Method for preparing methoxycresol based on Co-Cu bimetallic catalyst

By using the Co-Cu bimetallic nanoparticle catalyst prepared by using ZIF-67 template in the vanillin hydrodeoxygenation reaction, the problems of high cost of noble metal catalysts and unsatisfactory activity of non-noble metal catalysts were solved, and efficient and low-cost methanol was achieved. Oxycresol preparation and catalyst recycling.

CN118791369APending Publication Date: 2024-10-18QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411056271.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the prior art, the catalysts used in the vanillin hydrodeoxygenation reaction are usually precious metals, which have high costs and scarce reserves. The preparation process of non-precious metal catalysts is complex and time-consuming and has unsatisfactory catalytic activity, which limits large-scale application.

Method used

A Co-Cu bimetallic nanoparticle catalyst using ZIF-67 as a template was prepared through enzymatic hydrolysis of lignin, microwave one-pot solvothermal method and argon carbothermal reduction method to form a lignin-based carbon wrapped outside the regular structure of ZIF. balls to achieve high dispersion and synergy of Co-Cu bimetallic catalysts.

Benefits of technology

It achieves efficient and highly selective conversion of vanillin into methoxycresol under mild conditions, and the catalyst can be recycled, reducing production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791369A_ABST
    Figure CN118791369A_ABST
Patent Text Reader

Abstract

The invention relates to a method for catalyzing vanillin hydrodeoxygenation reaction by non-noble bimetallic nanoparticles based on a biomass charcoal carrier, in particular to a method for preparing methoxycresol by catalyzing vanillin water-phase selective hydrodeoxygenation by adopting Co-Cu bimetallic nanoparticles based on ZIF-based lignin carbon spheres, and belongs to the technical field of biomass catalytic conversion. According to the preparation method, an industrial byproduct enzymatic hydrolysis lignin resource which is low in cost and easy to obtain is adopted as a carbon source material, ZIF-67 which has a good carbon framework template effect, is high in metal content and contains nitrogen is adopted as a precursor, a nitrogen-containing carbon sphere carrier which has a stable and high-dispersion effect on metal is constructed, and a second metal Cu is introduced to form a bimetal center; therefore, efficient directional catalytic conversion from vanillin to methoxycresol under mild conditions is realized. According to the method, a renewable enzymatic hydrolysis lignin resource is taken as a matrix, non-noble metals Co and Cu are taken as active centers, a catalytic system is constructed by combining microwave solvothermal one-pot synthesis and an argon carbon thermal reduction method, and high-temperature hydrogen reduction or a chemical reducing agent is not needed; the method can convert another lignin-based platform compound to a higher value-added direction with excellent activity and selectivity, is low in cost, high in efficiency and clean in process, and is a green catalytic process for taking lignin and using the lignin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for efficiently preparing cresol by hydrodeoxygenation of vanillin catalyzed by a non-precious bimetallic catalyst, specifically a method for preparing cresol by hydrodeoxygenation of vanillin in an aqueous phase catalyzed by Co-Cu bimetallic nanoparticles based on ZIF-based lignin carbon balls, belonging to the technical field of biomass catalytic conversion. Background Art

[0002] With the continuous reduction of fossil energy reserves, it is urgent to find more environmentally friendly renewable energy and resources. Lignin, as a natural macromolecular renewable resource containing an aromatic ring structure, has the characteristics of high carbon content, good thermal stability, and rich functional groups such as hydroxyl, carboxyl, carbonyl and methoxyl. However, it is far from being fully utilized. Most of it is discarded or used as low-grade fuel or concrete additive, causing environmental pollution and waste of resources. Therefore, the high-value utilization and deep processing of lignin resources are hot topics in biomass conversion research. Among them, methoxycresol (MMP), which has important application value in the fields of fuel, medicine and fragrance intermediates, can be prepared by selective hydrogenation and deoxygenation of vanillin (VL), a typical platform compound derived from lignin. However, in the prior art, the catalysts used in this process often use precious metals as active centers, which are expensive and scarce, thus limiting the prospects for large-scale application (Industrial Crops and Products, 2023, 192: 116055; Applied Catalysis A: General, 2018, 561: 137-149; RSC Advances, 2016, 6(73): 69045-69051; Green Chemistry, 2022, 24(24): 9489-9495). However, the development of non-precious metal catalysts often has problems such as complex and time-consuming preparation process, high energy consumption, high-temperature hydrogen reduction and unsatisfactory catalytic activity (Catalysis Science & Technology, 2022, 12(16): 5178-5188; Fuel, 2022, 318: 123694; RSC Advances, 2021, 11(18): 10996-11003; Journal of Industrial and Engineering Chemistry, 2024, 131: 653-661).

