Low-thermal-conductivity chromium-zirconium-corundum brick for hazardous waste treatment and preparation method thereof

By adopting the preparation method of low-thermal conductivity chromium zirconium corundum bricks, a stable three-dimensional network structure is formed by modifying hydroxy iron oxide and water glass, which solves the problem of insufficient heat resistance and corrosion resistance of existing refractory materials under high temperature and high pressure. It significantly improves the operating efficiency and safety of the incinerator.

CN118993706AActive Publication Date: 2024-11-22ZHENGZHOU RUITAI REFRACTORY MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411045863.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The refractory materials in the lining of existing hazardous waste incinerators are not heat-resistant enough at high temperatures and are not corrosive enough, resulting in low efficiency and short service life of the incinerator, making it difficult to meet the working conditions of high temperature and high pressure.

Method used

Low thermal conductivity chromium zirconium corundum bricks are used to prepare low-quality diatomaceous earth and modified water glass as raw materials. Thermal conduction of chromium zirconium corundum bricks and through specific preparation processes such as hydroxy iron oxide and water glass modification treatment, a stable three-dimensional network structure is formed to improve compressive strength and mechanical properties.

Benefits of technology

It significantly improves heat resistance, corrosion resistance and mechanical properties, extends the service life of refractory materials, and improves the operating efficiency and safety of incinerators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973476680000091
    Figure BDA0004973476680000091
Patent Text Reader

Abstract

The invention belongs to the technical field of refractory materials, and particularly relates to a low-heat-conductivity chromium-zirconium-corundum brick for hazardous waste treatment and a preparation method of the low-heat-conductivity chromium-zirconium-corundum brick. The low-heat-conductivity chromium-zirconium corundum brick with high compressive strength, low heat conductivity coefficient and good thermal shock resistance stability is obtained by mixing, pressing, drying and firing raw materials including fused white corundum powder, zirconium oxide micro powder, chromium oxide micro powder, aluminum oxide micro powder, metakaolin, iron oxyhydroxide modified diatomite and modified water glass. The added hydroxyl ferric oxide modified diatomite and sodium tetraborate modified water glass can generate chemical bonding with other raw materials in the mixing process to form good interface bonding, so that the mechanical property of the product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, in particular to a low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment and a preparation method thereof. Background Art

[0002] With the development of modern industry, the amount of hazardous waste generated has increased year by year, and the harm it brings to the human living environment has become increasingly serious. If the disposal of hazardous waste cannot be properly controlled, it will lead to environmental pollution. Reducing the harm caused by hazardous waste to humans and the environment is a major problem that needs to be solved urgently. Among them, incineration can effectively and permanently destroy, detoxify and even eliminate hazardous waste, and greatly reduce the content of hazardous waste. Due to the complex structure of hazardous waste incinerators, long construction period and large investment, the selection of materials for the lining of the incinerator has a great influence on the application efficiency of the incinerator. In the actual production process, the life of the lining refractory materials for hazardous waste is often related to production costs and efficiency. Therefore, in order to ensure the safe and efficient operation of the incinerator, the selection of refractory materials for its lining is crucial. In order to meet the use requirements of hazardous waste incinerators, its lining refractory materials need to withstand the thermal shock generated during the working process. High thermal shock stability is also the key to determining the life of refractory materials.

