High-zirconium refractory material as well as preparation method and application thereof
By designing a multi-layer structure and gradient Al2O3 content in high-zirconium refractory materials, combined with sintering technology, the problems of cracks and pores in the preparation of high-zirconium refractory bricks are solved, the thermal shock resistance and glass liquid erosion resistance are improved, and the furnace's performance is improved. service life.
Patent Information
- Application Number
- CN202411288423.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Existing high-zirconium refractory bricks are prone to cracks and pores during the preparation process, and have poor thermal shock resistance, which affects the life of the glass furnace and the quality of the glass.
High-zirconium refractory materials with a multi-layer structure are used. The surface layer, middle layer and transition layer all contain ZrO2 and Al2O3. The Al2O3 content is optimized through gradient design, combined with cold isostatic pressing or hot pressing sintering technology, to form a dense ZrO2-Al2O3 gradient symmetrical structure. .
It significantly improves the thermal shock resistance and glass liquid erosion resistance of the material, reduces the risk of cracks, improves the mechanical properties and density, and extends the service life of the kiln.
Smart Images

Figure CN118791301A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high temperature resistant materials, and in particular to a high zirconium refractory material and a preparation method and application thereof. Background Art
[0002] Zirconia is one of the key refractory materials that can come into direct contact with molten glass and is widely used in various glass kilns due to its excellent properties such as high temperature resistance, high mechanical strength, corrosion resistance and low pollution.
[0003] At present, high-zirconium refractory bricks prepared by the melt-casting method are widely used in the market, that is, melt-cast bricks with a zirconium oxide content of more than 85wt%. However, since the preparation of high-zirconium refractory bricks involves a melting and cooling process, the cooling rate is relatively fast, resulting in cracks easily appearing in the products and a high porosity content, so the yield is extremely low and the product price remains high. In addition, since zirconium oxide has a high thermal expansion coefficient and low thermal conductivity, its thermal shock resistance is poor. When subjected to thermal shock and uneven heating, it is very easy to crack, resulting in cracking and peeling, which damages the structure of the glass melting pool wall bricks and affects the life of the glass kiln and the quality of the glass.
[0004] Therefore, there is an urgent need to develop a refractory material for glass furnaces that has good resistance to glass liquid erosion and excellent thermal shock resistance. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention provides a high-zirconium refractory material for a glass melting pool having high toughness, high strength, high thermal shock stability and resistance to glass liquid corrosion, and a preparation method thereof.
[0006] The specific content of the invention is as follows: In a first aspect, the present invention provides a high-zirconium refractory material, comprising a surface layer, an intermediate layer, and a transition layer between the intermediate layer and the surface layer, wherein the surface layer, the intermediate layer and the transition layer all contain ZrO2 and Al2O3; wherein: In the surface layer, the volume fraction of Al2O3 is 0<V(Al2O3)≤10 vol%; In the intermediate layer, the volume fraction of Al2O3 is 20 vol%<V(Al2O3)<30 vol%; In the transition layer, the volume fraction of Al2O3 is 15 vol%<V(Al2O3)<20 vol%.
[0007] Optionally, the transition layer is a multi-layer structure, and in the transition layer, the Al2O3 content increases gradually from the surface layer to the middle layer.
[0008] Optionally, the number of layers of the multilayer structure is 1≤n≤4.
[0009] Optionally, in the multilayer structure, the ratio of the thickness of the nth layer to the thickness of the n-1th layer is 0.9-1.1.
[0010] Optionally, the thickness of the surface layer is 10%-30% of the total thickness of the high-zirconium refractory material; The thickness of the intermediate layer is 15%-25% of the total thickness of the high zirconium refractory material.
[0011] Optionally, the high-zirconium refractory material has a relative density of ≥98%, an open porosity of ≤0.4%, a bending strength of ≥600 MPa, and a critical thermal shock resistance temperature difference of ≥600°C.
