[0071] Step S1: Collect aluminum alloys (AlSi10Mg) of different particle sizes, the mass of aluminum alloy powder 0-20 μm is 1020 g, the mass of 53-150 μm is 4080 g; the mass of 150 μm and above is 900 g; use a mixer with nitrogen protection to homogenize and mix the above aluminum alloy powders; the details are as follows:

[0072] S11: Add aluminum alloy powder to W-500L double cone high efficiency mixer and start vacuuming after closing. When the vacuum degree is lower than 0.08MPa, stop vacuuming. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer.

[0073] S12: After the vacuuming is completed, nitrogen is charged; after the nitrogen is charged, the pressure in the mixer is consistent with the atmospheric pressure;

[0074] S13: Mixing powder, mixing time ≥ 30 minutes;

[0075] Step S2: The mixed metal powder is loaded into an isostatic pressing mold, wherein the mold radius r is 30 mm, the length h is 700 mm, and the wall thickness is 3 mm; the mold is made of polymer polyurethane or silicone material; after the powder is loaded into the mold, the mold is placed on a vibration platform, the vibration frequency is set to 30 Hz, and the vibration time is ≥ 120 s, so that the powder bulk ratio in the final mold is 1.48 g / cm 3 ;

[0076] Step S3: After the powder is loaded, the sealing mold is installed with a plug, and the encapsulated mold is placed in a cold isostatic pressing device for pressurization and pressure holding. The pressurization and pressure holding process are divided into 5 stages: the initial pressurization is 20Mpa, and the pressure holding time is 15min; the second pressurization is 70Mpa, and the pressure holding time is 15min; the third pressurization is 120Mpa, and the pressure holding time is 15min; the fourth pressurization is 170Mpa, and the pressure holding time is 15min; the fifth pressurization is 220Mpa, and the pressure holding time is 15min;

[0077] Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out. Figure 4 As shown;

[0078] Step S5: The pressed rods that have passed the pressing are loaded into the resistance furnace as raw materials for smelting, and the pressed rods are re-smelted into alloy ingots required by the vacuum gas atomization powder making equipment according to the steps of smelting aluminum alloy ingots in the smelting furnace, and then powdered again. Both the resistance furnace smelting and the vacuum atomization powder making adopt the commonly used technical means in the prior art, which will not be repeated here. The electron microscope image of the powder before pressing of this embodiment is as follows Figure 1 As shown, the aluminum alloy powder after atomization and powdering in this embodiment is as follows Figure 2 As shown, Figure 3 for Figure 2 Magnified image of .

[0079] Example 2

[0080] The present embodiment provides a method for recycling unfinished aluminum alloy powder, which comprises the following steps:

[0081] Step S1: collecting aluminum alloys (AlMgErZr) of different particle sizes, the mass of aluminum alloy powder 0-20 μm is 1320 g, the mass of 53-150 μm is 3480 g; the mass of 150 μm and above is 1200 g; using a mixer with nitrogen protection to homogenize and mix the above aluminum alloy powders; the details are as follows:

[0082] S11: Add aluminum alloy powder to W-500L double cone high efficiency mixer and start vacuuming after closing. When the vacuum degree is lower than 0.08MPa, stop vacuuming. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer.

[0083] S12: After the vacuuming is completed, nitrogen is charged; after the nitrogen is charged, the pressure in the mixer is consistent with the atmospheric pressure;

[0084] S13: Mixing powder, mixing time ≥ 30 minutes;

[0085] Step S2: The mixed metal powder is loaded into an isostatic pressing mold, wherein the mold radius r is 40 mm, the length h is 600 mm, and the wall thickness is 5 mm; the mold is made of polymer polyurethane or silicone material; after the powder is loaded into the mold, the mold is placed on a vibration platform, the vibration frequency is set to 30 Hz, and the vibration time is ≥ 120 s, so that the powder bulk ratio in the final mold is 1.5 g / cm 3 ;