[0003] The patent with application number CN202310090067.8 discloses an acid-resistant and salt-resistant modified corundum brick for a rotary kiln in a hazardous waste incineration system and a preparation method. The brick is made of dense fused corundum, brown corundum, zirconyl phosphate-modified zirconia composite, andalusite and silica fume as raw materials, and is obtained by screening, mixing, drying and sintering. The introduction of zirconyl phosphate-modified zirconia composite makes the prepared product stable at high temperature and has high heat resistance, and rare earth modification is added to zirconium oxide, which effectively improves the hardness and anti-aging properties of the product. The patent with application number CN202110997777.X discloses a high-toughness modified silicon corundum brick, which is composed of a liquid binder and a solid mixture, and is formed by sintering, crushing, mixing and secondary sintering in an oxygen-rich environment. The secondary sintering is beneficial to improving the porosity, and the rare earth element oxide is beneficial to improving the thermal conductivity and toughness of the refractory brick after two sinterings. With the development of new processes and technologies, the requirements for the refractory materials used are getting higher and higher. Therefore, developing a product with high compressive strength and good thermal insulation effect has become a research hotspot. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment and a preparation method thereof. By using fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder, metakaolin, diatomaceous earth modified with iron oxide and modified water glass as raw materials, a low thermal conductivity chromium-zirconium corundum brick is prepared.

[0005] The technical solution adopted by the present invention to solve the above technical problems is:

[0006] A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment, the corundum brick comprising, by weight, 55-75 parts of fused white corundum powder, 6-10 parts of zirconium oxide powder, 6-10 parts of chromium oxide powder, 6-8 parts of aluminum oxide powder, 12-16 parts of metakaolin, 5-9 parts of diatomaceous earth modified by oxyhydroxide, and 4-7 parts of modified water glass; preferably, 60 parts of fused white corundum powder, 8 parts of zirconium oxide powder, 8 parts of chromium oxide powder, 7 parts of aluminum oxide powder, 15 parts of metakaolin, 8 parts of diatomaceous earth modified by oxyhydroxide, and 6 parts of modified water glass.

[0007] Among them, chromium oxide is a dark green crystalline powder, which can form different solid solutions or high melting point compounds with some oxides, and can also form low eutectic with high melting point with some silicates. It has good corrosion resistance, especially for alkaline slag and acidic slag. Zirconium oxide is very stable in an oxidizing atmosphere and is also quite stable in a reducing atmosphere. It can resist the corrosion of acidic or neutral slag and has good chemical stability. There is a strong bonding force between aluminum and oxygen in alumina, and alumina has acid-base duality, so alumina has good chemical corrosion resistance.

[0008] Furthermore, the preparation process of the oxyhydroxide modified diatomaceous earth is as follows: ferric chloride hexahydrate and ammonium bicarbonate are mixed in anhydrous ethanol, and diatomaceous earth is added thereto, sealed, stirred at room temperature for 6-8 hours, and then filtered, the stirring speed is 100-150r / min, the filtrate is dried and then ground through an 80-mesh sieve to obtain oxyhydroxide modified diatomaceous earth; wherein the drying conditions are: drying in a vacuum drying oven at 50-60°C for 6-8 hours; wherein the molar ratio of ferric chloride hexahydrate to ammonium bicarbonate is 1-3:4-10; the amount of ferric chloride hexahydrate in anhydrous ethanol is 0.02-0.03g / mL, and the amount of diatomaceous earth in anhydrous ethanol is 0.03-0.05g / mL.

[0009] Diatomaceous earth is a silicate material with the characteristics of good stability, light bulk density, high strength, low thermal conductivity and good thermal insulation effect. Hydroxylated iron oxide is obtained by utilizing ferric chloride hexahydrate and ammonium bicarbonate and then added to diatomaceous earth to obtain diatomaceous earth modified with hydroxyl iron oxide, which provides a large number of hydroxyl groups on the surface of diatomaceous earth.

[0010] Furthermore, the preparation process of the modified water glass is: placing water glass in a container and adding sodium tetraborate thereto, starting stirring to obtain a stable solution, namely the modified water glass; wherein the stirring condition is 400-500r / min, stirring for 20-40min; and the mass ratio of sodium tetraborate to water glass is 0.1:15-25.