[0012] In a second aspect, the present invention provides a method for preparing the high zirconium refractory material according to the first aspect, the preparation method comprising: Preparation of ZrO2-Al2O3 composite powder: wet ball milling multiple groups of ZrO2-Al2O3 composite powders with different proportions, drying and sieving to obtain the powders required for forming the surface layer, middle layer and transition layer of high zirconium refractory materials; Molding and sintering: The powder is filled into a mold by layer-by-layer spreading, and is molded by cold isostatic pressing and then pressureless sintering is performed; alternatively, the powder is filled into a mold and sintered by hot pressing to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material.
[0013] Optionally, the liquid medium used in the wet ball milling is composed of a mixture of a polyvinyl alcohol solution and anhydrous ethanol; wherein the volume proportion of the polyvinyl alcohol solution is 10-30 vol%; the amount of the polyvinyl alcohol is 0.5% to 1.5% of the weight of the composite powder; The wet ball milling process has a ball milling time of 10-18 h and a rotation speed of 100-200 r / min.
[0014] Optionally, the cold isostatic pressing pressure is 200-400 Mpa, and the holding time is 2-5 min; The pressureless sintering temperature is 1550-1750°C, and the holding time is 2-4 hours; The hot pressing sintering pressure is 30-70 MPa, the temperature is 1450-1700°C, and the heat preservation and pressure holding time is 1-3 h.
[0015] In a third aspect, the present invention provides an application of the high-zirconium refractory material described in the first aspect, comprising using the high-zirconium refractory material for preparing a glass melt pool.
[0016] Compared with the prior art, the present invention has the following advantages: The present invention provides a high-zirconium refractory material, which includes a surface layer, an intermediate layer, and a transition layer located between the intermediate layer and the surface layer, wherein the surface layer, the intermediate layer and the transition layer all contain ZrO2 and Al2O3; wherein, in the surface layer, the volume fraction of Al2O3 is 0<V(Al2O3)≤10 vol%; in the intermediate layer, the volume fraction of Al2O3 is 20 vol%<V(Al2O3)<30 vol%; and in the transition layer, the volume fraction of Al2O3 is 15vol%<V(Al2O3)<20vol%.
[0017] The high-zirconium refractory material provided by the present invention is used as a raw material for preparing a glass kiln, and has excellent mechanical properties, thermal shock resistance, and resistance to erosion by molten glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 A schematic diagram of the structure of a high-zirconium refractory material provided in an embodiment of the present invention is shown; Figure 2 A flow chart of a method for preparing a high-zirconium refractory material provided by an embodiment of the present invention is shown; Figure 3 The cross-sectional SEM of the high-zirconium refractory material provided by the embodiment of the present invention is shown; Figure 4 The cross-sectional SEM image of the high zirconium refractory material provided by the embodiment of the present invention after being corroded at 1500°C for 4 hours is shown; Figure 5 The EDS surface scanning result diagram of Zr, Y and Si elements in the cross section of the high zirconium refractory material provided by the embodiment of the present invention after being corroded at 1500°C for 4 hours is shown; Figure 6 The figure shows the EDS element analysis result of the cross section of the high zirconium refractory material provided by the embodiment of the present invention after being corroded at 1500°C for 4 hours.
[0020] Description of reference numerals: D0, middle layer; D1, surface layer; D2, transition layer. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.
[0022] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.
[0023] Technologies, methods, and apparatus known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, such technologies, methods, and apparatus should be considered part of the authorization specification.
