Preparation process of azelaic dinitrile
By using TS-1 carrier-loaded calcium and chromium catalyst in the azelonitrile preparation process, combined with beta zeolite and attapulgite, and optimizing the reaction conditions, the problems of complex existing processes and easy loss of catalysts were solved, and azelonitrile was achieved. The effects of high yield and long catalyst life improve the economy and application prospects of the process.
Patent Information
- Application Number
- CN202411282757.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing preparation process of azelonitrile is complicated, the dehydrating agent used is corrosive or the yield of nonanediamine is low, and the catalyst is easy to be lost, which affects the process efficiency and economy.
Use TS-1 as a carrier to load the active components calcium and chromium, combine beta zeolite and attapulgite, grind evenly, spray granulate and roast to prepare the catalyst, and react azelaic acid with ammonia in the presence of the catalyst to optimize the reaction conditions. Improve the yield of azelonitrile.
It significantly improves the yield of azelonitrile and the life of the catalyst, reduces the loss of chromium, has a simple process, wide sources of raw materials, and has good application prospects and economic value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fine chemicals and more specifically relates to a preparation process of azelaic acid. Background Art
[0002] Azelonitrile is an important chemical raw material that can be used to produce high-temperature nylon P9AT and can also be used in the pharmaceutical industry and other industries.
[0003] In the prior art, there are three main methods for producing azelaic acid: 1. Using azelaic acid (azedarioic acid) as a raw material, azodicarbonamide is obtained by ammoniation, and then dehydration is performed to prepare azelaic acid; 2. Using 1,9-dihalononane as a raw material, it is obtained by substitution reaction with inorganic cyanide; 3. Nonanediol is ammoniated and dehydrated to prepare azelaic acid.
[0004] CN106220513A discloses a method for preparing nonanediamine, which uses azelaic acid as a raw material, and sequentially undergoes neutralization reaction, dehydration reaction and decompression reaction to prepare azelonitrile, and azelonitrile is hydrogenated to prepare nonanediamine. Compared with the prior art, the present invention provides a process route with a simple process, high efficiency and yield, and uses renewable biomass resources as raw materials, which have a wide source, and the process is relatively simple and feasible, which has great social significance and economic value.
[0005] CN104945279A discloses a method for preparing dinitriles by ammoxidation of diols. The method uses one or two of air or oxygen as oxygen sources, and one or two of ammonia, ammonia water, urea, ammonium chloride, ammonium carbonate, ammonium sulfate, ammonium phosphate, ammonium hydrogen phosphate, and ammonium formate as nitrogen sources. Under catalytic action, the diols are ammoxidized to dinitriles. The ammoxidation efficiency of the present invention is high, and the product yield is high; air or oxygen is used as the oxygen source, which is economical and environmentally friendly; the product and the catalyst are separated, and the post-processing is simple; the catalyst is easy to reuse, and has a good application prospect.
[0006] However, the above preparation process is complicated, or the dehydrating agent used is highly corrosive, or the yield of nonanediamine is low. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a preparation process of azelaic acid. The process steps include the following steps: reacting azelaic acid with ammonia in the presence of a catalyst. The catalyst of the present invention uses TS-1 as a carrier, loads active components of calcium and cadmium, and then grinds and mixes with beta zeolite and attapulgite, sprays granulates, and roasts to obtain a catalyst. The obtained catalyst has excellent catalytic performance, long service life, and high yield of the target product.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A preparation process of azelaic acid, the process steps comprising the following steps:
[0010] Azelaic acid is reacted with ammonia in the presence of a catalyst.
[0011] Preferably, the reaction conditions are: the molar ratio of azelaic acid to ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-1.5 h -1 ; The reaction temperature is 350~450℃.
[0012] A preferred technical solution is that the method for preparing the catalyst comprises the following steps:
[0013] (1): Calcium salt, chromium salt and TS-1 are ultrasonically dispersed in deionized water, stirred for a certain period of time, evaporated to dryness, and then calcined to obtain product A;
[0014] (2) Grind the product A, β zeolite, attapulgite and an appropriate amount of water to obtain a slurry, spray granulate the slurry, and calcine the slurry to obtain a catalyst.
[0015] Preferably, in step (1), the stirring time is 30 to 50 minutes.
[0016] Preferably, in step (1), the evaporation temperature is 80°C; and the calcination is performed at 450-550°C for 2-4h.
[0017] Preferably, in step (1), the calcium salt is at least one of calcium acetate, calcium chloride and calcium nitrate.
[0018] Preferably, in step (1), the chromium salt is at least one of chromium acetate, chromium chloride and chromium nitrate.
[0019] Preferably, in step (1), the ratio of the calcium salt, the chromium salt and TS-1 is: 0.03~0.05mol:0.01~0.03mol:100g.