[0011] Water glass is a water-soluble silicate solution. When heated, it will produce a large number of bubbles to form a lightweight foam material. However, the thermal insulation material prepared by direct foaming of water glass has low strength and uneven pore distribution. Therefore, sodium tetraborate is added thereto, in which boron enters the Si-O-Si network in the form of boron-oxygen tetrahedrons to form a Si-OB network structure. The presence of chain and ring Si-OT (Si, B) structures is beneficial to enhancing the density of the material matrix and improving the compressive strength of the material.

[0012] The present invention also provides a method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment, and the preparation process is as follows:

[0013] S1. Weigh the raw materials according to the above weight proportions and set aside. Soak the diatomaceous earth modified with iron oxyhydroxide in modified water glass for 10-20 minutes to obtain slurry A.

[0014] S2, mixing the metakaolin with the slurry A obtained in step S1 and stirring in a blender, then adding styrene acrylic emulsion and silane coupling agent, and continuing stirring to obtain slurry B; wherein the stirring conditions are: after mixing the metakaolin with the slurry A obtained in step S1, stirring in a blender at a speed of 80-100 r / min for 4-8 min, then changing the speed to 150-200 r / min and stirring for 3-5 min, adding styrene acrylic emulsion and silane coupling agent and stirring at a speed of 150-200 r / min for 5-8 min; wherein the silane coupling agent is silane coupling agent KH550; the mass ratio of styrene acrylic emulsion, silane coupling agent KH550, and metakaolin is 0.8-1.5:0.3-0.4:100;

[0015] S3, placing fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder and slurry B obtained in step S2 in a mixer and uniformly mixing to obtain a slurry;

[0016] S4, pressing the mud obtained in step S3 into a brick by a press and then placing it in a dryer for drying; wherein the drying standard is: drying until the residual dry moisture inside the brick is 1-5%;

[0017] S5. Load the qualified bricks after drying in step S4 into the high-temperature tunnel kiln, and select the finished products after high-temperature firing and heat preservation; wherein, the high-temperature firing temperature is 1450-1550°C, and the heat preservation is 6-8h.

[0018] Among them, the drying process of step S4 is divided into a constant rate drying stage and a deceleration drying stage, specifically: heating to 100°C at a heating rate of 5°C / h and then heating to 180°C at a heating rate of 3°C / h, drying until the residual dry moisture inside the brick is 1-5%.

[0019] The drying process of the brick blank is essentially that the preheated hot air or hot flue gas transfers heat to the blank, and the blank absorbs heat to increase the temperature so that the moisture evaporates and escapes from the blank and is discharged from the dryer with the hot gas; in the isotropic drying stage, the physical water on the surface of the brick blank is mainly removed, and the moisture evaporates on the surface of the blank. As the moisture is discharged, the blank shrinks accordingly. Therefore, the drying rate is reduced in this stage to prevent the blank from shrinking sharply and cracking; when the isotropic drying stage is basically completed and enters the deceleration drying stage, the evaporation of moisture gradually moves from the surface of the blank to the inside of the blank, and the brick blank absorbs heat from the heat carrier, which increases the temperature of the blank on the one hand and supplies moisture evaporation at the same time. After the moisture evaporates in the pores, it moves from the inside of the blank to the surface, and then diffuses into the heat carrier. When the temperature of the blank rises, and the amount of moisture evaporation is just the maximum amount of water vapor transferred from the pores to the outside, the safe drying speed of the blank is the largest at this time. Therefore, in the present invention, the brick blank is dried by adopting isotropic drying and deceleration drying to ensure that the brick blank has the maximum safe drying rate and avoid the generation of capillary cracks in the brick blank during the drying process.