[0086] Step S3: After the powder is loaded, the sealing mold is installed with a plug, and the encapsulated mold is placed in a cold isostatic pressing device for pressurization and pressure holding. The pressurization and pressure holding process are divided into 5 stages, with the initial pressurization of 50 MPa and a pressure holding time of 5 min; the second pressurization of 100 MPa and a pressure holding time of 5 min; the third pressurization of 150 MPa and a pressure holding time of 5 min; the fourth pressurization of 200 MPa and a pressure holding time of 5 min; the fifth pressurization of 250 MPa and a pressure holding time of 5 min;

[0087] Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out;

[0088] Step S5: The pressed rods that have passed the pressing are loaded into the resistance furnace as raw materials for smelting, and the pressed rods are re-smelted into alloy ingots required by the vacuum gas atomization powder making equipment according to the steps of smelting the aluminum alloy ingots in the smelting furnace, and then powdered again. Both the resistance furnace smelting and the vacuum atomization powder making adopt the commonly used technical means in the prior art, which will not be repeated here.

[0089] Example 3

[0090] The present embodiment provides a method for recycling unfinished aluminum alloy powder, which comprises the following steps:

[0091] Step S1: Collect aluminum alloy (7075) of different particle sizes, the weight of aluminum alloy powder 0-20 μm is 1200 g, the weight of aluminum alloy powder 53-150 μm is 3900 g; the weight of aluminum alloy powder above 150 μm is 900 g; use a mixer with nitrogen protection to homogenize and mix the above aluminum alloy powders; the details are as follows:

[0092] S11: Add aluminum alloy powder to W-500L double cone high efficiency mixer and start vacuuming after closing. When the vacuum degree is lower than 0.08MPa, stop vacuuming. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer.

[0093] S12: After the vacuuming is completed, nitrogen is charged; after the nitrogen is charged, the pressure in the mixer is consistent with the atmospheric pressure;

[0094] S13: Mixing powder, mixing time ≥ 30 minutes;

[0095] Step S2: The mixed metal powder is loaded into an isostatic pressing mold, wherein the mold radius r is 35 mm, the length h is 600 mm, and the wall thickness is 4 mm; the mold is made of polymer polyurethane or silicone material; after the powder is loaded into the mold, the mold is placed on a vibration platform, the vibration frequency is set to 30 Hz, and the vibration time is ≥ 120 s, so that the powder bulk ratio in the final mold is 1.52 g / cm 3 ;

[0096] Step S3: After the powder is loaded, the sealing mold is installed with a plug, and the encapsulated mold is placed in a cold isostatic pressing device for pressurization and pressure holding. The pressurization and pressure holding process are divided into 5 stages: initial pressurization of 40 MPa, and the pressure holding time is 10 min; secondary pressurization of 80 MPa, and the pressure holding time is 10 min; third pressurization of 120 MPa, and the pressure holding time is 10 min; fourth pressurization of 160 MPa, and the pressure holding time is 10 min; fifth pressurization of 200 MPa, and the pressure holding time is 10 min;

[0097] Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out. Figure 4 As shown;

[0098] Step S5: The pressed rods that have passed the pressing are loaded into the resistance furnace as raw materials for smelting, and the pressed rods are re-smelted into alloy ingots required by the vacuum gas atomization powder making equipment according to the steps of smelting the aluminum alloy ingots in the smelting furnace, and then powdered again. Both the resistance furnace smelting and the vacuum atomization powder making adopt the commonly used technical means in the prior art, which will not be repeated here.

[0099] Comparative Example 1 (Compared with Example 3, the powder particle size distribution is different)

[0100] Compared with Example 3, the difference is that aluminum alloy (7075) of different particle sizes is collected, and the weight of aluminum alloy powder 53-250 μm is 6000 g. Figure 5 shown.

[0101] Comparative Example 2 (Compared with Example 3, the aluminum alloy powder was replaced with steel alloy powder)

[0102] Compared with Example 3, the difference is that the aluminum alloy 7075 powder is replaced by the steel alloy 18Ni300 powder.

