Salt-nitrate separation method and system

By combining the nanofiltration process and the direct cooling nitrate extraction process with the MVR process, the problems of high energy consumption and low product quality in the existing salt and nitrate making processes are solved, and the preparation of high-purity products and the reduction of energy consumption are achieved, which is suitable for industrialization. Production.

CN118791016APending Publication Date: 2024-10-18自贡市轻工业设计研究院有限责任公司 +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411127242.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing salt and nitrate production processes have problems such as high energy consumption, low product quality, and being greatly affected by fluctuations in feed ingredients.

Method used

The nanofiltration process and the direct cooling nitrate extraction process are combined with the MVR salt production and nitrate production processes, and membrane separation and freeze crystallization technology are used to separate and purify sodium chloride and sodium sulfate to improve resource utilization and product purity.

Benefits of technology

It significantly reduces energy consumption, improves the product purity of sodium chloride and sodium sulfate, reaches above industrial standards, reduces production costs and carbon emissions, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791016A_ABST
    Figure CN118791016A_ABST
Patent Text Reader

Abstract

The invention discloses a salt and nitrate separation method and system, and relates to the technical field of salt production, nitrate production and high-salt wastewater treatment, and the salt and nitrate separation method comprises the following steps: adopting a process route I containing a nanofiltration process or a process route II without the nanofiltration process; the process route I comprises a nanofiltration process, a direct-cooling saltpeter extraction process, a saltpeter melting process, an MVR (Mechanical Vapor Recompression) salt preparation process and an MVR saltpeter preparation process, so that a sodium sulfate product and a sodium chloride product are obtained; the second process route has no nanofiltration procedure, and the rest are the same as the first process route. The method is reasonable in design, the solubility physical characteristics of the sodium chloride and the sodium sulfate are utilized, the refined salt product and the sodium sulfate or the mirabilite are produced in the same device by using the raw materials containing the sodium chloride and the sodium sulfate, resources are comprehensively utilized, the resource utilization rate is increased, and the energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the fields of salt making technology, nitrate making technology and high-salt wastewater treatment technology, and more specifically to the fields of a method and system technology for separating salt and nitrate. Background Art

[0002] The evaporation processes mainly include: multi-effect vacuum evaporation and MVR evaporation process. The multi-effect vacuum evaporation process is a method in which water evaporates step by step in multiple evaporation tanks with a combination of positive pressure and "vacuum" states, a pressure difference boiling is formed between each tank, the "secondary steam" of each evaporation tank is used step by step, and the secondary steam of the last effect enters the vacuum condensation system; the energy structure of multi-effect vacuum evaporation is: mainly consumes a small amount of electricity and a large amount of steam. MVR (Mechanical Vapor Recompressor---Mechanical Steam Recompression) is an energy-saving technology that uses external electricity to drive the steam compressor, compresses the low-energy secondary steam through the compressor, increases the temperature and pressure, and increases the thermal enthalpy, turning it into high-energy heating steam, and then enters the heat exchanger for condensation to make full use of the latent heat of steam, thereby reducing the demand for external energy. In normal production, according to the properties of the materials and the process, there is basically no need to supplement steam or a small amount of steam. It is only necessary to use a small amount of steam to heat the brine to the boiling point when starting. In normal production, since the power consumption of the compressor is relatively large compared to the multi-effect, the energy structure of MVR is: mainly consume a large amount of electricity and a small amount of steam. In order to protect the safe operation of the compressor and prevent it from being corroded, the secondary steam must go through a defoaming and washing process after leaving the evaporation chamber before it can enter the compressor for compression.

[0003] In the field of salt production, saltpeter production, and high-salt wastewater, the main methods for separating salt and sodium sulfate include thermal salting-out saltpeter co-production process, mother liquor circulation evaporation saltpeter co-production process, etc. The principle is based on the different solubility properties of NaCl and Na2SO4 at different temperatures in the NaCl-Na2SO4-H20 three-phase system: the solubility of NaCl increases with the increase of temperature, while Na2SO4 is the opposite, and its solubility decreases with the increase of temperature, so they are separated. The thermal salting-out saltpeter co-production is to concentrate the raw materials through a multi-effect evaporation process, and then the salt slurry discharged from the last-effect evaporator at a lower temperature is washed, cooled, and dissolved in Glauber's salt, and then dehydrated to obtain wet salt and salt mother liquor, and the wet salt is dried and packaged to obtain finished salt. A certain amount of powdered salt is added to the salt mother liquor, and then preheated and heated, and the temperature is kept and settled, and the crude salt is obtained by dehydration. The salt mother liquor is returned to evaporate and precipitate salt. This is the thermal salting-out saltpeter co-production process. This process has the disadvantages of high energy consumption and unstable and low quality of NaCl and Na2SO4 products.

[0004] The mother liquor circulation evaporation method for salt and nitrate co-production is a production process technology introduced from Sulzer Company in Switzerland, and is usually called thermal salt and nitrate co-production. That is, the raw materials are sent to the multi-effect evaporation system for evaporation and salt precipitation, and then discharged downstream to the low-temperature final evaporator. While NaCl is precipitated in large quantities in the final evaporator, Na2SO4 is concentrated. When the mother liquor for salt precipitation is heated, the solubility of Na2SO4 decreases and precipitates, while NaCl becomes an unsaturated component because its solubility increases with temperature. Evaporation of water can cause Na2SO4 to continue to precipitate and increase the concentration of NaCl. When the concentration of NaCl reaches or approaches saturation, the mother liquor for salt precipitation is cooled and evaporated, which can cause NaCl to precipitate out in supersaturation and Na2SO4 to be concentrated again. The mother liquor for salt precipitation is returned to heat up and recycled, so that NaCl and Na2SO4 can be separated. This process has the disadvantages of high energy consumption, large mother liquor circulation volume, low product quality, and great influence by feed component fluctuations. Summary of the invention

[0005] The purpose of the present invention is to solve the technical problems of high energy consumption, low product quality and great influence of feed component fluctuation in the existing process, and provide a method and system for separating salt and saltpeter. By utilizing the physical properties of the solubility of sodium chloride and sodium sulfate, raw materials containing sodium chloride and sodium sulfate are used to produce refined salt products and sodium sulfate or mirabilite in the same device, so that resources can be comprehensively utilized, resource utilization rate can be improved, energy consumption can be reduced, etc.

[0006] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0007] The first aspect of the present invention provides a method for separating salt and nitrate, comprising the following steps: using a process route 1 containing a nanofiltration step or a process route 2 without a nanofiltration step;

[0008] Process route 1 containing nanofiltration step: the raw liquid containing sodium chloride and sodium sulfate enters the nanofiltration step for membrane separation and denitrification. The side with high sodium sulfate content produced in the nanofiltration step is the nanofiltration concentrated water side, and the side with low sodium sulfate content is the nanofiltration produced water side. The nanofiltration produced water enters the MVR salt-making step to obtain the sodium chloride product; the nanofiltration concentrated water enters the direct cooling and nitrate extraction step, and the Glauber's salt solid obtained in the direct cooling and nitrate extraction step enters the nitration step. The sodium sulfate solution obtained in the nitration step enters the MVR nitration step to obtain the sodium sulfate product;

[0009] Process route 2 without nanofiltration step: the raw liquid containing sodium chloride and sodium sulfate enters the direct cooling and nitrate extraction step, the Glauber's salt solid obtained in the direct cooling and nitrate extraction step enters the nitrate transformation step, the sodium sulfate solution obtained in the nitrate transformation step enters the MVR nitrate production step to obtain the sodium sulfate product; the secondary low-nitrate and high-salt liquid produced in the nitrate transformation step enters the MVR salt production step to obtain the sodium chloride product.