[0020] The present invention has the following beneficial effects:

[0021] Diatomite is modified by reacting ferric chloride hexahydrate with ammonium bicarbonate to generate ferric hydroxide. By loading ferric hydroxide on diatomite, the dispersibility of diatomite can be improved and a large number of hydroxyl groups are introduced on the surface of diatomite to form chemical bonds with water glass in the raw materials, forming a good interface bonding; at the same time, the introduction of sodium tetraborate helps to form chain and cyclic Si-OT (Si, B) structures, making the material matrix structure more compact, which is beneficial to the improvement of the compressive strength of the product; in addition, in the process of mixing with raw materials such as kaolin, a kaolin-based polymer with a stable three-dimensional network structure can be formed, further improving the mechanical properties of the product; in addition, in the preparation process, the brick blank is dried by adopting the method of constant speed drying and deceleration drying to ensure that the brick blank has the maximum safe drying rate and avoid the formation of capillary cracks in the brick blank during the drying process. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0023] The fused white corundum powder used in the present invention (particle size 5-3, 3-1, ≤1 and ≤0.074mm; ratio of (5-3 and 3-1mm): (≤1 and ≤0.074mm) = 3:4 (mass ratio)), zirconium oxide powder (particle size 50-100μm), chromium oxide powder (≤0.074mm), aluminum oxide powder (5μm), metakaolin purchased from Gongyi Youxing Mineral Products Co., Ltd., diatomaceous earth with an average particle size of 5μm purchased from Guangzhou Dewei Chemical Co., Ltd., water glass purchased from Hubei Xinrunde Chemical Co., Ltd. (purity 99%), styrene-acrylic emulsion purchased from Shandong Yilai New Materials Technology Development Co., Ltd. (purity: 46-48%), and all reagents used are commonly available on the market.

[0024] Example 1

[0025] A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment comprises, by weight, 60 parts of fused white corundum powder, 8 parts of zirconium oxide micropowder, 8 parts of chromium oxide micropowder, 7 parts of aluminum oxide micropowder, 15 parts of metakaolin, 8 parts of diatomaceous earth modified by iron oxide hydroxide, and 6 parts of modified water glass.

[0026] The preparation process of diatomite modified with ferric oxyhydroxide is as follows: ferric chloride hexahydrate and ammonium bicarbonate are mixed in anhydrous ethanol, and diatomite raw soil is added thereto, the mixture is sealed, stirred at a speed of 120 r / min at room temperature for 8 hours, and then filtered, the filtrate is placed in a vacuum drying oven, dried at 55° C. for 8 hours, and then ground through an 80-mesh sieve to obtain diatomite modified with ferric chloride hexahydrate; wherein the molar ratio of ferric chloride hexahydrate to ammonium bicarbonate is 3:8, the amount of ferric chloride hexahydrate in anhydrous ethanol is 0.025 g / mL, and the amount of diatomite in anhydrous ethanol is 0.04 g / mL.

[0027] The preparation process of modified water glass is as follows: placing water glass in a container and adding sodium tetraborate thereto, stirring at a speed of 450 r / min for 40 minutes to obtain a stable solution, namely the modified water glass; wherein the mass ratio of sodium tetraborate to water glass is 0.1:20.

[0028] A method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment, the preparation process is:

[0029] S1. Weigh the raw materials according to the above weight proportions and set aside. Soak the diatomaceous earth modified with iron oxyhydroxide in modified water glass for 20 minutes to obtain slurry A.

[0030] S2, mixing the metakaolin with the slurry A obtained in step S1 and stirring in a stirrer, stirring at a speed of 90 r / min for 6 min and then changing the speed to 180 r / min for 5 min, then adding styrene acrylic emulsion and silane coupling agent KH550, stirring at a speed of 180 r / min for 6 min to obtain slurry B; wherein the mass ratio of styrene acrylic emulsion, silane coupling agent KH550 and metakaolin is 1:0.35:100;

[0031] S3, placing the fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder and the slurry B obtained in step S2 in a mixer and uniformly mixing them to obtain a mud material;

[0032] S4, pressing the mud obtained in step S3 into a brick by a press and then drying it in a dryer; wherein the drying process is: heating the temperature to 100°C at a heating rate of 5°C / h and then heating the temperature to 180°C at a heating rate of 3°C / h, and drying until the residual dry moisture inside the brick is 1%;

[0033] S5. Load the qualified bricks after drying in step S4 into the high-temperature tunnel kiln, and select the finished products after high-temperature firing and heat preservation; wherein, the high-temperature firing temperature is 1500° C. and the heat preservation is 8 hours.