[0020] Preferably, in step (2), the mass ratio of the product A, β zeolite and attapulgite is 1:0.4-0.8:0.3-0.5; and the calcination treatment is performed at 500-600° C. for 5-9 hours.
[0021] Preferably, the azelaic acid is preheated before the reaction, and the preheating temperature is 220-240°C.
[0022] In the present invention, a preferred technical solution is a preparation process of azelaic acid nitrile, and the specific process steps are:
[0023] S1, taking 1 kg of catalyst to prepare a catalyst bed;
[0024] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;
[0025] S3, the azelaic acid feeder enters the preheating section after metering, and after preheating, enters the catalyst bed together with ammonia to react;
[0026] S4. The crude product is purified by distillation to obtain the product azelaic acid nitrile.
[0027] The present invention has the following beneficial effects:
[0028] (1) The present invention uses TS-1 as a carrier to load active components of calcium and chromium, and utilizes the interaction between the activated components to significantly improve the yield of azelaic acid;
[0029] (2) The catalyst obtained by mixing with β-zeolite and attapulgite, spray granulation and calcination not only reduces the loss of chromium, but also improves the life of the catalyst. The catalyst has higher activity and a higher yield of azelaic acid nitrile.
[0030] (3) The process of the present invention is simple, the raw material sources are wide, and the application prospects are good. DETAILED DESCRIPTION
[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0032] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0033] Example 1
[0034] A method for preparing a catalyst comprises the following steps:
[0035] (1) 0.04 mol calcium acetate, 0.02 mol chromium chloride and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 40 min, evaporated to dryness at 80 °C, and then calcined at 500 °C for 3 h to obtain product A;
[0036] (2) 100 g of product A, 60 g of β zeolite, 40 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 550°C for 7 h to obtain a catalyst.
[0037] Example 2
[0038] A method for preparing a catalyst comprises the following steps:
[0039] (1) 0.05 mol calcium chloride, 0.01 mol chromium nitrate and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 50 min, evaporated to dryness at 80 °C, and then calcined at 550 °C for 2 h to obtain product A;
[0040] (2) 100 g of product A, 80 g of β zeolite, 30 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 600°C for 5 h to obtain a catalyst.
[0041] Example 3
[0042] A method for preparing a catalyst comprises the following steps:
[0043] (1) 0.03 mol calcium nitrate, 0.03 mol chromium acetate and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 30 min, evaporated to dryness at 80 °C, and then calcined at 450 °C for 4 h to obtain product A;
[0044] (2) 100 g of product A, 40 g of β zeolite, 50 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 500°C for 9 h to obtain a catalyst.
[0045] Comparative Example 1
[0046] A method for preparing a catalyst comprises the following steps:
[0047] (1) 0.06 mol calcium acetate and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 40 min, evaporated to dryness at 80 °C, and then calcined at 500 °C for 3 h to obtain product A;
[0048] (2) 100 g of product A, 60 g of β zeolite, 40 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 550°C for 7 h to obtain a catalyst.
[0049] Comparative Example 2
[0050] A method for preparing a catalyst comprises the following steps:
[0051] (1) 0.06 mol chromium chloride and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 40 min, evaporated to dryness at 80 °C, and then calcined at 500 °C for 3 h to obtain product A;
[0052] (2) 100 g of product A, 60 g of β zeolite, 40 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 550°C for 7 h to obtain a catalyst.
[0053] Comparative Example 3
[0054] A method for preparing a catalyst comprises the following steps:
[0055] (1) 0.04 mol calcium acetate, 0.02 mol chromium chloride and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 40 min, evaporated to dryness at 80 °C, and then calcined at 500 °C for 3 h to obtain product A;
[0056] (2) Grind 100 g of product A, 100 g of β zeolite and an appropriate amount of water to obtain a slurry, spray granulate the slurry, and calcine the slurry at 550°C for 7 h to obtain a catalyst.
[0057] Comparative Example 4
[0058] A method for preparing a catalyst comprises the following steps:
[0059] (1) 0.04 mol calcium acetate, 0.02 mol chromium chloride and 100 g TS-1 were ultrasonically dispersed in 200 mL deionized water, stirred for 40 min, evaporated to dryness at 80 °C, and then calcined at 500 °C for 3 h to obtain product A;
[0060] (2) Grind 100 g of product A, 100 g of attapulgite and an appropriate amount of water to obtain a slurry, spray granulate the slurry, and calcine at 550°C for 7 h to obtain a catalyst.
[0061] Comparative Example 5
[0062] A method for preparing a catalyst comprises the following steps:
[0063] 160 g of β zeolite, 40 g of attapulgite and an appropriate amount of water were ground evenly to obtain a slurry, which was spray granulated and calcined at 550° C. for 7 h to obtain a catalyst.
