Water-based single-component quick-drying light anti-corrosion coating and preparation method thereof

By modifying tertiary ethylene carbonate/acrylate copolymer with silica sol, the problems of insufficient dryness, water resistance and salt spray resistance of water-based metal light anti-corrosion coatings are solved, and the efficient construction and excellent performance of single-component quick-drying coatings are achieved. performance, meeting the requirements for strong and light anti-corrosion of metal substrates.

CN118791682APending Publication Date: 2024-10-18WUHAN RES INST OF MATERIALS PROTECTION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410240160.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing water-based metal light anti-corrosion coatings have deficiencies in dryness, water resistance and salt spray resistance, and the construction of conventional systems is cumbersome and costly. Solvent-based and two-component systems have problems of environmental pollution and inconvenience of use.

Method used

Silica sol modified tertiary ethylene carbonate/acrylate copolymer is used to prepare a one-component quick-drying light anti-corrosion coating through the copolymerization reaction of silane-modified nano-silica sol and water-based acrylic acid to improve the film-forming speed and construction efficiency of the coating. , reduce costs, and enhance the water resistance and anti-rust properties of the coating through phosphate ester emulsifiers and polymerization.

Benefits of technology

It achieves the excellent comprehensive performance of water-based one-component quick-drying light anti-corrosion coating, including high water resistance, acid and alkali resistance and salt spray resistance, simplifying the construction process, reducing costs, and improving the wear resistance and Scratch resistance meets the strong and light anti-corrosion requirements of metal substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791682A_ABST
    Figure CN118791682A_ABST
Patent Text Reader

Abstract

The invention discloses a water-based single-component quick-drying light anti-corrosion coating and a preparation method thereof.According to the coating, vinyl versatate modified acrylate serves as a film forming matter, vinyl versatate copolymer emulsion is further modified through silica sol, the capillary acting force of particle shrinkage deformation in the emulsion film forming and drying process is accelerated, and the anti-corrosion performance of the coating is improved; moisture discharge and volatilization are promoted, and paint film hard drying is accelerated; the coating modified pigment filler is preferably matched, so that the coating has high stability and acid and alkali resistance; a polytetrafluoroethylene wax water emulsion is matched and migrated to the surface of a coating to form a hydrophobic layer after film formation; meanwhile, based on the synergistic effect of liquid and solid corrosion inhibition antirust agents, passivation shielding and cathode protection corrosion prevention are achieved; and a functional additive is further screened and matched, so that good guarantee is provided for stability and construction of a coating system. The coating disclosed by the invention is a single-component normal-temperature quick-drying system, is universal in bottom surface, simple in preparation process, convenient to construct, low in price and relatively high in cost performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of water-based coatings and relates to a single-component coating, in particular to a water-based single-component quick-drying light anti-corrosion coating and a preparation method thereof. Background Art

[0002] Metal surfaces are susceptible to rust due to the natural environment, reducing their service life. To effectively prevent this, applying protective coatings to steel surfaces is an effective method. Currently, the primary film-forming materials for protective coatings are organic resins, often using solvent-based systems. However, during the coating application process, large amounts of organic solvents evaporate, causing environmental pollution. With advancements in industrial technology and living standards, people's demands for the environment are also increasing, leading to a growing demand for environmentally friendly water-based coatings.

[0003] Among the numerous industrial water-based coating systems, especially for light metal protection, water-based acrylic resins offer excellent weather resistance, gloss and color retention, and odor resistance. These resins also possess mature synthetic modification technologies, resulting in a highly cost-effective solution. However, due to limitations in drying properties, water resistance, and salt spray resistance, acrylic resins remain limited in their application in industrial metal surface protection. Furthermore, conventional light metal surface anti-corrosion coating systems, consisting of three coating systems—one for the base or the other for the base and the middle—result in cumbersome construction and complex processes, hindering the widespread adoption and promotion of water-based coatings.