[0034] Example 2

[0035] A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment. The corundum brick comprises, by weight, 55 parts of fused white corundum powder, 6 parts of zirconium oxide micropowder, 6 parts of chromium oxide micropowder, 6 parts of aluminum oxide micropowder, 12 parts of metakaolin, 5 parts of diatomaceous earth modified by iron oxide hydroxide, and 4 parts of modified water glass.

[0036] The preparation process of diatomite modified by ferric oxyhydroxide is as follows: ferric chloride hexahydrate and ammonium bicarbonate are mixed in anhydrous ethanol, and diatomite raw soil is added thereto, sealed, stirred at a speed of 100 r / min at room temperature for 6 hours, and then filtered, the filtrate is placed in a vacuum drying oven and dried at 50°C for 6 hours, and then ground through an 80-mesh sieve to obtain diatomite modified by ferric chloride hexahydrate; wherein the molar ratio of ferric chloride hexahydrate to ammonium bicarbonate is 1:4, the amount of ferric chloride hexahydrate in anhydrous ethanol is 0.02 g / mL, and the amount of diatomite in anhydrous ethanol is 0.03 g / mL.

[0037] The preparation process of modified water glass is as follows: placing water glass in a container and adding sodium tetraborate thereto, stirring at a speed of 400 r / min for 20 minutes to obtain a stable solution, namely the modified water glass; wherein the mass ratio of sodium tetraborate to water glass is 0.1:15.

[0038] A method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment, the preparation process is:

[0039] S1. Weigh the raw materials according to the above weight proportions and set aside. Soak the diatomaceous earth modified with iron oxyhydroxide in modified water glass for 10 minutes to obtain slurry A.

[0040] S2, mixing the metakaolin with the slurry A obtained in step S1 and stirring in a stirrer, stirring at a speed of 80 r / min for 4 min and then changing the speed to 150 r / min and stirring for 3 min, then adding styrene acrylic emulsion and silane coupling agent KH550, stirring at a speed of 150 r / min for 5 min to obtain slurry B; wherein the mass ratio of styrene acrylic emulsion, silane coupling agent KH550 and metakaolin is 0.8:0.3:100;

[0041] S3, placing the fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder and the slurry B obtained in step S2 in a mixer and uniformly mixing them to obtain a mud material;

[0042] S4, pressing the mud obtained in step S3 into a brick by a press and then placing it in a dryer for drying; wherein the drying process is: heating the temperature to 100°C at a heating rate of 5°C / h and then heating the temperature to 180°C at a heating rate of 3°C / h, and drying until the residual dry moisture inside the brick is 3%;

[0043] S5. Load the qualified bricks after drying in step S4 into the high-temperature tunnel kiln, and select the finished products after high-temperature firing and heat preservation; wherein, the high-temperature firing temperature is 1450°C and the heat preservation is 6 hours.

[0044] Example 3

[0045] A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment. The corundum brick comprises, by weight, 75 parts of fused white corundum powder, 10 parts of zirconium oxide powder, 10 parts of chromium oxide powder, 8 parts of aluminum oxide powder, 16 parts of metakaolin, 9 parts of diatomaceous earth modified by iron oxide hydroxide, and 7 parts of modified water glass.

[0046] The preparation process of diatomite modified by ferric oxyhydroxide is as follows: ferric chloride hexahydrate and ammonium bicarbonate are mixed in anhydrous ethanol, and diatomite raw soil is added thereto, the mixture is sealed, stirred at a speed of 150 r / min at room temperature for 8 hours, and then filtered, the filtrate is placed in a vacuum drying oven, dried at 60° C. for 8 hours, and then ground through an 80-mesh sieve to obtain diatomite modified by ferric chloride hexahydrate; wherein the molar ratio of ferric chloride hexahydrate to ammonium bicarbonate is 3:10, the amount of ferric chloride hexahydrate in anhydrous ethanol is 0.03 g / mL, and the amount of diatomite in anhydrous ethanol is 0.05 g / mL.