[0024] In the description of the present invention, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0025] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0026] It should be noted that the components of the high zirconium refractory material provided by the present invention are ZrO2 and Al2O3, wherein ZrO2 refers to Y-stabilized ZrO2. The specific implementation contents of the present invention are as follows: In the first aspect, the present invention provides a high zirconium refractory material, see Figure 1The schematic diagram of the structure of the high zirconium refractory material is shown, wherein the high zirconium refractory material comprises a surface layer D1, an intermediate layer D0, and a transition layer D2 located between the intermediate layer D0 and the surface layer D1, wherein the components of the surface layer D1, the intermediate layer D0 and the transition layer D2 all contain ZrO2 and Al2O3; in the surface layer D1, the volume fraction of Al2O3 is 0<V(Al2O3)≤10 vol%; in the intermediate layer D0, the volume fraction of Al2O3 is 20 vol%<V(Al2O3)<30 vol%; due to the difference in thermal expansion coefficients between zirconium oxide (ZrO2) and aluminum oxide (Al2O3), as the aluminum oxide content increases, the difference in linear expansion coefficients between the surface layer D1 and the intermediate layer D0 of the material will gradually increase, and during the sintering process, the shrinkage force of the intermediate layer D0 rich in Al2O3 is smaller than that of the surface layer D1 region with a high zirconium content. Therefore, the surface layer D1 of the gradient material will produce tensile stress, and there will be compressive stress inside the material; if the stress value is too large, it will damage the material structure (for example, cracks or layer cracks will occur in the surface layer D1). Therefore, the present invention sets a transition layer D2 between the surface layer D1 and the middle layer D0, and the volume fraction of Al2O3 in the transition layer D2 is 15vol%<V(Al2O3)<20 vol%; with the help of the transition layer, the stress value can be optimized to the minimum; in addition, the existence of compressive stress inside the material can reduce the stress at the crack tip, and at the same time, with the release of stress, it will promote the phase transformation of metastable tetragonal zirconium oxide and promote the phase transformation toughening effect; at the same time, due to the existence of the interlayer interface, the crack will be blocked, absorbed, scattered, induced, etc. by the interface, reducing the energy of the crack tip and causing the crack to deflect, extending the crack propagation path. Therefore, on the basis of the phase transformation toughening of zirconium oxide and the dispersion strengthening of the second phase alumina particles, the residual stress caused by the layered structure of the gradient material and the toughening effect of the interface characteristics effectively improve the thermal shock resistance of the material.
[0027] In addition, the present invention optimizes the number of layers, layer thickness and composition of each layer to enable the material to have the minimum thermal stress and the optimal stress gradient, thus having excellent comprehensive performance (relative density ≥ 98%, open porosity ≤ 0.4%, bending strength ≥ 600 Mpa, critical thermal shock resistance temperature difference ≥ 600 ℃). Among them, the transition layer D2 is a multi-layer structure, and the transition layer D2 can be set to d1 (close to D0), d2, d3...d n Layer, but d n :d n-1 The thickness ratio of the layers should be 0.9-1.1, where 1≤n≤4; in the transition layer D2, the alumina content increases gradually from the surface layer D1 to the middle layer D0; the thickness of the middle layer D0 is 15%-25% of the total thickness of the high zirconium refractory material; the thickness of the surface layer D1 is 10%-30% of the total thickness of the high zirconium refractory material.
[0028] In a second aspect, the present invention provides a method for preparing a high-zirconium refractory material. Figure 2 The flowchart of the preparation method of the high zirconium refractory material provided by the embodiment of the present invention is shown as follows: Figure 2 As shown, the preparation method of high zirconium refractory material includes the preparation, molding and sintering of ZrO2-Al2O3 composite powder, which specifically includes the following steps: S1. Wet ball milling of multiple groups of ZrO2-Al2O3 composite powders with different proportions, drying and sieving to obtain powders required for forming the surface layer, middle layer and transition layer of high zirconium refractory materials; In specific implementation, in the powder required for the surface layer, the volume fraction of Al2O3 is 0<V(Al2O3)≤10 vol%; in the powder required for the middle layer, the volume fraction of Al2O3 is 20 vol%<V(Al2O3)<30 vol%; in the powder required for the transition layer, the volume fraction of Al2O3 is 15 vol%<V(Al2O3)<20 vol%. Furthermore, according to actual use, the transition layer can be further gradient-designed into a multi-layer structure, and the Al2O3 content is increased gradually from the surface layer to the middle layer by changing the volume proportion of Al2O3 in the ZrO2-Al2O3 composite powder used to prepare the transition layer. In this way, due to the existence of the interlayer interface, the crack will be blocked, absorbed, scattered, and induced by the interface, which reduces the energy at the crack tip and deflects the crack, extending the crack propagation path. Therefore, on the basis of zirconium oxide phase transformation toughening and second-phase alumina particle dispersion strengthening, the residual stress and interface characteristic toughening caused by the layered structure of the gradient material effectively improve the thermal shock resistance of the material.