[0103] Comparative Example 3 (Compared with Example 3, the pressurization process is different)

[0104] Compared with Example 3, the difference is that the pressurization and pressure-holding process is divided into 5 stages, with an initial pressurization of 40 MPa and a pressure-holding time of 10 min; a second pressurization of 80 MPa and a pressure-holding time of 10 min; a third pressurization of 120 MPa and a pressure-holding time of 10 min; a fourth pressurization of 150 MPa and a pressure-holding time of 10 min; and a fifth pressurization of 150 MPa and a pressure-holding time of 10 min.

[0105] Comparative Example 4 (Compared with Example 3, paraffin was added to the powder)

[0106] Compared with Example 3, the difference is that before the powder is loaded into the mold, 50g of paraffin is added and mixed evenly with the powder.

[0107] Comparative Example 5 (Different mold size compared to Example 3)

[0108] Compared with Example 3, the difference is that the size of the mold for loading the powder is a radius r of 50 mm, a length h of 1000 mm, and a wall thickness of 4 mm.

[0109] Comparative Example 6 (Compared with Example 3, no vibration was performed)

[0110] Compared with Example 3, the difference is that after the powder is loaded into the mold, the mold is not placed on a vibration platform, and the loose ratio of the metal powder in the mold is 1.2 g / cm 3 .

[0111] The comparison of the test conditions of Examples 1-3 and Comparative Examples 1-6 is shown in Table 1:

[0112] Table 1

[0113]

[0114] The compression conditions and the performance test results after final powder making of Examples 1-3 and Comparative Examples 1-6 are shown in Table 2:

[0115] Table 2

[0116]

[0117] The powder oxygen increment is measured by ON-3000 oxygen and nitrogen analyzer to detect the oxygen content of the alloy ingot after smelting or the oxygen content of the re-made powder. The powder oxygen increment in this table refers to the oxygen content of the powder after re-making compared with the original powder.

[0118] The amount of smoke is directly related to the density of the pressed bar. The greater the density of the pressed bar, the closer it is to the density of the alloy ingot, the smaller the smoke, and the smaller the burnout of the active components. This is because the pressed bar will contain more or less air, and the air gas contained in it will be continuously released during the melting process of the pressed material. The oxygen in the gas will react chemically with the active elements in the alloy components at high temperatures, causing some of the active elements in contact with these gases to oxidize and smoke and be lost. Some of the oxygen remains in the alloy liquid, causing the oxygen content of the smelted alloy ingot to increase. In addition, the continuous smoke from the alloy liquid will also destroy the liquid film on the surface of the alloy liquid, increase the probability of contact between the metal liquid surface and the oxygen content, and also increase the probability of an increase in the oxygen content of the alloy.

[0119] The aluminum alloy powders obtained in Examples 1-3 have a lower oxygen content increment than the original powder, which is less than 25ppm. This is because the aluminum alloy loaded into the mold has a low air content, which does not affect the quality of the aluminum alloy powder obtained after the subsequent smelting and powdering of the aluminum alloy rods. The composition of the re-produced aluminum alloy powder is stable, and its oxygen content is not significantly higher than that of the original powder. The unfinished aluminum alloy powder in the re-produced aluminum alloy powder can be recycled again and again using the method of the present invention to achieve wireless recycling without affecting the quality of the final aluminum alloy powder. The pressed aluminum alloy rods have no cracks and a density of up to 2.6g / cm 3 In addition, the amount of smoke generated during the smelting process of aluminum alloy bars is small, which makes it easy to observe the smelting process and is more conducive to safe production.

[0120] By comparing Comparative Examples 1-3 with Example 3, it is shown that the particle size distribution has a great influence on the compression molding, the type of pressed powder, and the pressure during the compression process. The molding effect of mixed compression of powders of different coarseness and fineness is much greater than the compression effect of powders of a single particle size segment. This is because the smaller particle size particles are squeezed into the gap between the larger particles during the compression process, which increases the contact between the particles and makes it easier to form during the compression process. The density of steel alloy powder is larger than that of aluminum alloy powder. After testing, it is found that steel alloy powder cannot be pressed into shape. When pressurizing, the setting of the maximum pressure has a great influence on the compression molding. When the pressing pressure is too large, the mold will be damaged, and the compressed liquid will enter the mold and pollute the material. However, if the pressure is too low, the compression molding cannot be carried out, and thus the powder cannot be made again. When the pressure is within the scope of the present invention, the compression molding can be achieved without affecting the subsequent powder making quality.