[0047] The preparation process of modified water glass is as follows: placing water glass in a container and adding sodium tetraborate thereto, stirring at a speed of 500 r / min for 40 minutes to obtain a stable solution, namely the modified water glass; wherein the mass ratio of sodium tetraborate to water glass is 0.1:25.

[0048] A method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment, the preparation process is:

[0049] S1. Weigh the raw materials according to the above weight proportions and set aside. Soak the diatomaceous earth modified with iron oxyhydroxide in modified water glass for 20 minutes to obtain slurry A.

[0050] S2, mixing the metakaolin with the slurry A obtained in step S1 and stirring in a stirrer, stirring at a speed of 100 r / min for 8 min, then changing the speed to 200 r / min and stirring for 5 min, then adding styrene acrylic emulsion and silane coupling agent KH550, stirring at a speed of 200 r / min for 8 min to obtain slurry B; wherein the mass ratio of styrene acrylic emulsion, silane coupling agent KH550 and metakaolin is 1.5:0.4:100;

[0051] S3, placing the fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder and the slurry B obtained in step S2 in a mixer and uniformly mixing them to obtain a mud material;

[0052] S4, pressing the mud obtained in step S3 into a brick by a press and then placing it in a dryer for drying; wherein the drying process is: heating the temperature to 100°C at a heating rate of 5°C / h and then heating the temperature to 180°C at a heating rate of 3°C / h, and drying until the residual dry moisture inside the brick is 5%;

[0053] S5. Load the qualified bricks after drying in step S4 into the high-temperature tunnel kiln, and select the finished products after high-temperature firing and heat preservation; wherein, the high-temperature firing temperature is 1550°C and the heat preservation is 8h.

[0054] Comparative Example 1

[0055] Compared with Example 1, in this comparative example, the diatomaceous earth is not modified in the raw material components, and the original diatomaceous earth is directly added, and the rest is the same as Example 1.

[0056] Comparative Example 2

[0057] Compared with Example 1, in this comparative example, water glass is not modified in the raw material components, and water glass is directly added, and the rest is referred to Example 1.

[0058] Comparative Example 3

[0059] Compared with Example 1, in this comparative example, diatomaceous earth and water glass are not modified in the raw material components, and the original diatomaceous earth and water glass are directly added.

[0060] Comparative Example 4

[0061] A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment comprises, by weight, 60 parts of fused white corundum powder, 8 parts of zirconium oxide micropowder, 8 parts of chromium oxide micropowder, 7 parts of aluminum oxide micropowder, 15 parts of metakaolin, 8 parts of diatomaceous earth, and 6 parts of water glass.

[0062] A method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment, the preparation process is:

[0063] S1. The raw materials are weighed according to the above weight parts and placed in a mixer and mixed evenly to obtain a mud material;

[0064] S2, pressing the mud obtained in step S1 into a brick by a press and then placing it in a dryer for drying; wherein the drying process is: heating the temperature to 100°C at a heating rate of 5°C / h and then heating the temperature to 180°C at a heating rate of 3°C / h, and drying until the residual dry moisture inside the brick is 1%;

[0065] S3, loading the qualified bricks after drying in step S2 into the high-temperature tunnel kiln, and selecting the finished products after high-temperature firing and heat preservation; wherein, the high-temperature firing temperature is 1500°C and the heat preservation is 8h.

[0066] Related tests

[0067] The performance of the corundum bricks prepared in Examples 1-3 and Comparative Examples 1-4 was tested, and the test results are shown in Table 1.