[0004] Therefore, in order to better meet customer needs and promote market development, a universal quick-drying water-based metal light anti-corrosion coating that combines both base and surface, and is both anti-corrosive, weather-resistant, and acid- and alkali-resistant, has become a new research and development direction. Patents CN115368790A and CN115873483A both disclose a base-and-surface coating, but both are solvent-based systems with high VOC emissions; Patent CN115975485B discloses a water-based base-and-surface coating, but it is a two-component system with a limited construction window, is not convenient to use, and has a high cost. Patent CN202210057518.3 discloses a quick-drying water-based acrylic marking paint for containers and a preparation method thereof. It uses a baking drying film-forming method and has quick-drying properties, but has high energy consumption; Patent CN202210057518.3 discloses a quick-drying water-based acrylic marking paint for containers and a preparation method thereof. It uses a two-component mode of cross-linking reaction with an isocyanate curing agent to promote cross-linking and achieve the purpose of quick drying. Summary of the Invention

[0005] In view of the shortcomings of the prior art, one of the objectives of the present invention is to provide a method for preparing a silica sol-modified versatate vinyl ester / acrylate copolymer, wherein silica sol and versatate vinyl ester are used to modify water-based acrylic acid to obtain a modified water-based acrylic acid emulsion, which can be used to prepare a single-component quick-drying coating.

[0006] Another object of the present invention is to use the above-mentioned silica sol-modified versatate vinyl ester / acrylate copolymer to prepare a water-based one-component quick-drying light anti-corrosion coating, which not only obtains excellent comprehensive performance of the coating, but also increases the film-forming speed of the coating, reduces construction costs, and improves construction efficiency.

[0007] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows: A method for preparing a silica sol-modified versatate vinyl carbonate / acrylate copolymer comprises the following steps: i) Preparation of silane-modified nano-silica sol: The nano-silica sol is injected into a reaction vessel, and then the first co-solvent is slowly added and dispersed in an ultrasonic disperser for a period of time; The reaction container is heated to a first temperature, and an excess of γ-glycidyloxypropyltrimethoxysilane is slowly added under mechanical stirring. After stirring at a constant temperature for a period of time, the reaction is performed by centrifugation to filter out excess γ-glycidyloxypropyltrimethoxysilane to obtain a silane-modified nano-silica sol. ii) Preparation of silica sol modified versatate vinyl ester / acrylate copolymer: Weighing monomers methyl methacrylate (MMA), butyl acrylate (BA), methacrylic acid (MAA), monomer VeoVa10, and an emulsifier aqueous solution, adding them to a pre-emulsification kettle equipped with a mechanical stirrer, heating to a second temperature, and stirring at a high speed to obtain a pre-emulsion; Continue to add a mixed aqueous solution of water, emulsifier, initiator and buffer into the pre-emulsification kettle, and heat it to the third temperature under controlled low-speed stirring. Then, transfer the pre-emulsion liquid to the reaction kettle, heat it to the reaction temperature, and keep it warm for a period of time after the blue light appears to obtain a seed emulsion; After the insulation is completed, the reactor is charged with materials in two stages, as follows: The first stage of feeding: the remaining pre-emulsion and the mixed aqueous solution of the initiator and the buffer are simultaneously added dropwise to the reactor. After a period of time after the addition begins, the silane-modified nano-silica sol prepared in step i) is simultaneously added dropwise to the reactor; Second stage of feeding: After the first stage of feeding, add diacetone acrylamide (DAAM) aqueous solution; After the addition is completed, the temperature is maintained at the reaction temperature for a period of time, then cooled to the fourth temperature, tert-butyl hydroperoxide (TBHP) and sodium formaldehyde sulfoxylate solution are added in two portions, and the temperature is maintained for a period of time; the temperature is further cooled to the fifth temperature, appropriate amounts of triethanolamine and ammonia water are added to adjust the pH value to a weak alkaline state, an aqueous adipic acid dihydrazide solution is added, and finally the material is filtered to remove insoluble matter to obtain a silica sol-modified versatate vinyl carbonate / acrylate copolymer emulsion; Among them, the temperature range of the first temperature is 60-70°C, the temperature range of the second temperature is 35-45°C, the temperature range of the third temperature is 71-78°C, the temperature range of the reaction temperature is 80-90°C, the temperature range of the fourth temperature is 71-78°C, and the temperature range of the fifth temperature is 28-35°C.

[0008] Preferably, the initiator is a common initiator for acrylates, preferably a peroxide initiator, such as benzoyl peroxide (BPO).