[0029] S2. The powder is filled into a mold by layer-by-layer spreading method, and pressureless sintering is performed after forming by cold isostatic pressing; or, the powder is filled into a mold and sintered by hot pressing to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material.
[0030] In the specific implementation, when the pressureless sintering method is adopted, the powder is filled in the mold, and under the action of cold isostatic pressing at 200-400 MPa and holding time of 2-5 min, a prefabricated body is obtained, and the prefabricated body is placed at 1550-1750 ℃ for pressureless sintering and kept warm for 2-4 h to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material; when the hot pressing sintering method is adopted, the pressure is controlled at 30-70 MPa, the temperature is 1450-1700 ℃, and the heat and pressure are kept for 1-3 h to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material.
[0031] In some embodiments, the liquid medium used for wet ball milling consists of a polyvinyl alcohol solution and anhydrous ethanol; wherein the volume ratio of the polyvinyl alcohol solution is 10-30 vol%; the amount of polyvinyl alcohol is 0.5% to 1.5% of the weight of the composite powder; the wet ball milling time is 10-18 h, and the rotation speed is 100-200 r / min.
[0032] In a third aspect, the present invention provides an application of the high-zirconium refractory material described in the first aspect, comprising using the high-zirconium refractory material for preparing a glass melt pool.
[0033] The present invention combines the structural design concept of symmetry + gradient to provide a high-zirconium refractory material. The high zirconium content layer on the surface can maintain the excellent glass liquid corrosion resistance of the zirconia material; the aluminum-rich content layer in the middle layer uses the addition of the second phase aluminum oxide to reduce the thermal expansion coefficient of the zirconia material and improve the thermal conductivity of the material, thereby optimizing the thermal shock resistance of the composite material; the layered gradient layer between the surface layer and the middle layer can minimize the stress gradient, reduce the residual stress of the material, and thus reduce structural defects; the symmetrical structural design can keep the shrinkage rate of each layer of the material synchronized during the sintering process to avoid warping of the material. As a high-zirconium refractory material for glass melting pools, it can reduce the thermal expansion coefficient and improve the thermal conductivity, improve the thermal shock resistance, and use the gradient interface layered structure to improve the mechanical properties, while maintaining the excellent glass liquid corrosion resistance of the zirconia material.
[0034] In order to enable those skilled in the art to more clearly understand the present invention, a high-zirconium refractory material and a preparation method and application thereof according to the present invention are now described in detail through the following examples.
[0035] Example 1 (1) Preparation of ZrO2-Al2O3 composite powder The ZrO2-Al2O3 composite powders with different proportions were ball milled by liquid phase method. The ball milling time was 12 h, the speed was 120r / min, and the liquid medium was 20 vol% polyvinyl alcohol solution and 80 vol% anhydrous ethanol, wherein the amount of polyvinyl alcohol was 0.8% of the weight of the composite powders. After ball milling, the powders were dried and sieved to obtain the powders required for each layer of the gradient material. The composition of each layer of powder is: The composition of the surface layer D1 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 should be 10 vol%.
[0036] The composition of the middle layer D0 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 is 25 vol%.
[0037] The gradient transition layer D2 is composed of ZrO2 and Al2O3, in which the volume fraction of Al2O3 is 17 vol%.
[0038] In this embodiment, the D2 layer is set to 1 layer, that is, n=1.
[0039] (2) Material forming and sintering The powders required for each layer involved in (1) are spread layer by layer, combined with cold isostatic pressing at 300 MPa for 3 minutes to obtain a prefabricated embryo; The thickness of each layer is as follows: the thickness of the surface layer D1 is 17% of the total thickness, the thickness of the middle layer D0 is 22% of the total thickness, and the thickness of the gradient transition layer D2 is 22% of the total thickness.
[0040] The prefabricated body was pressurelessly sintered and kept at 1700 ℃ for 2 h to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material, which has a relative density of about 98%, an open porosity of about 0.38%, a flexural strength of about 660 MPa, and a critical thermal shock resistance temperature difference of about 700-800 ℃.