[0064] The catalytic effects of Examples 1-3 and Comparative Examples 1-5 were tested. The specific test results are shown in Table 1, wherein the lifespans of Examples 1-3 and Comparative Examples 3-5 were tested.
[0065] A preparation process of azelaic acid, the specific process steps are:
[0066] S1, taking 1 kg of catalyst to prepare a catalyst bed;
[0067] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;
[0068] S3, the azelaic acid feeder enters the preheating section after metering, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 230°C; the reaction conditions of the reaction are that the molar ratio of azelaic acid to ammonia is 1:10; the reaction pressure is 2.5Mpa, and the raw material space velocity is 0.8h-1 ; The reaction temperature is 400°C;
[0069] S4. The crude product is purified by distillation to obtain the product azelaic acid nitrile.
[0070] Table 1:
[0071]
[0072] It can be seen from Table 1 that the active components loaded in the present invention and the raw materials interact with each other. Under the presence of the joint action, the catalyst has a long life and excellent catalytic activity, and the yield of azelaic acid is above 98%.
[0073] The yield of Test Example 1 under different reaction conditions is shown in Test Example 1-2.
[0074] Test Example 1: A preparation process of azelaic acid, wherein the specific process steps are:
[0075] S1, taking 1 kg of catalyst to prepare a catalyst bed;
[0076] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;
[0077] S3, the azelaic acid feeder enters the preheating section after metering, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is: 240°C; the reaction conditions of the reaction are: the molar ratio of azelaic acid to ammonia is: 1: 20; the reaction pressure is 0.1Mpa, and the raw material space velocity is 1.5h -1 ; The reaction temperature is 450°C;
[0078] S4, the crude product is purified by distillation to obtain the product azelaic acid nitrile, wherein the yield of azelaic acid nitrile is 98.9%.
[0079] Test Example 2:
[0080] A preparation process of azelaic acid, the specific process steps are:
[0081] S1, taking 1 kg of catalyst to prepare a catalyst bed;
[0082] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;
[0083] S3, the azelaic acid feeder enters the preheating section after metering, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is: 220°C; the reaction conditions of the reaction are that the molar ratio of azelaic acid to ammonia is: 1:2; the reaction pressure is 5Mpa, and the raw material space velocity is 0.1h -1 ; The reaction temperature is 350°C;
[0084] S4, the crude product is purified by distillation to obtain the product azelaic acid nitrile, wherein the yield of azelaic acid nitrile is 98.6%.
[0085] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A process for preparing azelaic acid nitrile, Features: The preparation process comprises the following steps: reacting azelaic acid with ammonia in the presence of a catalyst; The reaction conditions are as follows: the molar ratio of azelaic acid to ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-1.5 h -1 ; Reaction temperature is 350~450℃; The preparation method of the catalyst comprises the following steps: (1) Ultrasonic dispersion of calcium salt, chromium salt and TS-1 in deionized water, stirring, evaporating water, and then calcining to obtain product A; (2) Grind the product A, β zeolite, attapulgite and an appropriate amount of water to obtain a slurry, spray granulate the slurry, and calcine the slurry to obtain a catalyst.
2. A process for preparing azelaic acid according to claim 1, Features: In step (1), the stirring time is 30 to 50 minutes.
3. A process for preparing azelaic acid according to claim 1, Features: In step (1), the evaporation temperature is 80°C; and the calcination is performed at 450-550°C for 2-4h.
4. A process for preparing azelaic acid according to claim 1, Features: In step (1), the calcium salt is at least one of calcium acetate, calcium chloride and calcium nitrate.
5. A process for preparing azelaic acid according to claim 1, Features: In step (1), the chromium salt is at least one of chromium acetate, chromium chloride and chromium nitrate.
6. A process for preparing azelaic acid according to claim 1, Features: In step (1), the ratio of the calcium salt, the chromium salt and TS-1 is: 0.03~0.05 mol: 0.01~0.03 mol: 100 g.
7. A process for preparing azelaic acid according to claim 1, Features: In step (2), the mass ratio of the product A, β zeolite and attapulgite is 1:0.4-0.8:0.3-0.5; and the calcination treatment is performed at 500-600° C. for 5-9 hours.
8. A process for preparing azelaic acid according to claim 1, Features: The azelaic acid is preheated before the reaction, and the preheating temperature is 220-240°C.
Citation Information
Patent Citations
Decyldiamine laurate and its prepn process and application
CN101088983A
Manufacturing method for nitrile and corresponding amine thereof
CN105001033A
Preparation method of sebaconitrile
CN109206341A
Continuous preparation method of sebaconitrile and catalyst used in continuous preparation method
CN117756668A
Use of diamine microcapsules for thermal energy storage
WO2013088013A1