[0010] Specifically, if higher purity salt is to be produced, process route 1 with nanofiltration process can be adopted. The nanofiltration concentrated water enters the direct cooling and nitrate extraction process, and the nanofiltration produced water enters the MVR salt production process. See the attached Figure 1 On the contrary, if only high-purity salt is produced, process route 2 without nanofiltration can be used. See attached for details. Figure 2 .

[0011] In one embodiment, in the process route 1 containing the nanofiltration step, the nanofiltration step comprises the following steps:

[0012] S1. If the raw material liquid containing sodium chloride and sodium sulfate contains organic matter that affects the operation of the membrane, sodium hypochlorite needs to be added to remove it first, and then the pH value is adjusted between 5 and 9 through a pH adjustment device to meet the operation requirements of the nanofiltration membrane denitrification system;

[0013] S2, the raw liquid then enters the sodium sulfite addition device to ensure that the free chlorine before entering the membrane is always stable;

[0014] S3, then the raw liquid enters the activated carbon adsorption tower, and the activated carbon adsorption tower adsorbs residual chlorine, low molecular organic matter and other pollutants in the water, and has a more obvious adsorption and removal effect on heavy metal ions, COD, etc. in the water, and can also reduce the odor, color and odor in the water. The free chlorine content is normally less than 0.1mg / L. The activated carbon filter can effectively prevent organic pollution and oxidative degradation of the nanofiltration membrane, and is not affected by its own water inlet temperature, pH value and organic mixture. After passing through the activated carbon adsorption tower, it enters the security filter;

[0015] S4, security filter To prevent tiny particles from entering the membrane system and clogging the membrane elements, the raw liquid containing sodium chloride and sodium sulfate filtered by the security filter is transported to the nanofiltration process through a high-pressure pump;

[0016] S5. The main function of the nanofiltration process is to separate and remove nitrate from the raw liquid containing sodium chloride and sodium sulfate after pretreatment. Since its membrane pore diameter is just between monovalent and divalent ions and has a negative charge, it has a very high removal capacity for sulfate, and the sodium chloride solution has a good permeability. It is safe, flexible and easy to operate. The side with a high sodium sulfate content produced by the nanofiltration process is the nanofiltration concentrated water side, and the side with a low sodium sulfate content is the nanofiltration produced water side;

[0017] Specifically, the sodium sulfate content on the nanofiltration water side is 1-5g / l, and the sodium sulfate content on the nanofiltration concentrated water side is 30-65g / l. The nanofiltration process pre-separates the sodium sulfate in the raw materials, and the sodium sulfate content in the nanofiltration produced water is only 1-5g / l, which is conducive to the production of higher purity salt in the salt-making process, such as pharmaceutical-grade salt. At the same time, since the amount of concentrated water is greatly reduced compared to the amount of raw materials, the load on the refrigeration system is reduced, but the investment and operating costs of the refrigeration system are increased. If higher purity salt is produced, process route 1 with a nanofiltration process can be adopted. The nanofiltration concentrated water enters the direct cooling and nitration extraction process, and the nanofiltration produced water enters the MVR salt-making process. See the attached for details. Figure 1 On the contrary, if only high-purity salt is produced, process route 2 without nanofiltration can be used. See attached for details. Figure 2 .

[0018] In one embodiment, for process route 1, the nanofiltration concentrated water enters the direct cooling and nitration extraction process, and the direct cooling and nitration extraction process includes the following steps:

[0019] A1. The nanofiltration concentrated water first passes through the plate precooler and the tube-and-tube precooler in sequence to obtain a low-nitrate and high-salt feed solution;

[0020] A2. The low-nitrate and high-salt liquid then enters the first-stage direct cooling tube-and-tube freezing crystallizer (including tube-and-tube exchanger, circulation pipe, circulation pump, and freezing crystallizer) and directly exchanges cold with the low-temperature refrigerant of the electric energy-driven refrigeration ice machine. The refrigerant flows through the shell side of the tube-and-tube exchanger, and the material flows through the tube side of the tube-and-tube exchanger. The refrigerant temperature of the refrigeration ice machine is -15℃-6℃. By increasing the refrigerant circulation volume in the shell of the first-stage direct cooling tube-and-tube exchanger and controlling the suction pressure of the ice machine, the refrigerant shell temperature of the first-stage direct cooling tube-and-tube exchanger is controlled at -3℃-7℃, and the raw material is frozen to 0℃-10℃, that is, the heat transfer temperature difference is controlled within 3℃ to avoid excessive heat transfer temperature difference, which may cause scaling of the exchanger. At the same time, the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , to avoid the generation of excessively fine Glauber's salt and scaling of the cooler, and at the same time control the retention time of the material in the primary direct cooling tube freezing crystallizer to be greater than 3 hours, so as to increase the particle size of the crystallized Glauber's salt, and float the fine Glauber's salt out through flotation to participate in crystallization, which is beneficial to the separation of Glauber's salt and low-nitrate clear liquid, thereby reducing the floating salt content of the low-nitrate clear liquid;

[0021] A3, a first-stage direct cooling tube freezing crystallizer obtains a slurry of sodium sulfate ((Na2SO4·10H2O)) and a first-stage low-nitrate high-salt feed liquid, and the sodium sulfate ((Na2SO4·10H2O)) slurry is subjected to first-stage direct cooling centrifugal dehydration to obtain a sodium sulfate ((Na2SO4·10H2O)) solid, and the sodium sulfate solid enters the nitrate conversion process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer;

[0022] A4. The primary low-nitrate high-salt liquid enters the secondary direct-cooling tube-and-tube freezing crystallizer (including tube-and-tube exchanger, circulation pipe, circulation pump, and freezing crystallizer) and directly exchanges cold with the low-temperature refrigerant of the electric energy-driven refrigeration ice machine. The refrigerant goes through the shell side of the tube-and-tube exchanger, and the material goes through the tube side of the tube-and-tube exchanger. The refrigerant temperature of the refrigeration ice machine is -15℃-6℃. By increasing the refrigerant circulation volume in the shell of the secondary direct-cooling tube-and-tube exchanger and controlling the suction pressure of the ice machine, the refrigerant shell temperature of the secondary direct-cooling tube-and-tube exchanger is controlled at -13℃-7℃, and the raw material is frozen to -10℃-10℃, that is, the heat transfer temperature difference is controlled within 3℃ to avoid excessive heat transfer temperature difference, which may cause blockage of the secondary direct-cooling tube-and-tube exchanger. At the same time, the supersaturation of the material in the secondary direct-cooling tube-and-tube exchanger is controlled to be less than 1kg / m 3 , to avoid the generation of excessively fine Glauber's salt and scaling of the secondary direct cooling tube exchanger, and at the same time control the retention time of the material in the secondary direct cooling tube freezing crystallizer to be greater than 3 hours, so as to increase the particle size of the crystallized Glauber's salt, and float the fine Glauber's salt out by flotation to participate in crystallization, which is beneficial to the separation of Glauber's salt and low-nitrate clear liquid, thereby reducing the floating salt content of the low-nitrate clear liquid;