[0121] By comparing Comparative Examples 4-6 with Example 3, it is shown that the addition of paraffin not only mixes in impurities, but also seriously affects the quality of the final powder. Since the mold size is too large and the looseness before pressing is relatively low, the alloy rods obtained by pressing have severe smoking during the smelting process, which poses a safety hazard, and the oxygen content of the final powder is still relatively high.

[0122] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recycling unfinished aluminum alloy powder, characterized in that: The following steps are involved: Step S1: collecting aluminum alloy powders of different particle sizes, wherein the mass percentage of aluminum alloy powders of 0-20 μm is 17-22%, the mass percentage of aluminum alloy powders of 53-150 μm is 58-68%, and the mass percentage of aluminum alloy powders of 150 μm and above is 15-20%; using a mixer with inert gas protection to homogenize and mix the above aluminum alloy powders; Step S2: loading the mixed metal powder into an isostatic pressing mold, wherein the powder bulk ratio in the mold is ≥55% of the alloy density; Step S3: After the powder is filled, a plug is installed on the sealing mold, and the mold after encapsulation is placed in a cold isostatic pressing device for pressurization and pressure holding, and pressurization and pressure holding are performed for multiple times; Step S4: After the pressing is completed, the equipment is gradually depressurized, the pressed mold is taken out, the plug on the mold is removed, and the pressed rod is taken out; Step S5: The qualified pressed bars are loaded into a resistance furnace or a medium frequency furnace as raw materials for smelting, and the pressed bars are re-smelted into alloy ingots required by the vacuum air atomization powder making equipment according to the steps of refining aluminum alloy ingots in the smelting furnace, and then powdered again.

2. The method according to claim 1, characterized in that In step S1, the mass percentage of aluminum alloy powder with a particle size of 0-20 μm is 20%, the mass percentage of aluminum alloy powder with a particle size of 53-150 μm is 65%, and the mass percentage of aluminum alloy powder with a particle size of more than 150 μm is 15%.

3. The method according to claim 1, characterized in that: In step S1, using a mixer to homogenize the powder includes: S11: Add aluminum alloy powder to the mixer and start vacuuming after closing it. The amount of aluminum alloy powder added shall not exceed 2 / 3 of the rated volume of the mixer. When the vacuum degree is lower than -0.08MPa, stop vacuuming. S12: After the vacuum is completed, fill with inert gas; S13: Mix the powders, mixing time ≥ 30 minutes.

4. The method according to claim 3, characterized in that In step S12, after the inert gas is filled, the absolute value of the pressure difference between the mixer and the atmospheric pressure is ≤3 KPa.

5. The method according to claim 1, characterized in that In step S2, the mold radius r is 30-40 mm, the length h≤700 nm, and the wall thickness is 3-5 mm.

6. The method according to claim 1, characterized in that In step S2, the mold is made of high molecular weight polyurethane material or silicone material.

7. The method according to claim 1, characterized in that In step S2, after the powder is loaded into the mold, the mold is placed on a vibration platform, and the vibration frequency is set to 30 Hz and the vibration time is ≥ 120 s.

8. The method according to claim 1, characterized in that In step S3, the cold isostatic pressing equipment is oil isostatic pressing or water isostatic pressing.

9. The method according to claim 1, characterized in that: The pressurization and pressure-holding process in step S3 is divided into 5 stages: initial pressurization P1, the pressure-holding time is 5-15min; secondary pressurization P2, the pressure-holding time is 5-15min; tertiary pressurization P3, the pressure-holding time is 5-15min; quaternary pressurization P3, the pressure-holding time is 5-15min; fifth pressurization P5, the pressure-holding time is 5-15min; and P1≥20Mpa, P5>P4>P3>P2>P1, 200Mpa≤P5≤250Mpa.

10. The method according to claim 9, characterized in that 50Mpa≥P2-P1≥p3-p2≥p4-p3≥p5-p4≥20Mpa.