[0009] The buffer solution is a sodium bicarbonate (NaHCO3) solution.

[0010] Preferably, the content of versatate carbonic acid in the versatate vinyl ester / acrylate copolymer is 30-50%, and optimally 32%.

[0011] Preferably, the nano-silica sol is an alkaline silica sol solution with a solid content of 25-35%, and the optimal solid content is 30%.

[0012] Preferably, the mass ratio of diacetone acrylamide to adipic acid dihydrazide is 1.5-2.5:1.

[0013] Preferably, the mass ratio of the γ-glycidyloxypropyltrimethoxysilane to the nano-silica sol is 1:1.5-2.5.

[0014] Preferably, the first co-solvent is a mixture of deionized water and ethanol, with the optimal mass ratio being 1:1.

[0015] Preferably, the emulsifier is a phosphate-reactive emulsifier.

[0016] Preferably, 15-25% of the pre-emulsion is transferred to the reactor to prepare the seed emulsion.

[0017] Preferably, during the first stage of addition, the remaining pre-emulsion and the initiator buffer aqueous solution are added dropwise for 15-25 minutes before the silane-modified nano-silica sol is added dropwise, and the simultaneous addition time is 35-55 minutes; Preferably, during the second stage of adding, the diacetone acrylamide aqueous solution is added dropwise for 60-120 minutes.

[0018] Preferably, when the first cosolvent is added, the dispersion is carried out in an ultrasonic disperser for 0.5-1.5 hours, and optimally for 1 hour.

[0019] Preferably, after adding an excess of γ-glycidyloxypropyltrimethoxysilane, stirring is carried out at a constant temperature for 4-10 hours to achieve sufficient reaction and modification.

[0020] Preferably, in the pre-emulsification kettle, the rotation speed of the high-speed stirring is 2000-3000 rpm.

[0021] Preferably, after adding water, emulsifier and initiator buffer aqueous solution into the pre-emulsification kettle, the number of revolutions of low-speed stirring is 150-300 rpm.

[0022] Preferably, the pre-emulsification kettle is kept warm for 20-40 minutes after the blue light appears.

[0023] Preferably, after the two-stage addition of materials to the reactor is completed, the reactor is kept at the reaction temperature for 1.5-3 hours to allow for sufficient reaction.

[0024] Preferably, ammonia water is added to adjust the pH value to about 8.

[0025] Preferably, the mass concentration of the diacetone acrylamide (DAAM) aqueous solution added dropwise is 8-12%, and optimally 10%.

[0026] Preferably, after adding tert-butyl hydroperoxide (TBHP) and sodium formaldehyde sulfoxylate solution, the temperature is kept for 10-20 minutes.

[0027] Preferably, the mass concentration of the added adipic acid dihydrazide (ADH) aqueous solution is 8-12%, and optimally 10%.

[0028] Preferably, when discharging, a filter cloth with 200, 300 or 400 mesh is selected for filtration. The specific mesh number is selected according to the viscosity of the emulsion. The higher the viscosity, the lower the mesh number is selected.

[0029] In another aspect, the present invention provides a water-based one-component quick-drying light anti-corrosion coating comprising the following components: 2-8 parts of the second cosolvent, pH regulator, 0.5-2 parts of dispersant, 0.1-0.5 parts of defoaming agent, 0.1-1 parts of leveling agent, 5-15 parts of rust inhibitor, 5-15 parts of filler, 5-15 parts of pigment, 10-20 parts of deionized water, 1-3 parts of thickener, 0.5-2 parts of anti-flash rust agent and 35-60 parts of the silica sol modified versatate vinyl ester / acrylate copolymer emulsion prepared above.

[0030] In another aspect, the present invention provides a method for preparing a water-based one-component quick-drying light anti-corrosion coating, comprising the following steps: Weigh each component according to the ratio and set aside; add a certain amount of deionized water into the sand mill, add dispersant, part of the defoamer, filler, pigment, rust inhibitor, and cosolvent in sequence at 500-1000rpm, and disperse for 10-20 minutes; Replace the sand grinding disc, add grinding balls, and grind and disperse at a high speed of 2000-3000 rpm for 30-60 minutes until the fineness is less than 15 μm, and then filter to obtain a slurry; Add silica sol-modified versatate vinyl carbonate / acrylate copolymer emulsion into a stirring container, control the rotation speed to 800-1500 rpm, add the above slurry under stirring, add the second co-solvent and water, adjust the pH, add defoaming agent, leveling agent, and anti-flash rust agent; after fully mixing, filter and package to obtain a one-component water-based quick-drying light anti-corrosion coating.