[0023] A5, the slurry of sodium sulfate (Na2SO4·10H2O) obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt feed liquid containing 1g / L-20g / L sodium sulfate, the secondary low nitrate high salt feed liquid is pre-cooled and fed, the slurry of sodium sulfate (Na2SO4·10H2O) is subjected to secondary direct cooling centrifugal dehydration to obtain sodium sulfate (Na2SO4·10H2O) solid, and the sodium sulfate solid enters the nitrate conversion process;

[0024] Specifically, by using plate precoolers and shell-and-tube precoolers to recover the coldness of the secondary low-nitrate high-salt liquid, the load of the refrigeration ice machine is reduced and the operating cost is reduced; by adding steam heating to the shell-and-tube precooler where crystallization may occur, the rapid crystal melting pipeline is increased to improve the operating cycle; by increasing the circulation volume of the refrigerant in the shell of the primary direct-cooling shell-and-tube exchanger and the suction pressure of the refrigeration control ice machine, the inlet refrigerant temperature of the primary and secondary direct-cooling shell-and-tube freezing crystallizers is made the same, so that one refrigeration ice machine can be used to supply refrigerant to the primary and secondary direct-cooling shell-and-tube freezing crystallizers, without the need for two ice machines, and the investment, operating cost, management and maintenance cost are greatly reduced; by controlling the heat transfer temperature difference between the refrigerant and the material to within 3°C, the heat transfer temperature difference is avoided to be too large, which may cause blockage of the exchanger, and the refrigerant is directly transferred to the material, and the refrigerant is used to freeze the coolant, and then the coolant is used to freeze the material, which greatly improves the cooling efficiency and reduces the load of the ice machine and the operating cost by 15-30%.

[0025] In one embodiment, the nitrification process comprises the following steps:

[0026] The thenardite solid enters the nitrification process, and in the nitrification process, the thenardite is heated to above 32.38°C by introducing a heat source (the heat source is steam from outside the system when it is started, and the normal operation uses the waste heat in the non-condensable steam containing a small amount of steam in the MVR salt-making system to save consumption). The temperature is controlled in the range of 35°C-60°C. If the temperature is too low, the thenardite solid cannot be completely converted into sodium sulfate solution, and if it is too high, too much energy is wasted and additional steam is required to obtain a solution or slurry containing sodium sulfate. The solution or slurry containing sodium sulfate is centrifuged and dehydrated to obtain wet sodium sulfate solid, and the centrifugal mother liquor enters the MVR nitrification process.

[0027] In one embodiment, the MVR nitrate production process comprises the following steps:

[0028] The centrifugal mother liquor is first preheated to 75°C-105°C by a nitrate making condensate preheater, and then enters an MVR nitrate making evaporator. The evaporation temperature of the MVR nitrate making evaporator is controlled at 85°C-110°C. The evaporated secondary steam is washed by a secondary steam washing tower and then heated and pressurized by an MVR nitrate making compressor driven by electric energy. The heated and pressurized steam is superheated steam. After being sprayed with condensed water to eliminate the overheating, the temperature is 15°C-20°C higher than that of the secondary steam. It returns to the heating chamber of the MVR nitrate making evaporator for heat exchange with the circulating material. The steam condensate generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry enters a nitrate slurry dehydration system to obtain wet sodium sulfate solid, and the wet sodium sulfate solid passes through a wet sodium sulfate drying system to obtain a dry sodium sulfate product.

[0029] Specifically, due to the use of freezing and nitrification processes, similar to recrystallization, the purity of sodium sulfate is ≥99.1%, which exceeds the requirement of ≥99% purity of Class I first-class sodium sulfate in industrial anhydrous sodium sulfate GB / T 6009, thereby improving product quality and selling the product. The slurry can also enter the nitrification process as a heat source for nitrification; the MVR nitrification process uses electricity as the main energy source and only requires a small amount of steam as steam for startup and product drying.

[0030] In one embodiment, the nanofiltration produced water enters the MVR salt production process, and the MVR salt production process includes the following steps:

[0031] The nanofiltration water is first preheated by the salt making mother liquor preheater, then enters the salt making condensate preheater to be preheated to 75℃-115℃, and then enters the MVR salt making evaporator. The evaporation temperature of the MVR salt making evaporator is controlled at 85℃-120℃. The evaporated secondary steam is washed by the secondary steam washing tower and then heated and pressurized by the MVR salt making compressor driven by electric energy. The heated and pressurized steam is superheated steam. After spraying condensed water to eliminate the overheating, the steam temperature is 19℃-21℃ higher than the secondary steam, and then returns to the heating of the MVR salt making evaporator. The chamber exchanges heat with the circulating material, and the high-temperature condensed water generated by the heat exchange of the MVR salt evaporator is used to preheat the feed. The non-condensable steam discharged from the heating chamber of the MVR salt evaporator enters the nitrate barrel of the nitrate system to remove the mirabilite. The MVR salt evaporator obtains salt slurry containing sodium chloride by evaporation. After the salt slurry is washed and flotated by the low-nitrate feed, the small-particle powder salt and impurities are returned to the MVR salt evaporator. The large-particle high-purity salt is dehydrated by the salt slurry dehydration system to obtain wet sodium chloride solid. The wet sodium chloride solid is dried by the wet salt drying system to obtain a dry sodium chloride product.

[0032] Specifically, due to the low sodium sulfate content in the feed of the MVR salt evaporator, coupled with the salt retreat washing and flotation process, the sodium chloride purity is ≥99.5%, which exceeds the industrial salt standard GB / T5462 and the edible salt standard GB / T5461. The requirements of the purity of sodium chloride in the superior grade ≥99.1% have improved the product quality. The MVR salt production process uses electricity as the main energy source, and only requires a small amount of steam for startup and product drying.

[0033] In one embodiment, in process route 2 without a nanofiltration step, the low-nitrate, high-salt liquid containing 3g / L-22g / L sodium sulfate obtained in the direct cooling and nitration extraction step is pre-cooled as the feed for the direct cooling and nitration extraction step, and directly enters the MVR salt production step after recovering the cold.

[0034] The second aspect of the present invention provides a salt-nitre separation system, which adopts the above-mentioned salt-nitre separation method.

[0035] In one embodiment, it includes a first process route system corresponding to process route one or a second process route system corresponding to process route two, the first process route system includes a nanofiltration process system, and the second process route system does not include a nanofiltration process system.

[0036] In one embodiment, the first process route system or the second process route system includes a direct cooling nitrate extraction process system, a nitrate chemical process system, an MVR salt production process system and an MVR nitrate production process system.