[0041] Example 2 (1) Preparation of ZrO2-Al2O3 composite powder The ZrO2-Al2O3 composite powders with different proportions were ball milled by liquid phase method. The ball milling time was 12 h, the speed was 120r / min, and the liquid medium was 20 vol% polyvinyl alcohol solution and 80 vol% anhydrous ethanol, wherein the amount of polyvinyl alcohol was 0.8% of the weight of the composite powders. After ball milling, the powders were dried and sieved to obtain the powders required for each layer of the gradient material. The composition of each layer of powder is: The composition of the surface layer D1 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 should be 10 vol%.
[0042] The composition of the middle layer D0 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 is 25 vol%.
[0043] The gradient transition layer D2 is composed of ZrO2 and Al2O3, wherein the volume fraction of Al2O3 is 17 vol%.
[0044] In this embodiment, the D2 layer is set to 1 layer, that is, n=1.
[0045] (2) Material forming and sintering The powders required for each layer involved in (1) are placed in a mold by layer-by-layer spreading method, and hot pressing and sintering are carried out at 1550 °C for 2 h under a pressure of 45 MPa to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material. The relative density of the material is about 99%, the porosity is about 0.28%, the flexural strength is about 750 MPa, and the critical thermal shock resistance temperature difference is about 700-800 °C.
[0046] The thickness of each layer is as follows: the thickness of the surface layer D1 is 17% of the total thickness, the thickness of the middle layer D0 is 22% of the total thickness, and the thickness of the gradient transition layer D2 is 22% of the total thickness.
[0047] Example 3 (1) Preparation of ZrO2-Al2O3 composite powder The ZrO2-Al2O3 composite powders with different proportions were ball milled by liquid phase method. The ball milling time was 12 h, the speed was 120r / min, and the liquid medium was 20 vol% polyvinyl alcohol solution and 80 vol% anhydrous ethanol, wherein the amount of polyvinyl alcohol was 0.8% of the weight of the composite powders. After ball milling, the powders were dried and sieved to obtain the powders required for each layer of the gradient material. The composition of each layer of powder is: The composition of the surface layer D1 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 should be 10 vol%.
[0048] The composition of the middle layer D0 is ZrO2 and Al2O3, wherein the volume fraction of Al2O3 is 25 vol%.
[0049] In the gradient transition layer D2, the composition of d1 is ZrO2 and Al2O3, of which the volume fraction of Al2O3 is 19 vol%; the composition of d2 is ZrO2 and Al2O3, of which the volume fraction of Al2O3 is 17 vol%.
[0050] In this embodiment, the D2 layer is set to 2 layers, that is, n=2.
[0051] (2) Material forming and sintering The powders required for each layer involved in (1) are spread layer by layer, combined with cold isostatic pressing at 300 MPa for 3 minutes to obtain a prefabricated embryo; The thickness of each layer is as follows: the thickness of the surface layer D1 is 17% of the total thickness, the thickness of the middle layer D0 is 14% of the total thickness, the thickness of d1 in the gradient transition layer D2 is 13% of the total thickness, and the thickness of d2 is 13% of the total thickness.
[0052] The prefabricated body was pressurelessly sintered and kept at 1650℃ for 3 h to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material, which has a relative density of about 98%, an open porosity of about 0.35%, a flexural strength of about 680 Mpa, and a critical thermal shock resistance temperature difference of about 700-800℃.
[0053] Comparative Example 1 The same material composition as the surface layer D1 of the embodiment is used to prepare a ZrO2-10 vol% Al2O3 composite powder, and the other process parameters are the same as those of the embodiment to obtain a ZrO2-10 vol% Al2O3 single-layer composite material. The material has a relative density of about 97.8%, an open porosity of about 1.2%, a flexural strength of about 450 Mpa, and a critical thermal shock resistance temperature difference of about 500-600°C.