[0031] Preferably, the grinding balls are glass beads with a diameter of about 2-3 mm.

[0032] Preferably, the second cosolvent is an alcohol ether solvent, including one or a mixture of alcohol ester dodecanol, ethylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, and propylene glycol. The most preferred mixture is alcohol ester dodecanol and propylene glycol, with a mass ratio of 4:1. Because the modified emulsion obtained by polymerization has a low film-forming temperature, minimal cosolvent is required. The addition of 3 parts of the cosolvent promotes rapid drying of the paint film.

[0033] Preferably, the pH adjuster is one or a combination of ammonia, triethylamine, AMP-95, and DMEA. DMEA is optimal. Ammonia evaporates quickly and has a strong odor, while triethylamine and AMP-95 evaporate slowly, resulting in long-term residues on the coating surface during film formation, affecting the coating's initial water resistance and salt spray resistance. The lone pairs of electrons in DMEA's nitrogen atoms have electron-donating properties and are easily captured by the metal that has lost ions, slowing corrosion of the metal substrate to a certain extent and improving salt spray resistance. The coating system is adjusted to a pH of 8-9.

[0034] Preferably, the dispersant is anionic, nonionic, or a combination thereof. The most preferred nonionic dispersant is ADDITOL VXW 6208, which exhibits strong adsorption or anchoring effects on the surfaces of pigments and fillers, and has a long molecular chain to form steric hindrance, thereby achieving a stable result. Preferably, the defoaming agent is one or a mixture of polysiloxane defoaming agent, polyether defoaming agent and polyether-modified polysiloxane defoaming agent; the best is 104BC combined with BYK346, with a mass ratio of 2:1.

[0035] Preferably, the leveling agent is a mixture of one or more silicone leveling agents, acrylic leveling agents and acetylenic alcohol leveling agents.

[0036] The anti-flash rust agent is one or a mixture of hydrochloric acid type or organic polymer compound type, specifically Enze CK-34, which is composed of organic complex and multiple polymer compounds, has a good inhibitory effect on early flash rust, and can work synergistically with preservatives.

[0037] Preferably, the filler is one or a combination of calcium carbonate, barium sulfate, talc, mica powder, and silica powder, specifically silica powder. Calcium carbonate has the advantages of being low in price, non-toxic and non-irritating, having a good color, and having a high whiteness, but it is not acid-resistant and not salt-spray-resistant. Barium sulfate has stable performance, but has a high specific gravity and is easy to settle. Talc and sericite have a flaky structure and a good physical barrier effect, but have a large oil absorption capacity, which affects the rheological properties and gloss of the system. Silica powder performs well in all aspects. Taking into account the use of silica powder, 1250 mesh, and surface modification, the present invention also provides a better modified silica powder as a filler.

[0038] The filler modification method comprises a wet process in which silica micropowder is mixed with water and stirred to form a 40% by mass slurry. The slurry is heated to 60°C, a sodium stearate solution is added as a modifier, and the mixture is stirred for 60 minutes to obtain a modified silica micropowder suspension. A sample of the modified suspension is filtered and dried to obtain a modified silica micropowder.

[0039] Modified silica powder is filled in the coating, and its surface modifier forms a tough continuous film between the particles and the base material, which promotes good interfacial bonding and quickly forms a network structure when the coating dries, thereby improving the strength, hardness, wear resistance, scratch resistance, etc. of the coating; The pigment-to-binder ratio (PVC) should be controlled at 40-45%. When the pigment and filler content is too high, the film-forming resin is insufficient to wet and encapsulate the pigment and filler particles, resulting in voids within the paint film. This weakens the bond strength and sealing properties, reduces the ability to resist the penetration of corrosive media, and reduces the corrosion resistance of the paint film. Overall, a PVC ratio of 40-45% offers the best value for money.