[0037] The beneficial effects of the present invention are as follows:

[0038] 1. The present invention recovers sodium chloride and sodium sulfate in raw materials to obtain high-quality products, wherein the purity of sodium chloride is ≥99.5%, which exceeds the requirement of ≥99.1% of sodium chloride in the superior grade in industrial salt standard GB / T5462 and edible salt standard GB / T5461, and the purity of sodium sulfate is ≥99.1%, which exceeds the requirement of ≥99% of purity of Class I first-class sodium sulfate in industrial anhydrous sodium sulfate GB / T6009, thereby improving product quality and being sold as products.

[0039] 2. The present invention adopts direct cooling nitrate extraction + nitrate chemical treatment + MVR recrystallization nitrate production + MVR salt production process, especially the unique design of the direct cooling process, which greatly improves the cooling efficiency and reduces the load of the ice machine. The comprehensive energy consumption level is about 34kgce / ton of salt nitrate, which is significantly lower than the existing process of 75-110kgce / ton of salt nitrate, thereby reducing the production cost.

[0040] 3. The present invention uses electricity as the main energy source and only requires a small amount of steam as steam for startup and drying products. The carbon emissions are greatly reduced, which is green and environmentally friendly and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 It is a schematic flow diagram of process route 1 of the present invention.

[0043] Figure 2 yes Figure 1 Schematic diagram of the structure of the upper part.

[0044] Figure 3 yes Figure 1 Schematic diagram of the structure of the lower part.

[0045] Figure 4 It is a schematic flow diagram of process route 2 of the present invention.

[0046] Figure 5 yes Figure 4 Schematic diagram of the structure of the upper part.

[0047] Figure 6 yes Figure 4 Schematic diagram of the structure of the lower part. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0049] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] Example 1

[0051] A method for separating salt and nitrate, adopting process route 1, including nanofiltration process, direct cooling and nitrate extraction process, nitrate chemical process, MVR salt making process, MVR nitrate making process, raw material liquid containing sodium chloride and sodium sulfate has components of NaCl: 295g / l, Na2SO4: 24g / l, contains oil organic matter that affects membrane operation, and has a temperature of 28°C. The specific process treatment is as follows:

[0052] The nanofiltration process includes the following steps:

[0053] S1, adding sodium hypochlorite to remove oily organic matter;

[0054] S2, then adjust the pH value to 7 through the pH adjustment device;

[0055] S3, add a sodium sulfite adding device to ensure that the free chlorine before entering the membrane is always stable;

[0056] S4, and then enters the activated carbon adsorption tower, where the free chlorine content is less than 0.1 mg / L;

[0057] S5, then enters the security filter to prevent tiny particles from entering the membrane system and clogging the membrane elements;

[0058] S6, and then transported to the nanofiltration process through a high-pressure pump. The nanofiltration pressure is controlled at 2-3MPa. The sodium sulfate content on the nanofiltration water side is 2g / l, the NaCl content is 300g / l, and the sodium sulfate content on the concentrated water side is 56g / l, NaCl

[0059] The content is 290g / l, the concentrated water enters the direct cooling and nitrate extraction process, and the produced water enters the MVR salt making process.

[0060] The direct cooling and nitrate extraction process includes the following steps:

[0061] A1. Nanofiltration concentrated water enters this process. The nanofiltration concentrated water first passes through the plate precooler and the low-nitrate high-salt liquid from the freezing crystallizer to cool down to 18°C, and then enters the shell-and-tube precooler and the low-nitrate high-salt liquid from the freezing crystallizer to cool down to 13°C; there is sodium sulfate crystallization in the shell-and-tube precooler, and the crystallized sodium sulfate slurry enters the precooling crystallization centrifuge to obtain sodium sulfate solid after centrifugal dehydration. The sodium sulfate solid enters the nitrate treatment process, and the precooled low-nitrate high-salt liquid enters the direct cooling shell-and-tube freezing crystallizer.

[0062] A2. The low-temperature refrigerant entering the first-stage direct cooling tube freezing crystallizer is directly exchanged with the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is about -1°C. By increasing the circulation volume of the refrigerant in the shell of the first-stage direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant is controlled at about 5°C in the shell of the first-stage direct cooling tube exchanger, and the raw material is frozen to about 8°C. The heat transfer temperature difference is 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours,

[0063] A3, the slurry of the sodium sulfate obtained in the first-stage direct cooling tube freezing crystallizer is centrifugally dehydrated to obtain the sodium sulfate solid, which enters the nitrate conversion process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer;

[0064] A4. The primary low-nitrate high-salt liquid enters the secondary direct cooling tube freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is -1°C. By increasing the refrigerant circulation volume in the shell of the primary direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant temperature in the shell of the primary direct cooling tube exchanger is controlled at 1°C, and the raw material is frozen to 4°C, that is, the heat transfer temperature difference is controlled to within 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours;

[0065] A5. The slurry of Glauber's salt obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt liquid containing 20g / L sodium sulfate are used for pre-cooling and feeding, and then returned to the nanofiltration process. The slurry of Glauber's salt is centrifugally dehydrated to obtain Glauber's salt solid, and the Glauber's salt solid enters the nitration process.

[0066] The nitrification process includes the following steps:

[0067] The solid sodium sulfate from the freezing process enters the saltpeter barrel of the saltpeter barrel, and a heat source (the heat source is the steam from the outside of the system when the system is started, and the waste heat in the non-condensable steam containing a small amount of steam from the MVR salt-making system is used in normal operation) is introduced into the saltpeter barrel to heat the sodium sulfate to 45°C to obtain a slurry containing sodium sulfate. The slurry is centrifugally dehydrated and the centrifugal mother liquor enters the MVR salt-making process;

[0068] The MVR nitrate making process includes the following steps:

[0069] The solution from the nitration process is first preheated to 85°C by the condensed water from the MVR nitration process, and then enters the MVR nitration evaporator with the evaporation temperature controlled at 95°C. The evaporated secondary steam is washed by the scrubber and then heated and pressurized by the steam compressor. After spraying condensed water to eliminate overheating, the temperature is 16°C higher than that of the secondary steam, and enters the heating chamber of the MVR nitration evaporator for heat exchange with the circulating material. The steam condensed water generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry is discharged into the nitration barrel and enters the dehydration and drying process of sodium sulfate together with the solid in the nitration barrel. The solid is dried to obtain the sodium sulfate product.

[0070] The MVR salt production process includes the following steps:

[0071] The nanofiltration water is first preheated by the evaporation mother liquor of the MVR salt-making process, the primary condensate water preheating, and the secondary condensate water preheating, and then preheated to about 100°C, and then enters the MVR salt-making evaporator. The evaporation temperature is controlled at about 120°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After spraying condensate water to eliminate the superheat, the temperature is 19°C higher than that of the secondary steam, and enters the heating chamber of the MVR salt-making evaporator to exchange heat with the circulating material. The steam condensate generated by the heat exchange preheats the feed. The non-condensable steam discharged from the heating chamber enters the nitration barrel of the nitration system to remove the mirabilite. The salt-making mother liquor of the MVR salt-making process is preheated by the flash device and the feed is cooled to 50°C, and then enters the feed tank of the refrigeration system. The slurry containing sodium chloride obtained by evaporation in the MVR salt-making process is subjected to salt removal, washing and flotation. The large-particle-size, high-purity salt product is discharged into the centrifugal dehydration process. After centrifugal dehydration, wet sodium chloride solid is obtained. The solid is dried to obtain the sodium chloride product, which can also be directly sold as wet salt.