[0003] The present invention utilizes the characteristics of lignin resources with high carbon content aromatic ring macromolecular structure, adopts the strategy of using molecular sieve imidazole skeleton ZIF-67 as template and industrial by-product enzymatic lignin as carbon source to prepare catalyst carrier (ACSSustainable Chemistry & Engineering, 2019, 7 (19): 16585-16594), and provides a method for preparing methoxycresol by catalyzing vanillin aqueous phase hydrodeoxygenation using Co-Cu bimetallic nanoparticles. It is characterized in that ZIF-67 is used as a precursor, nitrogen source and metal Co source at the same time, enzymatic lignin is used as a carbon source precursor, and a second metal Cu is introduced, and a highly dispersed Co-Cu bimetallic catalyst anchored by lignin-based carbon balls wrapped outside the regular structure of ZIF is prepared by a one-pot method. Based on the high metal content and good carbon framework template effect of ZIF-67, the stable and high dispersion effect of the obtained nitrogen-containing carbon balls on metals, the good performance of Co-based and Cu-based active centers in hydrodeoxygenation reactions, and the synergistic effect of bimetallic centers (International Journal of Hydrogen Energy, 2020, 45(56): 31440-31451; ACSCatalysis, 2020, 10(15): 8672-8682; ChemSusChem, 2017, 10(9): 1892-1897; Small, 2018, 14(36): 1801953; Chemical Engineering Journal, 2023, 473: 145375; Fuel Processing Technology, 2023, 247: 107764), the catalyst exhibits extremely high catalytic activity and selectivity in the hydrodeoxygenation of vanillin to produce cresol. At the same time, the preparation of the Co-Cu bimetallic catalyst provided by the present invention adopts microwave solvent thermal one-pot synthesis and argon carbon thermal reduction method, which is simple and clean to operate. The present invention promotes the effective utilization of lignin resources from the two perspectives of the development of new catalytic materials and the efficient preparation of high value-added chemicals. It is a new green method of "taking lignin and using lignin". So far, there has been no relevant report on the application of Co-Cu bimetallic catalyst materials based on ZIF-based lignin carbon balls in catalytic hydrodeoxygenation reactions at home and abroad. Summary of the invention

[0004] The purpose of the present invention is to provide a catalytic method for preparing methoxycresol by hydrogenation deoxygenation reaction of vanillin with low cost, high efficiency, mild conditions and catalyst recyclability, using enzymatic lignin, 2-methylimidazole, cobalt nitrate and copper nitrate as raw materials, combined with microwave one-pot solvothermal method and argon carbon thermal reduction method to prepare Co-Cu bimetallic nanoparticles based on ZIF-based lignin carbon balls as catalysts, and providing a preparation process of the catalyst.

[0005] In the catalyst preparation process of the present invention, during the microwave one-pot solvothermal synthesis, the enzymatically hydrolyzed lignin is wrapped around the regular structure of ZIF-67 with Co as the central ion to form a spherical morphology, and the morphology is maintained during the carbonization process; at the same time, Co and Cu migrate to the surface of the carbon ball to achieve good dispersion, and undergo carbon reduction to form a synergistic catalytic active center, thereby presenting efficient and highly selective catalytic characteristics for the hydrogenation and deoxygenation reaction of vanillin.