[0040] Preferably, the rust inhibitor includes phosphates, molybdates, borates, ion exchange types, etc., such as aluminum tripolyphosphate, zinc phosphate, aluminum zinc tripolyphosphate, zinc molybdate, strontium chrome yellow, etc. The ion activity of aluminum tripolyphosphate and zinc phosphate is relatively low, making it difficult to form a dense passivation film in the early stage and unable to demonstrate good rust prevention performance. Zinc molybdate has slightly higher ion activity, but is expensive and has average salt spray resistance, making it not cost-effective. Strontium chrome yellow has a good rust prevention effect, but contains heavy metals and is naturally yellow, which affects the user's color matching. In addition, the use of rust-proof pigments will reduce the glossiness of the coating and affect the appearance of the coating. The present invention preferably uses Ascodi's 142DA compounded with aluminum zinc tripolyphosphate in a ratio of 1:5. As a liquid rust inhibitor, 142DA has strong flow permeability and can passivate and shield the substrate interface in the early stage, isolating air and moisture, thereby achieving a good anti-rust effect. Zinc aluminum tripolyphosphate has a good passivation effect on the metal substrate in the later stage, and the zinc metal contained therein can also alleviate metal corrosion through cathode action, thereby improving the corrosion resistance of the coating.

[0041] Preferably, the pigment is one or a combination of carbon black, titanium dioxide, red iron oxide or yellow iron oxide; the most preferred is rutile titanium dioxide, which has a more stable structure. Furthermore, the titanium dioxide surface is treated with silicon, aluminum, and zirconium coatings, which has good hiding and chemical stability, acid and alkali resistance, and good gloss and hiding effects. Specifically, Chemours R902 + .

[0042] Preferably, the thickener is one or a combination of cellulose, alkali-swellable, or associative polyurethane. The optimal combination is a cellulose-to-associative thickener in a mass ratio of 2:1. Alkali-swellable thickeners thicken the aqueous phase, exhibiting low viscosity under high shear conditions and high viscosity under static and low shear conditions. Therefore, after application, the viscosity rapidly increases, preventing sagging. However, this can lead to poor leveling, severe brush marks, and application spattering. Associative polyurethane thickeners, on the other hand, thicken latex particles. The associative structure they form with the particles is easily disrupted by shear forces, reducing the viscosity of the system. Once the shear force subsides, the viscosity recovers, preventing sagging during application. Furthermore, their viscosity recovery exhibits a certain hysteresis, which facilitates coating leveling. The hydrophobic groups they contain have a strong affinity for the coating matrix, enhancing the coating's water resistance. This combination maintains a good low-shear, high-viscosity profile, which facilitates storage, while also promoting leveling during application. Specifically, RD and RM-8W are listed.

[0043] Preferably, other additives may be added, and the other additives are polytetrafluoroethylene wax water emulsion, which migrates to the coating surface to form a hydrophobic layer after film formation, specifically Nanjing Tianshi New Material PTFE-1008.

[0044] The quick-drying principle of the anti-corrosion coating of the present invention is as follows: like Figure 4 As shown in Figure 1, the drying and film-forming process of conventional one-component water-based acrylic emulsions mainly includes four stages: (1) After coating, water begins to evaporate and the emulsion gradually becomes thicker; (2) As the water in the emulsion continues to evaporate, the latex particles gradually move closer and contact each other to reach a dense state; (3) When the water evaporates to a certain extent, the gaps between the latex particles become smaller and form fine capillaries. Under the action of the capillary extreme pressure, the water evaporates faster, the particles deform and gradually fuse until the interface between the particles disappears; (4) The latex particles aggregate and age and reach a mechanical drying state. Finally, the emulsion will form a dense protective film on the metal surface. The third and fourth stages of the drying and film-forming process have the most important impact on the coating film. As the particles approach each other, the particles begin to deform and accumulate. In most cases, surface tension and capillary pressure are the main driving forces for particle deformation and fusion, which have a decisive effect on the actual drying and comprehensive performance of the paint film.

[0045] The present invention introduces tert-butyl vinyl carbonate into an acrylic acid system and adopts silica sol for solution polymerization modification to enhance the water resistance, corrosion resistance and drying performance of the coating.