[0054] Experimental Example (The refractory materials obtained from Example 1 and Comparative Example 1 were selected to perform the following performance tests) (1) Microstructure and mechanical properties Figure 3 The cross-sectional SEM of the high zirconium refractory material provided by the embodiment of the present invention is shown. Figure 3 (a) is a cross-sectional SEM of the high zirconium refractory material provided in Comparative Example 1, Figure 3 (b) is the cross-sectional SEM of the high-zirconium refractory material provided in Example 1. It can be seen that the interlayer interface of the high-zirconium refractory material provided in the embodiment of the present invention is obvious and has good interface bonding. There are a small amount of closed pores inside the material, and there are no obvious defects such as interlayer cracks. According to the national standard GB / T25995-2010, the density and open porosity of the sample were measured by the Archimedes drainage method. The results show that the density of both reached more than 97%; the flexural strength of the material was analyzed by the three-point bending method. It was found that the flexural strength of the ZrO2-Al2O3 gradient material can reach 660 Mpa, which is about 46% higher than that of the ZrO2-Al2O3 single-layer composite material (450 Mpa).
[0055] (2) Thermal shock resistance The water quenching method is used to test the thermal shock resistance, that is, the sample to be tested is placed in a muffle furnace, heated to 400, 600, and 800°C for 10 minutes, then taken out and placed in running water at room temperature for water quenching. The operation is repeated twice. After the sample is cooled and dried, the critical thermal shock resistance temperature difference of the material is determined based on the residual strength of the sample to determine the thermal shock resistance of the sample.
[0056] Analysis of the residual strength of the ZrO2-Al2O3 gradient material after thermal shock testing provided in Example 1 under different thermal shock temperature differences shows that when the thermal shock temperature difference is lower than 600°C, the strength of the material does not decrease significantly; when the thermal shock temperature difference is 700-800°C, the residual strength of the gradient material drops suddenly by about 300-400 Mpa, indicating that the critical thermal shock resistance temperature difference of the material is 800°C, which is about 200°C higher than that of the ZrO2-Al2O3 single-layer composite material.
[0057] (3) Anti-corrosion performance of glass liquid A high-temperature thermal simulation erosion experiment was used to study the sample's resistance to glass liquid erosion. The surface of the test sample was covered with glass powder and placed in a muffle furnace. It was heated to 1500 ℃ and kept warm for 4 h. After cooling with the furnace, a scanning electron microscope (SEM) combined with energy spectrum analysis (EDS) was used to analyze the corrosion of the sample.
[0058] Figure 4 The cross-sectional SEM image of the high zirconium refractory material provided by the embodiment of the present invention after being corroded at 1500°C for 4 hours is shown. Figure 5 The EDS surface scan result of Zr, Y and Si elements in the cross section of the high zirconium refractory material provided by the embodiment of the present invention after being eroded at 1500°C for 4 hours is shown; wherein, Figure 5 (a) shows the EDS surface scan result of Si element. Figure 5 (b) EDS surface scan result of Zr element. Figure 5 (c) EDS surface scan result diagram of element Y; Figure 6 The figure shows the EDS element analysis result of the cross section of the high zirconium refractory material provided by the embodiment of the present invention after being corroded at 1500°C for 4 hours; Figure 4-6 It can be seen that the ZrO2-Al2O3 gradient material provided in Example 1 is in close contact with the glass liquid, and the interface between the two is smooth without obvious corrosion layer. The EDS surface scan results show that there is no obvious diffusion of Zr and Si elements, and the boundary line of element distribution between the glass phase and the gradient material is clearly visible. In addition, the content of the stabilizer element Y in the zirconium oxide raw material powder in the glass liquid is relatively low, indicating that the dissolution of the Y element in the glass liquid is limited. The cross-sectional SEM image of the ZrO2-Al2O3 single-layer composite material and the EDS surface scan result image are similar to Figure 4 , Figure 5 The above results show that the prepared gradient material has excellent anti-glass erosion performance. Compared with the ZrO2-Al2O3 single-layer composite material, it has the same anti-glass erosion effect.
[0059] In summary, compared with ZrO2-Al2O3 single-layer composite materials, ZrO2-Al2O3 gradient materials have equivalent resistance to glass liquid erosion, but ZrO2-Al2O3 gradient materials have better mechanical properties and thermal shock resistance. Refractory brick materials used in glass kilns can effectively improve the service life of the kiln.