[0006] The technical solution of the present invention is:

[0007] The catalyst Co-Cu / NC ZIF@EL The raw material vanillin is placed in a flange kettle, with 40g of catalyst per mole of vanillin, and deionized water is added as the reaction solvent at a ratio of 10L of water per mole of vanillin. The air in the kettle is replaced with H2, and then 1.0-1.5MPa of H2 is filled in. The reaction is carried out at a reaction temperature of 125-150°C and stirred at 400rpm for 6-7h. After the reaction is completed, the catalyst is separated by magnetic force or centrifugation, and the liquid product is extracted with ethyl acetate and dried and then quantitatively analyzed by gas chromatography.

[0008] The catalyst described in the above technical solution is a Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls. ZIF@EL , and its preparation method is:

[0009] Co(NO3)2·6H2O and Cu(NO3)2·3H2O in a molar ratio of 3:1 or 4:1 were mixed, and stirred at a ratio of 50 mL methanol per millimole of metal salt until completely dissolved to prepare solution A. 2-Methylimidazole was dissolved at a ratio of 37.6 mmol / 50 mL methanol to prepare solution B. Solution A and solution B were mixed in equal volumes, and then enzymatic lignin was added at a ratio of 1.0 g per millimole of metal salt. After ultrasonic dissolution, the mixture was placed in a microwave reactor and reacted at 150°C for 4 h. The solid product was centrifuged, washed with methanol and vacuum dried. In an argon atmosphere, the temperature was raised to 200°C at a rate of 10°C / min and maintained for 5 min. Then, the temperature was raised to 600°C at a rate of 10°C / min and calcined for 2 h. After cooling, the mixture was ground to obtain Co-Cu / NC ZIF@EL catalyst.

[0010] The method for preparing methoxycresol by aqueous phase hydrodeoxygenation of vanillin using Co-Cu bimetallic nanoparticle catalyst based on ZIF-based lignin carbon balls provided by the present invention has the following characteristics compared with the prior art:

[0011] (1) The method provided by the present invention uses ZIF-67 as a precursor to encapsulate enzymatic lignin and simultaneously introduce the second metal Cu, which can simultaneously obtain the stable high dispersion and synergistic effect of nitrogen-containing carbon balls on the Co and Cu bimetallic centers, thereby achieving extremely high catalytic activity and selectivity.

[0012] (2) The preparation of the Co-Cu bimetallic nanoparticle catalyst provided by the present invention adopts a microwave solvent thermal one-pot synthesis and an argon carbon thermal reduction method, which does not require high-temperature hydrogen reduction or chemical reducing agents, has low cost, high efficiency, and a simple and clean process.

[0013] (3) Co-Cu / NC provided by the present invention ZIF@EL The catalytic vanillin aqueous phase hydrodeoxygenation method can efficiently and selectively convert vanillin into the target product methoxycresol under relatively mild reaction conditions without generating other by-products. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Attached Figure 1 The Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls prepared in Example 1 ZIF@EL TEM images and particle size distribution.

[0015] Attached Figure 2 The Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls prepared in Example 1 ZIF@EL XRD spectrum of .

[0016] Attached Figure 3 The Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls prepared in Example 1 ZIF@EL XPS score.

[0017] Attached Figure 4 The Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls prepared in Example 1 ZIF@EL XPS Co2p fine map.

[0018] Attached Figure 5 The Co-Cu bimetallic nanoparticle catalyst Co-Cu / NC based on ZIF-based lignin carbon balls prepared in Example 1 ZIF@EL XPS Cu2p fine map. DETAILED DESCRIPTION

[0019] The following examples are used to further illustrate the present invention, but are not intended to limit the present invention.

[0020] [Example 1]

[0021] 0.4mmol Co(NO3)2·6H2O and 0.1mmol Cu(NO3)2·3H2O were mixed and completely dissolved in 25mL methanol, and quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g enzymatic lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol, vacuum dried, and heated to 200℃ at a rate of 10℃ / min in an argon atmosphere for 5min, and then heated to 600℃ at a rate of 10℃ / min for calcination for 2h. After cooling, it was ground to obtain Co-Cu / NC ZIF@EL Ⅰ catalyst.