[0046] Among them, the vinyl functional groups contained in tertiary esters can be copolymerized with acrylic ester monomers. The tertiary carbonic acid groups contained in them have great steric hindrance and shielding effects, protecting the ester bonds from hydrolysis. At the same time, since there is no hydrogen on the α-carbon atom, it will not degrade under the action of ultraviolet light, thus bringing excellent water resistance, alkali resistance and weather resistance.

[0047] Furthermore, in the present invention, nano-silica sol is first modified with γ-glycidyloxypropyltrimethoxysilane, and the surface of the silica sol particles is covered with silanol groups (─Si─OH). These surface active groups then continue to participate in emulsion polymerization, and the silanol bonds undergo condensation and cross-linking reactions to form an appropriate network structure, thereby increasing the cross-linking density of the latex film. At the same time, the arrangement of methyl groups in the molecular structure makes it hydrophobic, thereby providing water resistance. The high-energy chemical bond, Si-O bond, has a bond energy far greater than that of C-H bond, C-C bond, and C-O bond, which makes the molecular chain segments have excellent stability.

[0048] The molecular structure of silica sol modified versatate / acrylate copolymer obtained by polymerization is as follows Figure 5 As shown, -OCH3 is a group specific to methyl methacrylate, -OCH2 is a group specific to butyl acrylate, and -OCH is a group specific to tert-butyl carbonate. At the same time, silanol groups (─Si─OH) are also grafted onto the molecular chain through cross-linking.

[0049] During the drying and film-forming process of the paint film, as the water evaporates, the particles gradually aggregate and the gaps between them decrease. Due to the steric hindrance effect of the tertiary carbonic acid group, it can repel the water near the group and promote the volatilization of water. When the gaps between the latex particles become smaller and form tiny capillaries, under the action of the capillary extreme pressure and the hydrophobic network structure of Si-O, -CH4, it can accelerate the release of water molecules into the air through the capillary channels, thereby accelerating the drying time of the paint film.

[0050] In the emulsion polymerization, a reactive phosphate emulsifier is introduced. When a reactive emulsifier is used in the polymerization process, the reactive functional group can directly participate in the polymerization reaction, so that the emulsifier is polymerized to the latex particles through chemical bonds, thereby avoiding the migration of the emulsifier, improving the water resistance of the coating, and helping to reduce the corrosion current, thereby improving the anti-rust performance of the emulsion. At the same time, the phosphate group can not only form a dense phosphate film on the surface of the metal substrate to provide anti-rust protection for the substrate, but the hydroxyl group in the phosphate group can also chelate with the surface of the metal substrate to form a metal complex (such as Figure 5 As shown in the figure, the polymer is tightly bonded to the metal surface, thereby improving the adhesion of the coating. Finally, the hydrophilic groups in the phosphate ester are converted into hydrophobic groups, which prevents the penetration of water molecules, oxygen and chloride ions, and further enhances the anti-corrosion performance of the modified composite emulsion system.

[0051] In the preparation of the coating, by rationally matching various raw materials and using preferred pigments and modified fillers, it has strong stability and acid and alkali resistance; with polytetrafluoroethylene wax aqueous emulsion, after film formation, it migrates to the coating surface to form a hydrophobic layer; at the same time, based on the synergistic effect of liquid and solid corrosion inhibitors, passivation forms a protective film and blocks electrochemical reactions, effectively protecting the metal substrate from oxidation and corrosion, extending its service life; further screening and matching additives, including wetting dispersants, rheological thickeners, etc., provide good guarantees for the stability of the coating system and construction. In addition, the water-based one-component quick-drying light anti-corrosion coating of the present invention can be used as a bottom and top layer, and an excellent coating can be obtained by directly applying 2-3 coats.

[0052] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing a water-based one-component light anti-corrosion coating, which has excellent water resistance, acid and alkali resistance and corrosion resistance, dries quickly at room temperature, and has salt spray resistance of up to 500 hours. It has a simple preparation process, convenient construction, unified bottom and surface, and excellent performance. It can meet the strong light anti-corrosion requirements of general metal substrates and has a high cost-effectiveness ratio.

[0053] Compared with the single-component acrylic paint in the prior art, the present invention increases the film-forming speed by about 20% while retaining excellent water resistance, acid and alkali resistance and corrosion resistance, thereby saving construction time, improving construction efficiency and reducing costs.