[0060] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0061] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0062] The above is a detailed introduction to a high-zirconium refractory material and its preparation method and application provided by the present invention. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A high zirconium refractory material, characterized in that: The high-zirconium refractory material comprises a surface layer, an intermediate layer, and a transition layer between the intermediate layer and the surface layer, wherein the surface layer, the intermediate layer and the transition layer all contain ZrO2 and Al2O3; wherein, In the surface layer, the volume fraction of Al2O3 is 0<V(Al2O3)≤10 vol%; In the intermediate layer, the volume fraction of Al2O3 is 20 vol%<V(Al2O3)<30 vol%; In the transition layer, the volume fraction of Al2O3 is 15 vol%<V(Al2O3)<20 vol%.
2. The high zirconium refractory material according to claim 1, characterized in that: The transition layer is a multi-layer structure, and in the transition layer, the Al2O3 content increases gradually from the surface layer to the middle layer.
3. The high zirconium refractory material according to claim 2, characterized in that: The number of layers of the multilayer structure is 1≤n≤4.
4. The high zirconium refractory material according to claim 2, characterized in that: In the multilayer structure, the ratio of the thickness of the nth layer to the thickness of the n-1th layer is 0.9-1.
1.
5. The high zirconium refractory material according to claim 1, characterized in that: The thickness of the surface layer is 10%-30% of the total thickness of the high zirconium refractory material; The thickness of the intermediate layer is 15%-25% of the total thickness of the high zirconium refractory material.
6. The high zirconium refractory material according to claim 1, characterized in that: The high-zirconium refractory material has a relative density of ≥98%, an open porosity of ≤0.4%, a bending strength of ≥600 Mpa, and a critical thermal shock resistance temperature difference of ≥600°C.
7. A method for preparing the high zirconium refractory material according to any one of claims 1 to 6, characterized in that: The preparation method comprises: Preparation of ZrO2-Al2O3 composite powder: wet ball milling multiple groups of ZrO2-Al2O3 composite powders with different proportions, drying and sieving to obtain the powders required for forming the surface layer, middle layer and transition layer of high zirconium refractory materials; Molding and sintering: The powder is filled into a mold by layer-by-layer spreading, and is molded by cold isostatic pressing and then pressureless sintering is performed; alternatively, the powder is filled into a mold and sintered by hot pressing to obtain a dense ZrO2-Al2O3 gradient symmetrical structure refractory material.
8. The method for preparing a high-zirconium refractory material according to claim 7, characterized in that: The liquid medium used in the wet ball milling is composed of a mixture of polyvinyl alcohol solution and anhydrous ethanol, wherein the volume proportion of the polyvinyl alcohol solution is 10-30 vol%; the amount of the polyvinyl alcohol is 0.5% to 1.5% of the weight of the composite powder; The wet ball milling process has a ball milling time of 10-18 h and a rotation speed of 100-200 r / min.
9. The method for preparing a high-zirconium refractory material according to claim 7, characterized in that: The cold isostatic pressing pressure is 200-400 Mpa, and the holding time is 2-5 min; The pressureless sintering temperature is 1550-1750°C, and the holding time is 2-4 hours; The hot pressing sintering pressure is 30-70 MPa, the temperature is 1450-1700°C, and the heat preservation and pressure holding time is 1-3 h.
10. An application of the high zirconium refractory material according to any one of claims 1 to 6, characterized in that: The high-zirconium refractory material is used for preparing a glass melting pool.
Citation Information
Patent Citations
Method for preparing ceramic coat with biphase gradients of zirconia and alumina on surface of zirconium base
CN101092732A
Alumina / alumina-zirconia laminar composite with composite structure and preparation method thereof
CN103072325A
Zirconia and alumina gradient composite coat and production method thereof
CN104711541A
Glass material preparation crucible and preparation method
CN108395074A
Graphene self-lubricating gradient ceramic cutter material with pressure stress on surface and preparation method thereof
CN110483059A