[0068] Table 1 Product performance test results

[0069]

[0070] The room temperature compressive strength and apparent porosity of the prepared products were tested with reference to GB / T5072-2008 and GB / T 2997-2000. The thermal shock stability times were measured by the following method: a sample with a size of 20 cm×10 cm×10 cm was heated to 1500°C in a heating furnace for 15 min, then taken out and cooled in air for 15 min, and the cycle was repeated until cracks were observed with the naked eye. The cycle number was counted as the thermal shock stability times. Corrosion resistance test: the products prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to For the corrosion resistance test, a crucible sample with a size of φ50mm×50mm and an inner hole size of φ22mm×18mm was made. A static corrosion resistance test method was adopted, and 20g of ladle slag was filled in the crucible sample. The sample was placed in a carbon-buried atmosphere and kept warm at 1500℃ for 3h. After the furnace was cooled, the crucible was cut open in the height direction, and the invasion (penetration) area S of the central section of the crucible was measured. The corrosion index S / S0×100% (S0 is the cross-sectional area of ​​the original crucible center hole) was calculated to evaluate the corrosion resistance of the sample.

[0071] It can be seen from the test results in Table 1 that the test results of Examples 1-3 are better than the test results of Comparative Examples 1-4. By comparing Example 1 with Comparative Examples 1-3, it can be seen that the addition of diatomaceous earth modified with ferric oxyhydroxide and water glass modified with sodium tetraborate can improve the performance of the product, and the simultaneous addition of the two can further improve the performance of the product; by comparing Example 1 with Comparative Example 4, it can be seen that compared with directly mixing the raw materials, the addition of modified diatomaceous earth, water glass and metakaolin can form a more stable three-dimensional structure during the preparation process, thereby obtaining a product with better performance.

[0072] In the present invention, ferric chloride hexahydrate and ammonium bicarbonate are reacted to generate ferric hydroxide to modify diatomite. Diatomite, as a biological siliceous sedimentary rock, has the characteristics of high chemical stability, light bulk density, low thermal conductivity and good thermal insulation effect. Ferric hydroxide has a good chemical state. The dispersibility of diatomite can be improved by loading ferric hydroxide on diatomite, and a large number of hydroxyl groups are introduced on the surface of diatomite. Further, the hydroxyl groups on the surface of diatomite form chemical bonds with the Si-OH groups contained in the modified water glass in the raw material, so that a good interface bonding is formed therebetween. In the mixing preparation process, the Si-OH bonds are mutually dehydrated and associated to form Si-O-Si bonds, forming a stable three-dimensional structure. Further, sodium tetraborate is added to the water glass, and boron will be present in the form of Boron-oxygen tetrahedrons enter the Si-O-Si network to form a Si-OB network structure, and the presence of chain and cyclic Si-OT (Si, B) structures makes the matrix structure of the material more compact, which is beneficial to the improvement of the compressive strength of the product; at the same time, water glass can be used as an alkali activator in the mixing process, and reacts with kaolin mixed with styrene acrylic emulsion and silane coupling agent to form a kaolin-based polymer with a stable three-dimensional network structure, in which the presence of styrene acrylic emulsion and silane coupling agent can absorb part of the load through their own plastic deformation, thereby further improving the mechanical properties of the prepared product; in addition, in the preparation process, the bricks are dried by adopting constant-speed drying and decelerated drying methods to ensure that the bricks have the maximum safe drying rate and avoid capillary cracks in the bricks during the drying process.

[0073] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0074] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.