[0072] Example 2

[0073] A method for separating salt and nitrate, adopting process route 2, including direct cooling and nitrate extraction process, nitrate chemical process, MVR salt making process, MVR nitrate making process, raw material liquid containing sodium chloride and sodium sulfate has components of NaCl: 295g / l, Na2SO4: 24g / l, contains oil organic matter that affects membrane operation, temperature is 28°C, and specific process treatment is as follows:

[0074] The direct cooling and nitrate extraction process includes the following steps:

[0075] A1. The raw material liquid first passes through the plate precooler and the low nitrate and high salt liquid from the freezing crystallizer to cool down to 12°C, and then enters the tube-type precooler and the low nitrate and high salt liquid from the freezing crystallizer to cool down to 7°C; the precooled liquid enters the direct cooling tube freezing crystallizer;

[0076] A2. The low-temperature refrigerant entering the first-stage direct cooling tube freezing crystallizer is directly exchanged with the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is about -6°C. By increasing the circulation volume of the refrigerant in the shell of the first-stage direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant is controlled at a shell temperature of about 0°C in the first-stage direct cooling tube exchanger, and the raw material is frozen to about 3°C. The heat transfer temperature difference is 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours,

[0077] A3. The slurry of mirabilite obtained by the first-stage direct cooling tube freezing crystallizer is centrifugally dehydrated to obtain mirabilite solid, which enters the nitrate treatment process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer.

[0078] A4. The primary low-nitrate high-salt liquid enters the secondary direct cooling tube freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is -6°C. By increasing the refrigerant circulation volume in the shell of the primary direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant temperature in the shell of the primary direct cooling tube exchanger is controlled at -4°C, and the raw material is frozen to -1°C, that is, the heat transfer temperature difference is controlled within 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours;

[0079] A5. The slurry of mirabilite obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt liquid containing 14.5g / L sodium sulfate are pre-cooled and fed into the MVR salt making process. The mirabilite slurry is centrifugally dehydrated to obtain mirabilite solid, which enters the nitrate making process.

[0080] The nitrification process includes the following steps:

[0081] The solid Glauber's salt from the freezing process enters the nitration barrel of the nitration process. A heat source is introduced into the nitration barrel (the heat source is steam from outside the system when it is started, and the waste heat in the non-condensable steam containing a small amount of steam from the MVR salt-making system is used in normal operation) to heat the Glauber's salt to 45°C to obtain a slurry containing sodium sulfate. The slurry is centrifuged and the mother liquor of the centrifugal dehydration enters the MVR nitration process.

[0082] The MVR nitrate making process includes the following steps:

[0083] The solution from the nitration process is first preheated to 90°C by the condensed water from the MVR nitration process, and then enters the MVR nitration evaporator with the evaporation temperature controlled at 100°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After being sprayed with condensed water to eliminate overheating, the temperature is 17°C higher than that of the secondary steam. It enters the heating chamber of the MVR nitration evaporator for heat exchange with the circulating material. The steam condensed water generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry is discharged into the nitration barrel and enters the sodium sulfate dehydration and drying process together with the solid in the nitration barrel. The solid is dried to obtain the sodium sulfate product.

[0084] The MVR salt production process includes the following steps:

[0085] The nanofiltration water is first preheated by the evaporation mother liquor of the MVR salt-making process, the primary condensate water preheating, and the secondary condensate water preheating, and then preheated to about 95°C, and then enters the MVR salt-making evaporator. The evaporation temperature is controlled at about 115°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After spraying condensate water to eliminate the superheat, the temperature is 19°C higher than that of the secondary steam, and enters the heating chamber of the MVR salt-making evaporator to exchange heat with the circulating material. The steam condensate generated by the heat exchange preheats the feed. The non-condensable steam discharged from the heating chamber enters the nitration barrel of the nitration system to remove the mirabilite. The salt-making mother liquor of the MVR salt-making process is preheated by the flash device and the feed is cooled to 45°C, and then enters the feed tank of the refrigeration system. The slurry containing sodium chloride obtained by evaporation in the MVR salt-making process is subjected to salt removal, washing and flotation. The large-particle-size, high-purity salt product is discharged into the centrifugal dehydration process. After centrifugal dehydration, wet sodium chloride solid is obtained. The solid is dried to obtain the sodium chloride product, which can also be directly sold as wet salt.

[0086] Example 3

[0087] A method for separating salt and nitrate, adopting process route 1, including nanofiltration process, direct cooling and nitrate extraction process, nitrate chemical process, MVR salt making process, MVR nitrate making process, raw material components NaCl: 295g / l, Na2SO4: 24g / l, no oil organic matter affecting membrane operation, temperature 28°C, specific process treatment is as follows:

[0088] The nanofiltration process includes the following steps:

[0089] S1. Adjust the pH value to 7 through the pH adjustment device.

[0090] S2, then enter the activated carbon adsorption tower

[0091] S3, then enters the security filter to prevent tiny particles from entering the membrane system and clogging the membrane elements.

[0092] S4, and then transported to the nanofiltration process through a high-pressure pump. The nanofiltration pressure is controlled at 2-3MPa. The sodium sulfate content on the nanofiltration water side is 2g / l, the NaCl content is 300g / l, and the sodium sulfate content on the concentrated water side is 56g / l, NaCl

[0093] The content is 290g / l, the concentrated water enters the direct cooling and nitrate extraction process, and the produced water enters the MVR salt making process.

[0094] The direct cooling and nitrate extraction process includes the following steps:

[0095] A1. Nanofiltration concentrated water enters this process. The nanofiltration concentrated water first passes through the plate precooler and the low-nitrate high-salt liquid from the freezing crystallizer to cool down to 18°C, and then enters the shell-and-tube precooler and the low-nitrate high-salt liquid from the freezing crystallizer to cool down to 13°C; there is sodium sulfate crystallization in the shell-and-tube precooler, and the crystallized sodium sulfate slurry enters the precooling crystallization centrifuge to obtain sodium sulfate solid after centrifugal dehydration. The sodium sulfate solid enters the nitrate treatment process, and the precooled low-nitrate high-salt liquid enters the direct cooling shell-and-tube freezing crystallizer.

[0096] A2. The low-temperature refrigerant entering the first-stage direct cooling tube freezing crystallizer is directly exchanged with the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is about -1°C. By increasing the circulation volume of the refrigerant in the shell of the first-stage direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant is controlled at about 5°C in the shell of the first-stage direct cooling tube exchanger, and the raw material is frozen to about 8°C. The heat transfer temperature difference is 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours,

[0097] A3. The slurry of mirabilite obtained by the first-stage direct cooling tube freezing crystallizer is centrifugally dehydrated to obtain mirabilite solid, which enters the nitrate treatment process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer.