[0022] [Example 2]

[0023] 0.375mmol Co(NO3)2·6H2O and 0.125mmol Cu(NO3)2·3H2O were mixed and completely dissolved in 25mL methanol, and quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g enzymatic lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol, vacuum dried, and heated to 200℃ at a rate of 10℃ / min in an argon atmosphere for 5min, and then heated to 600℃ at a rate of 10℃ / min for calcination for 2h. After cooling, it was ground to obtain Co-Cu / NC ZIF@EL Ⅱ catalyst.

[0024] [Example 3]

[0025] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL Ⅰ The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0026] [Example 4]

[0027] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL ⅡThe catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0028] [Example 5]

[0029] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL Ⅰ The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.5 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0030] [Example 6]

[0031] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL Ⅰ The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 125 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0032] [Example 7]

[0033] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL Ⅰ The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 130 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0034] [Example 8]

[0035] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL ⅠThe catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 150 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0036] [Example 9]

[0037] Take 40 mg of Co-Cu / NC prepared in Example 1 ZIF@EL Ⅰ The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 130 ° C for 7 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 1.

[0038] Table 1 Co-Cu / NC ZIF@EL Catalytic performance of hydrodeoxygenation of vanillin to produce cresols

[0039]

[0040] [Examples 10-13] Co-Cu / NC ZIF@EL Ⅰ Recycling performance of catalyst in hydrodeoxygenation of vanillin

[0041] The solid catalyst recovered after the reaction in Example 7 was ultrasonically washed three times with anhydrous ethanol and vacuum dried, and then added to a flange reactor together with 152 mg of vanillin and 10 mL of deionized water. The air in the reactor was replaced with H2 and then filled with 1.0 MPa H2. The reaction was carried out at 130°C for 6 hours under stirring conditions of 400 rpm. After the reaction was completed, the solid catalyst was separated by magnetic force and the above steps were repeated. The mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatograph. The results of the catalyst recycling four times are shown in Table 2.

[0042] Table 2 Co-Cu / NC ZIF@EL Ⅰ Catalyst recycling performance

[0043]

[0044] [Comparative Example 1]

[0045] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g enzymatic lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, the temperature was increased to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. Then, the temperature was increased to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, it was ground to obtain Co / NC ZIF@EL catalyst.

[0046] Take 40 mg of the Co / NC prepared above ZIF@EL The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0047] [Comparative Example 2]

[0048] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g sodium lignin sulfonate was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, the temperature was increased to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. Then, the temperature was increased to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, it was ground to obtain Co / NC ZIF@SLS catalyst.

[0049] Take 40 mg of the Co / NC prepared above ZIF@SLS The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0050] [Comparative Example 3]

[0051] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g alkali lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, the temperature was increased to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. Then, the temperature was increased to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, it was ground to obtain Co / NC ZIF@AL catalyst.

[0052] Take 40 mg of the Co / NC prepared above ZIF@AL The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0053] [Comparative Example 4]

[0054] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.5g dealkalized lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, the temperature was increased to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. Then, the temperature was increased to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, it was ground to obtain Co / NC ZIF@DL catalyst.

[0055] Take 40 mg of the Co / NC prepared above ZIF@DL The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0056] [Comparative Example 5]

[0057] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, and mixed rapidly with 25mL methanol containing 1.54g 2-methylimidazole and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, the temperature was increased to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. Then, the temperature was increased to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, the Co / NC was ground. ZIF catalyst.

[0058] Take 40 mg of the Co / NC prepared above ZIF The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0059] [Comparative Example 6]

[0060] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 0.2g enzymatic lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol. After vacuum drying, it was heated to 200℃ at a rate of 10℃ / min in an argon atmosphere and maintained for 5min. It was then heated to 600℃ at a rate of 10℃ / min and calcined for 2h. After cooling, it was ground to obtain Co / NC ZIF@EL0.2 catalyst.