Claims

1. A low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment, characterized in that: The corundum brick comprises, by weight, 55-75 parts of fused white corundum powder, 6-10 parts of zirconium oxide powder, 6-10 parts of chromium oxide powder, 6-8 parts of aluminum oxide powder, 12-16 parts of metakaolin, 5-9 parts of diatomaceous earth modified by iron oxyhydroxide, and 4-7 parts of modified water glass; The preparation process of the ferric oxyhydroxide modified diatomaceous earth is as follows: ferric chloride hexahydrate and ammonium bicarbonate are mixed in anhydrous ethanol, and diatomaceous earth is added thereto, the mixture is sealed, stirred evenly at room temperature, and then filtered by suction, and the filtrate is dried, ground, and sieved to obtain the ferric oxyhydroxide modified diatomaceous earth; The preparation process of the modified water glass is as follows: placing water glass in a container and adding sodium tetraborate therein, and stirring the container to obtain a stable solution, namely the modified water glass.

2. The low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment according to claim 1 is characterized in that: During the preparation of the iron oxyhydroxide modified diatomaceous earth, stirring is performed at room temperature for 6-8 hours at a stirring speed of 100-150 r / min.

3. The low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment according to claim 1, characterized in that: The drying conditions during the preparation of the iron oxyhydroxide modified diatomaceous earth are: drying in a vacuum drying oven at 50-60° C. for 6-8 hours.

4. The low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment according to claim 1, characterized in that: During the preparation process of the iron oxyhydroxide modified diatomaceous earth, the diatomaceous earth is ground and sieved to a 80-mesh sieve.

5. The low thermal conductivity chromium-zirconium corundum brick for hazardous waste treatment according to claim 1, characterized in that: During the preparation of the modified water glass, the stirring conditions are: 400-500 r / min, stirring for 20-40 min.

6. The method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment according to any one of claims 1 to 5, characterized in that: The preparation process is: S1. Weigh the raw materials according to the above weight proportions and set aside. Soak the diatomaceous earth modified with iron oxyhydroxide in modified water glass for 10-20 minutes to obtain slurry A. S2, mixing the metakaolin with the slurry A obtained in step S1, stirring in a mixer, then adding styrene acrylic emulsion and silane coupling agent, and continuing stirring to obtain slurry B; S3, placing the fused white corundum powder, zirconium oxide powder, chromium oxide powder, aluminum oxide powder and the slurry B obtained in step S2 in a mixer and uniformly mixing them to obtain a mud material; S4, pressing the clay obtained in step S3 into a brick by a press and then placing it in a dryer for drying; S5, loading the qualified bricks after drying in step S4 into a kiln car and entering a high-temperature tunnel kiln, and after high-temperature firing and heat preservation, the finished products are selected.

7. The method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment according to claim 6, characterized in that: The stirring conditions in step S2 are as follows: after the metakaolin is mixed with the slurry A obtained in step S1, the mixture is stirred at a speed of 80-100 r / min for 4-8 min in a mixer, and then the speed is changed to 150-200 r / min and stirred for 3-5 min. After the styrene acrylic emulsion and the silane coupling agent are added, the mixture is stirred at a speed of 150-200 r / min for 5-8 min.

8. The method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment according to claim 6, characterized in that: The drying standard in step S4 is: drying until the residual dry moisture inside the brick is 1-5%.

9. The method for preparing low thermal conductivity chromium-zirconium corundum bricks for hazardous waste treatment according to claim 6, characterized in that: The high temperature firing temperature in step S5 is 1450-1550° C. and the temperature is kept for 6-8 hours.

Citation Information

Patent Citations

  • High-toughness modified silicon corundum brick

    CN113526946A

  • Acid-resistant and salt-resistant modified corundum brick for rotary kiln of hazardous waste incineration system and preparation method thereof

    CN116102343A

  • Zirconium-containing corundum spinel brick for hazardous waste disposal equipment and preparation method thereof

    CN111995379A

  • Corundum micro-nano pore heat insulation refractory material and preparation method thereof

    CN114105676A

  • Method for producing alumina-chromia fired brick

    JP2017206414A

Cited By

  • Thermal shock resistant refractory material for melting furnace and preparation method of thermal shock resistant refractory material

    CN120757389A

  • Thermal shock resistant refractory for fusion furnaces and method for producing the same

    CN120757389B