[0098] A4. The primary low-nitrate high-salt liquid enters the secondary direct cooling tube freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is -1°C. By increasing the refrigerant circulation volume in the shell of the primary direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant temperature in the shell of the primary direct cooling tube exchanger is controlled at 1°C, and the raw material is frozen to 4°C, that is, the heat transfer temperature difference is controlled to within 3°C, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours;

[0099] A5. The slurry of Glauber's salt obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt liquid containing 20g / L sodium sulfate are used for pre-cooling and feeding, and then returned to the nanofiltration process. The slurry of Glauber's salt is centrifugally dehydrated to obtain Glauber's salt solid, and the Glauber's salt solid enters the nitration process.

[0100] The nitrification process includes the following steps:

[0101] The solid Glauber's salt from the freezing process enters the nitrification barrel of the nitrification process. A heat source is introduced into the nitrification barrel (the heat source is steam from outside the system when it is started, and the waste heat in the non-condensable steam containing a small amount of steam from the MVR salt-making system is used in normal operation) to heat the Glauber's salt to 50°C to obtain a slurry containing sodium sulfate. The slurry is centrifuged and the mother liquor is dehydrated and enters the MVR nitrification process.

[0102] The MVR nitrate making process comprises the following steps:

[0103] The solution from the nitration process is first preheated to 90°C by the condensed water from the MVR nitration process, and then enters the MVR nitration evaporator with the evaporation temperature controlled at 100°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After being sprayed with condensed water to eliminate overheating, the temperature is 16°C higher than that of the secondary steam. It enters the heating chamber of the MVR nitration evaporator for heat exchange with the circulating material. The steam condensed water generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry is discharged into the nitration barrel and enters the sodium sulfate dehydration and drying process together with the solid in the nitration barrel. The solid is dried to obtain the sodium sulfate product.

[0104] The MVR salt production process includes the following steps:

[0105] The nanofiltration water is first preheated by the evaporation mother liquor of the MVR salt-making process, the primary condensate water preheating, and the secondary condensate water preheating, and then preheated to about 100°C, and then enters the MVR salt-making evaporator. The evaporation temperature is controlled at about 120°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After spraying condensate water to eliminate the superheat, the temperature is 19°C higher than that of the secondary steam, and enters the heating chamber of the MVR salt-making evaporator to exchange heat with the circulating material. The steam condensate generated by the heat exchange preheats the feed. The non-condensable steam discharged from the heating chamber enters the nitration barrel of the nitration system to remove the mirabilite. The salt-making mother liquor of the MVR salt-making process is preheated by the flash device and the feed is cooled to 50°C, and then enters the feed tank of the refrigeration system. The slurry containing sodium chloride obtained by evaporation in the MVR salt-making process is subjected to salt removal, washing and flotation. The large-particle-size, high-purity salt product is discharged into the centrifugal dehydration process. After centrifugal dehydration, wet sodium chloride solid is obtained. The solid is dried to obtain the sodium chloride product, which can also be directly sold as wet salt.

[0106] Example 4

[0107] A method for separating salt and nitrate, adopting process route 2, including direct cooling and nitrate extraction process, nitrate chemical process, MVR salt making process, MVR nitrate making process, raw material components NaCl: 295g / l, Na2SO4: 29g / l, containing oil organic matter that affects membrane operation, temperature 28°C,

[0108] The direct cooling and nitrate extraction process includes the following steps:

[0109] A1. The nitrate and high salt raw material liquid first passes through the plate precooler and exchanges cooling with the low nitrate and high salt liquid from the freezing crystallizer to 12°C, and then enters the tube-type precooler and exchanges cooling with the low nitrate and high salt liquid from the freezing crystallizer to 6°C; the precooled raw material liquid enters the direct cooling tube freezing crystallizer;

[0110] A2. The low-temperature refrigerant entering the first-stage direct cooling tube freezing crystallizer is directly exchanged with the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is about -10℃. By increasing the circulation volume of the refrigerant in the shell of the first-stage direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant is controlled at about -3℃ in the shell of the first-stage direct cooling tube exchanger, and the raw material is frozen to about 0℃. The heat transfer temperature difference is 3℃, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours,

[0111] A3. The slurry of mirabilite obtained by the first-stage direct cooling tube freezing crystallizer is centrifugally dehydrated to obtain mirabilite solid, which enters the nitrate treatment process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer.

[0112] A1. The primary low-nitrate high-salt liquid enters the secondary direct cooling tube freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the refrigeration ice machine. The refrigerant temperature of the refrigeration ice machine is -10℃. By increasing the circulation volume of the refrigerant in the shell of the primary direct cooling tube exchanger and controlling the suction pressure of the ice machine, the refrigerant temperature in the shell of the primary direct cooling tube exchanger is controlled at -8℃, and the raw material is frozen to -5℃, that is, the heat transfer temperature difference is controlled within 3℃, and the supersaturation of the material in the exchanger is controlled to be less than 1kg / m 3 , control the residence time of the material in the crystallizer to be greater than 3 hours;

[0113] A4. The slurry of Glauber's salt obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt liquid containing 7.2g / L sodium sulfate are pre-cooled and fed into the MVR salt making process. The slurry of Glauber's salt is centrifugally dehydrated to obtain Glauber's salt solid, which enters the nitrate making process.

[0114] The nitrification process includes the following steps:

[0115] The solid Glauber's salt from the freezing process enters the nitrification barrel of the nitrification process. A heat source is introduced into the nitrification barrel (the heat source is steam from outside the system when it is started, and the waste heat in the non-condensable steam containing a small amount of steam from the MVR salt-making system is used in normal operation) to heat the Glauber's salt to 50°C to obtain a slurry containing sodium sulfate. The slurry is centrifuged and the mother liquor is dehydrated and enters the MVR nitrification process.

[0116] The MVR nitrate making process includes the following steps:

[0117] The solution from the nitration process is first preheated to 90°C by the condensed water from the MVR nitration process, and then enters the MVR nitration evaporator with the evaporation temperature controlled at 100°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After being sprayed with condensed water to eliminate overheating, the temperature is 16°C higher than that of the secondary steam. It enters the heating chamber of the MVR nitration evaporator for heat exchange with the circulating material. The steam condensed water generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry is discharged into the nitration barrel and enters the sodium sulfate dehydration and drying process together with the solid in the nitration barrel. The solid is dried to obtain the sodium sulfate product.