[0061] Take 40 mg of the Co / NC prepared above ZIF@EL0.2 The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0062] [Comparative Example 7]

[0063] 0.5mmol Co(NO3)2·6H2O was completely dissolved in 25mL methanol, quickly mixed with 25mL methanol containing 1.54g 2-methylimidazole, and 1.0g enzymatic lignin was added and ultrasonicated for 15min. The mixture was transferred to a microwave reactor and reacted at 150℃ for 4h. The solid product was centrifuged and washed with methanol, vacuum dried, and heated to 200℃ at a rate of 10℃ / min in an argon atmosphere for 5min, and then heated to 600℃ at a rate of 10℃ / min for calcination for 2h. After cooling, it was ground to obtain Co / NC ZIF@EL1.0 catalyst.

[0064] Take 40 mg of the Co / NC prepared above ZIF@EL1.0 The catalyst and 152 mg of vanillin were placed in a flange reactor, and 10 mL of deionized water was added. The air in the reactor was replaced with H2, and then 1.0 MPa of H2 was filled in. The reaction was carried out at 140 ° C for 6 h under stirring conditions of 400 rpm. After the reaction, the solid catalyst was separated by magnetic force, the mixed solution was extracted with ethyl acetate, and the dried supernatant was quantitatively analyzed by gas chromatography. The catalytic reaction results are shown in Table 3.

[0065] Table 3 Performance of Co nanoparticles catalyzed hydrodeoxygenation of vanillin based on ZIF-based lignin carbon balls

[0066]

Claims

1. A method for hydrodeoxygenation of vanillin catalyzed by Co-Cu bimetallic nanoparticles based on ZIF-based lignin carbon balls, characterized in that: During the microwave one-pot solvothermal synthesis, enzymatic lignin was wrapped around the regular structure of ZIF-67 to form a spherical morphology. During the argon carbon thermal reduction, Co and Cu migrated to the surface of the carbon balls to achieve good dispersion. The prepared Co-Cu bimetallic nanoparticle catalyst catalyzed the hydrodeoxygenation of vanillin to produce cresol in water phase. The preparation method of the Co-Cu bimetallic nanoparticles based on ZIF-based lignin carbon balls is as follows: Co(NO3)2·6H2O and Cu(NO3)2·3H2O are mixed at a molar ratio of 3:1 or 4:1, stirred at a ratio of 50 mL methanol per millimole of metal salt until completely dissolved to prepare solution A, 2-methylimidazole is dissolved at a ratio of 37.6 mmol / 50 mL methanol to prepare solution B, solution A and solution B are mixed in equal volumes, and then enzymatic lignin is added at a ratio of 1.0 g per millimole of metal salt, and then ultrasonically dissolved and placed in a microwave reactor at 150°C for 4 hours, the solid product is centrifuged and washed with methanol and vacuum dried, and heated to 200°C at a rate of 10°C / min in an argon atmosphere and maintained for 5 minutes, and then heated to 600°C at a rate of 10°C / min for calcination for 2 hours, and then ground after cooling to obtain the Co-Cu bimetallic nanoparticle catalyst based on ZIF-based lignin carbon balls; The method for preparing methoxycresol by hydrodeoxygenation of vanillin is as follows: raw material vanillin, catalyst and solvent water are added into a flange kettle at a ratio of 40g catalyst and 10L water per mole of vanillin, the air in the kettle is replaced by H2 and then 1.0-1.5MPa H2 is filled in, the reaction is carried out at a reaction temperature of 125-150°C and 400rpm stirring for 6-7h, after the reaction is completed, the catalyst is separated by magnetic force or centrifugation, and the mixed liquid is extracted with ethyl acetate to collect the product.

Citation Information

Cited By

  • Cobalt-zinc bimetal modified lignin-based catalyst as well as preparation method and application thereof

    CN122517036A