[0054] The one-component water-based quick-drying light anti-corrosion coating is prepared by the method. The construction method of the product is flexible and diverse, and it can be sprayed, brushed or dipped. The bottom and the top can be integrated, and the product can quickly dry and form a film at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 These are the alkali-resistant immersion samples of the coatings in Examples 1, 2, 3 and Comparative Examples 1, 2, 3.

[0056] Figure 2 The salt spray test comparison diagram of Example 1 and Comparative Example 1 is shown.

[0057] Figure 3 Schematic diagram of the drying and film-forming process of a conventional one-component water-based acrylic emulsion in the prior art.

[0058] Figure 4 This is the molecular structure diagram of silica sol modified versatate vinyl ester / acrylate copolymer.

[0059] Figure 5 Schematic diagram of the principle of phosphate emulsifier's anti-rust protection effect on the substrate. DETAILED DESCRIPTION

[0060] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to illustrate the present invention and are not intended to limit the present invention. Any simple improvements to the preparation method of the present invention based on the concept of the present invention are within the scope of protection of the present invention.

[0061] Example: The preparation method of silica sol modified versatate vinyl ester / acrylic acid copolymer is as follows: i) Preparation of silane-modified nano-silica sol: A certain amount of alkaline silica sol solution with a solid content of 30% was injected into a three-necked flask, and then the first cosolvent was slowly added. The mixture was dispersed in an ultrasonic disperser for 1 hour. The flask was placed in a water bath and heated at 65°C. Under mechanical stirring, a certain amount of γ-glycidyloxypropyltrimethoxysilane was slowly added. After constant temperature stirring for 6 hours, the mixture was centrifuged several times at high speed and the excess γ-glycidyloxypropyltrimethoxysilane was filtered to obtain silane-modified nano-silica sol.

[0062] The mass ratio of the γ-glycidyloxypropyltrimethoxysilane to the nano-silica sol is 1:2; The first cosolvent is a mixture of deionized water and ethanol in a mass ratio of 1:1; ii) Preparation of silica sol modified versatate vinyl ester / acrylate copolymer: Weigh the monomers methyl methacrylate (MMA), butyl acrylate (BA), methacrylic acid (MAA), VeoVa10 monomer, and an emulsifier aqueous solution into a pre-emulsification kettle equipped with a mechanical stirrer. Heat to 40°C with high-speed stirring to obtain a pre-emulsion. Add water, emulsifier, initiator, and initiator buffer aqueous solution, and heat to 75°C at 200 rpm. Add 20% of the pre-emulsion to the reactor, heat to 85°C, and incubate for 30 minutes after the appearance of a blue light to obtain a seed emulsion. After incubation, simultaneously add the remaining pre-emulsion and initiator buffer aqueous solution dropwise to the reactor. After approximately 20 minutes of dropwise addition, place the silane-modified silica sol prepared in step i in a separate constant-pressure separatory funnel and add dropwise to the three-necked flask. Control the addition rate over 1 hour. Add a 10% DAAM aqueous solution. Keep the entire addition process constant over approximately 3 hours, and maintain a constant rate throughout. After the addition is completed, the mixture is kept at 85°C for 2 hours, then cooled to 75°C, and tert-butyl hydroperoxide (TBHP) and sodium formaldehyde sulfoxylate solution are added twice, and kept warm for 15 minutes; the temperature is further lowered to 30°C, ammonia water is added to adjust the pH value to 8, and a 10% adipic acid dihydrazide (ADH) aqueous solution is added. Finally, the material is filtered with a 300-mesh filter cloth to obtain a silica sol-modified versatate vinyl carbonate / acrylate copolymer.

[0063] The dosage ratio of DAAM to ADH is 2:1; The mass ratio of methyl methacrylate (MMA), butyl acrylate (BA), methacrylic acid (MAA), and monomer VeoVa10 is 14:7:1:10.

[0064] Based on the total amount of methyl methacrylate (MMA), butyl acrylate (BA), methacrylic acid (MAA), and monomer VeoVa10, the following components are used in percentage by mass as follows: DAAM, 2%; The emulsifier LRP-10, 10% The initiator is benzoyl peroxide (BPO), 0.6% The initiator solution is sodium bicarbonate (NaHCO3), appropriate amount.