[0118] The MVR salt production process includes the following steps:

[0119] The nanofiltration water is first preheated by the evaporation mother liquor of the MVR salt-making process, the primary condensate water preheating, and the secondary condensate water preheating, and then preheated to about 95°C, and then enters the MVR salt-making evaporator. The evaporation temperature is controlled at about 115°C. The evaporated secondary steam is washed by the washing tower and then heated and pressurized by the steam compressor. After spraying condensate water to eliminate the superheat, the temperature is 19°C higher than that of the secondary steam, and enters the heating chamber of the MVR salt-making evaporator to exchange heat with the circulating material. The steam condensate generated by the heat exchange preheats the feed. The non-condensable steam discharged from the heating chamber enters the nitration barrel of the nitration system to remove the mirabilite. The salt-making mother liquor of the MVR salt-making process is preheated by the flash device and the feed is cooled to 45°C, and then enters the feed tank of the refrigeration system. The slurry containing sodium chloride obtained by evaporation in the MVR salt-making process is subjected to salt removal, washing and flotation. The large-particle-size, high-purity salt product is discharged into the centrifugal dehydration process. After centrifugal dehydration, wet sodium chloride solid is obtained. The solid is dried to obtain the sodium chloride product, which can also be directly sold as wet salt.

[0120] Comparative Example 1

[0121] Thermal salting-out salt and saltpeter co-production process, raw material composition NaCl: 295g / l, Na2SO4: 24g / l, contains oil organic matter that affects membrane operation, temperature 28℃, evaporation salt system adopts six-effect evaporation process, raw material is preheated by condensed water and secondary steam preheated into the first effect of five-effect evaporation, then the first effect is converted to the second effect, the second effect is converted to the third effect, the third effect is converted to the fourth effect, the fourth effect is converted to the fifth effect, the fifth effect is converted to the sixth effect, the salt slurry discharged from the sixth effect is washed, cooled and dissolved in the mirabilite, and then dehydrated to obtain wet salt and salt mother liquor, the wet salt is dried and packaged to obtain finished salt. A certain amount of powdered salt is added to the salt mother liquor, preheated and heated, kept warm and settled, dehydrated to obtain crude saltpeter, and the salt mother liquor is returned to evaporate and precipitate salt.

[0122] Comparative Example 2

[0123] The mother liquor circulation evaporation method is a salt and saltpeter co-production process. The raw material composition is NaCl: 295g / l, Na2SO4: 24g / l, and contains oil organic matter that affects the operation of the membrane. The temperature is 28℃. The evaporation salt making system adopts a five-effect process, and the evaporation nitrate making system adopts a TVR evaporation + two-stage flash process. The raw material is preheated by condensed water and secondary steam preheating before entering the first effect of the five-effect evaporation, and then the first effect is converted to the second effect, the second effect is converted to the third effect, the third effect is converted to the fourth effect, and the fourth effect is converted to the fifth effect. The salt slurry discharged from each effect is washed and cooled by the feed, and then dehydrated and separated to obtain wet salt and salt mother liquor. The wet salt is dried and packaged to obtain finished salt. The salt mother liquor is preheated by the two-stage flash steam of the nitrate making system and enters the nitrate making evaporator. The secondary steam of the nitrate making evaporator is extracted by the steam jet pump to return part of the steam to the nitrate making heating chamber to heat the material, and the remaining secondary steam enters the flash heating chamber. The nitrate mother liquor enters the two-stage flash cooling and enters the five-effect evaporator of salt making. The salt precipitation mother liquor is then returned to be heated and recycled, so that NaCl and Na2SO4 can be separated.

[0124] The test results are shown in Table 1 below:

[0125]

[0126] The test results are shown in Table 2 below:

[0127]

[0128] As can be seen from Table 2, the quality of industrial salt, edible salt, and industrial anhydrous sodium sulfate prepared in Examples 1 to 4 meets the relevant standards, while the quality of industrial anhydrous sodium sulfate prepared in Comparative Examples 1 and 2 does not meet the relevant standards.

[0129] It can be seen from Table 1 and Table 2 that the energy structure of the processes of Examples 1 to 4 uses green electricity as the main energy source, while the energy structure of the processes of Comparative Examples 1 to 2 uses steam generated by boilers as the main energy source, and the carbon emissions of Examples 1 to 4 are greatly reduced, which are green and environmentally friendly and suitable for industrial production.

Claims

1. A method for separating saltpeter, characterized in that: The method comprises the following steps: adopting a process route 1 including a nanofiltration process or a process route 2 without a nanofiltration process; Process route 1 containing nanofiltration step: the raw liquid containing sodium chloride and sodium sulfate enters the nanofiltration step for membrane separation and denitrification. The side with high sodium sulfate content produced in the nanofiltration step is the nanofiltration concentrated water side, and the side with low sodium sulfate content is the nanofiltration produced water side. The nanofiltration produced water enters the MVR salt-making step to obtain the sodium chloride product; the nanofiltration concentrated water enters the direct cooling and nitrate extraction step, and the Glauber's salt solid obtained in the direct cooling and nitrate extraction step enters the nitration step. The sodium sulfate solution obtained in the nitration step enters the MVR nitration step to obtain the sodium sulfate product; Process route 2 without nanofiltration step: the raw liquid containing sodium chloride and sodium sulfate enters the direct cooling and nitrate extraction step, the Glauber's salt solid obtained in the direct cooling and nitrate extraction step enters the nitrate transformation step, the sodium sulfate solution obtained in the nitrate transformation step enters the MVR nitrate production step to obtain the sodium sulfate product; the secondary low-nitrate and high-salt liquid produced in the nitrate transformation step enters the MVR salt production step to obtain the sodium chloride product.

2. The method for separating saltpeter from saltpeter according to claim 1, characterized in that: In the process route 1 containing the nanofiltration process, the nanofiltration process includes the following steps: S1. If the raw liquid containing sodium chloride and sodium sulfate contains organic matter that affects the operation of the membrane, sodium hypochlorite needs to be added to remove it first, and then the pH value is adjusted between 5 and 9 through a pH adjustment device; S2, the raw liquid then enters the sodium sulfite addition device to ensure that the free chlorine before entering the membrane is always stable; S3, then the raw material liquid enters the activated carbon adsorption tower, and then enters the security filter after passing through the activated carbon adsorption tower; S4, security filter To prevent tiny particles from entering the membrane system and clogging the membrane elements, the raw liquid containing sodium chloride and sodium sulfate filtered by the security filter is transported to the nanofiltration process through a high-pressure pump; S5. The side with high sodium sulfate content produced by the nanofiltration process is the nanofiltration concentrated water side, and the side with low sodium sulfate content is the nanofiltration produced water side.

3. The method for separating salt and nitre according to claim 2, characterized in that: For process route 1, the nanofiltration concentrated water enters the direct cooling and nitration extraction process, which includes the following steps: A1. The nanofiltration concentrated water first passes through the plate precooler and the tube-and-tube precooler in sequence to obtain a low-nitrate and high-salt feed solution; A2. The low-nitrate and high-salt liquid then enters the first-stage direct cooling tube-type freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the electric energy-driven refrigeration ice machine. The refrigerant goes through the shell side of the tube-type cold exchanger, and the material goes through the tube side of the tube-type cold exchanger. The refrigerant temperature of the refrigeration ice machine is -15℃-6℃. By increasing the refrigerant circulation volume in the shell of the first-stage direct cooling tube-type cold exchanger and controlling the suction pressure of the ice machine, the refrigerant shell temperature of the first-stage direct cooling tube-type cold exchanger is controlled at -3℃-7℃, and the raw material is frozen to 0℃-10℃, that is, the heat transfer temperature difference is controlled within 3℃ to avoid excessive heat transfer temperature difference, which may cause scaling of the cold exchanger. At the same time, the supersaturation of the material in the cold exchanger is controlled to be less than 1kg / m 3 , to avoid the generation of excessively fine Glauber's salt and scaling of the cooler, and at the same time control the retention time of the material in the primary direct cooling tube freezing crystallizer to be greater than 3 hours, so as to increase the particle size of the crystallized Glauber's salt, and float the fine Glauber's salt out through flotation to participate in crystallization, which is beneficial to the separation of Glauber's salt and low-nitrate clear liquid, thereby reducing the floating salt content of the low-nitrate clear liquid; A3, a first-stage direct cooling tube freezing crystallizer obtains a slurry of sodium sulfate and a first-stage low-nitrate high-salt feed liquid. The sodium sulfate slurry is subjected to first-stage direct cooling centrifugal dehydration to obtain a sodium sulfate solid. The sodium sulfate solid enters the nitrate conversion process, and the first-stage low-nitrate high-salt feed liquid enters the second-stage direct cooling tube freezing crystallizer; A4. The primary low-nitrate high-salt liquid enters the secondary direct-cooling tube-type freezing crystallizer and directly exchanges cold with the low-temperature refrigerant of the electric energy-driven refrigeration ice machine. The refrigerant goes through the shell side of the tube-type cold exchanger, and the material goes through the tube side of the tube-type cold exchanger. The refrigerant temperature of the refrigeration ice machine is -15℃-6℃. By increasing the refrigerant circulation volume in the shell of the secondary direct-cooling tube-type cold exchanger and controlling the suction pressure of the ice machine, the refrigerant shell temperature of the secondary direct-cooling tube-type cold exchanger is controlled at -13℃-7℃, and the raw material is frozen to -10℃-10℃, that is, the heat transfer temperature difference is controlled to within 3℃, avoiding excessive heat transfer temperature difference, which may cause blockage of the secondary direct-cooling tube-type cold exchanger, and at the same time, the supersaturation of the material in the secondary direct-cooling tube-type cold exchanger is controlled to be less than 1kg / m 3 , to avoid the generation of excessively fine Glauber's salt and scaling of the secondary direct cooling tube exchanger, and at the same time control the retention time of the material in the secondary direct cooling tube freezing crystallizer to be greater than 3 hours, so as to increase the particle size of the crystallized Glauber's salt, and float the fine Glauber's salt out by flotation to participate in crystallization, which is beneficial to the separation of Glauber's salt and low-nitrate clear liquid, thereby reducing the floating salt content of the low-nitrate clear liquid; A5. The slurry of thenardite obtained by the secondary direct cooling tube freezing crystallizer and the secondary low nitrate high salt liquid containing 1g / L-20g / L sodium sulfate are used for pre-cooling and feeding. The slurry of thenardite is subjected to secondary direct cooling centrifugal dehydration to obtain the thenardite solid, which enters the nitrate-reducing process.

4. The method for separating saltpeter from saltpeter according to claim 3, characterized in that: The nitrification process comprises the following steps: The thenardite solid enters the nitrification process, where the temperature of the thenardite is raised to above 32.38°C by introducing a heat source and the temperature is controlled in the range of 35°C-60°C. If the temperature is too low, the thenardite solid cannot be completely converted into sodium sulfate solution, and if it is too high, too much energy is wasted and additional steam is required to obtain a solution or slurry containing sodium sulfate. The solution or slurry containing sodium sulfate is centrifugally dehydrated to obtain wet sodium sulfate solid, and the centrifugal mother liquor enters the MVR nitrification process.

5. The method for separating saltpeter from saltpeter according to claim 4, characterized in that: The MVR nitrate making process includes the following steps: The centrifugal mother liquor is first preheated to 75°C-105°C by a nitrate making condensate preheater, and then enters an MVR nitrate making evaporator. The evaporation temperature of the MVR nitrate making evaporator is controlled at 85°C-110°C. The evaporated secondary steam is washed by a secondary steam washing tower and then heated and pressurized by an MVR nitrate making compressor driven by electric energy. The heated and pressurized steam is superheated steam. After spraying condensate water to eliminate the overheating, the temperature is 15°C-20°C higher than that of the secondary steam. It then returns to the heating chamber of the MVR nitrate making evaporator for heat exchange with the circulating material. The steam condensate generated by the heat exchange preheats the feed, and a slurry containing sodium sulfate is obtained by evaporation. The sodium sulfate slurry enters a nitrate slurry dehydration system to obtain wet sodium sulfate solid, and the wet sodium sulfate solid passes through a wet sodium sulfate drying system to obtain a dry sodium sulfate product.

6. The method for separating saltpeter from saltpeter according to claim 2, characterized in that: The nanofiltration water enters the MVR salt-making process, which includes the following steps: The nanofiltration water is first preheated by the salt making mother liquor preheater, then enters the salt making condensate preheater to be preheated to 75℃-115℃, and then enters the MVR salt making evaporator. The evaporation temperature of the MVR salt making evaporator is controlled at 85℃-120℃. The evaporated secondary steam is washed by the secondary steam washing tower and then heated and pressurized by the MVR salt making compressor driven by electric energy. The heated and pressurized steam is superheated steam. After spraying condensed water to eliminate the overheating, the steam temperature is 19℃-21℃ higher than the secondary steam, and then returns to the heating of the MVR salt making evaporator. The chamber exchanges heat with the circulating material, and the high-temperature condensed water generated by the heat exchange of the MVR salt evaporator is used to preheat the feed. The non-condensable steam discharged from the heating chamber of the MVR salt evaporator enters the nitrate barrel of the nitrate system to remove the mirabilite. The MVR salt evaporator obtains salt slurry containing sodium chloride by evaporation. After the salt slurry is washed and flotated by the low-nitrate feed, the small-particle powder salt and impurities are returned to the MVR salt evaporator. The large-particle high-purity salt is dehydrated by the salt slurry dehydration system to obtain wet sodium chloride solid. The wet sodium chloride solid is dried by the wet salt drying system to obtain a dry sodium chloride product.

7. The method for separating salt and nitrate according to claim 1, characterized in that: In the process route 2 without the nanofiltration step, the low-nitrate and high-salt liquid containing 3g / L-22g / L sodium sulfate obtained in the direct cooling and nitration extraction step is pre-cooled as the feed of the direct cooling and nitration extraction step, and directly enters the MVR salt making step after recovering the cold.

8. A system for separating salt and nitrate, characterized in that: A method for separating saltpeter according to any one of claims 1 to 7.

9. The salt-nitrate separation system according to claim 8, characterized in that: It includes a first process route system corresponding to process route one or a second process route system corresponding to process route two, the first process route system includes a nanofiltration process system, and the second process route system does not include a nanofiltration process system.

10. The salt-nitrate separation system according to claim 8, characterized in that: The first process route system or the second process route system includes a direct cooling and nitrate extraction process system, a nitrate chemical process system, an MVR salt production process system and an MVR nitrate production process system.

Citation Information

Cited By

  • System for producing high-purity sodium chloride from brine and production method thereof

    CN121651384A