[0065] Oxidant tert-butyl hydroperoxide (TBHP), 0.04% Preparation method of water-based one-component quick-drying light anti-corrosion coating The formula of water-based one-component quick-drying light anti-corrosion coating is as follows: 35-60 parts of silica sol modified versatate vinyl carbonate / acrylate copolymer, 2-8 parts of second cosolvent, pH adjuster, 0.5-2 parts of dispersant, 0.1-0.5 parts of defoamer, 0.1-1 parts of leveling agent, 5-15 parts of rust inhibitor, 5-15 parts of filler, 5-15 parts of pigment, 10-20 parts of deionized water, 1-3 parts of thickener, 0.5-2 parts of anti-flash rust agent, and 0.1-1 parts of other additives.

[0066] The preparation method of the coating comprises the following steps: Weigh each component according to the ratio; add a certain amount of deionized water into the sand mill, add dispersant, part of the defoamer, filler, pigment, rust inhibitor, cosolvent, etc. in sequence at 500-1000 rpm, and disperse for 10-20 minutes; replace the sand mill disc, add 2-3 mm glass beads, grind and disperse at high-speed stirring of 2000-3000 rpm for 30-60 minutes until the fineness is less than 15 μm, and then filter to obtain a slurry; add silica sol-modified copolymer emulsion into a plastic tank, control the speed to 800-1500 rpm, add the above slurry under stirring, add the remaining cosolvent and water, adjust the pH, add defoamer, leveling agent, anti-flash rust agent, etc.; after fully mixing for 15-30 minutes, filter and package to obtain a single-component water-based quick-drying light anti-corrosion coating; The cosolvent is a mixture of alcohol ester dodecanol and propylene glycol, with a mass ratio of 4:1; The dispersant is non-ionic ADDITOL VXW 6208; The defoamer is UNIQ FOAM 292 W of the silicone type; The leveling agent is 104BC and BYK346, with a mass ratio of 2:1; The rust inhibitor is Ascodi's 142DA and zinc aluminum tripolyphosphate, with a mass ratio of 1:5; The filler is 1250 mesh modified silica powder; The other additives are Tianshi PTFE-1008; The pigment is titanium dioxide, R902+; The thickener is a combination of cellulose and associative thickener in a mass ratio of 2:1, specifically RD+RM-8W.

[0067] According to the above preparation method, the type and content of the film-forming material were changed to obtain Examples 1, 2, 3 and Comparative Examples 1, 2, 3, respectively, as shown in Table 1. The film-forming materials in Comparative Examples 1 and 2 were commercially available ordinary acrylic emulsions, the film-forming material in Comparative Example 3 was a non-silica sol-modified versatate vinyl carbonate / acrylate copolymer, and the film-forming material in Examples 1, 2, and 3 was a silica sol-modified versatate vinyl carbonate / acrylate copolymer. According to the above coating preparation method, the raw material compositions of the comparative examples and examples are as follows: Table 1 Raw materials and their quantities in Examples 1, 2, 3 and Comparative Examples 1, 2, 3

[0068] The construction was carried out on tinplate using Examples 1, 2, 3 and Comparative Examples 1, 2, 3, and the performance tests thereof are shown in the following table: Table 2 Test results of coating properties of Examples 1, 2, 3 and Comparative Examples 1, 2, 3

[0069] The test results show that compared with the ordinary acrylic acid system (Comparative Examples 1 and 2), the water resistance and alkali resistance of the tert-butyl carbonate / acrylate copolymer system (Comparative Example 3) are significantly improved after copolymerization modification of tert-butyl carbonate. Figure 1 As shown. Furthermore, by modifying the tertiary propylene copolymer with silica sol (Example 1), the drying property is further improved compared with the comparative example 3, and its acid and alkali resistance and paint film hardness are also improved simultaneously. However, further increasing the amount of rust inhibitor (Examples 2 and 3) leads to the accumulation of particles in the system, resulting in surface loss of gloss and low salt spray performance. Figure 2 Comparison of the neutral salt spray test in

[15] shows that the salt spray resistance of ordinary acrylic systems is less than 10 days, indicating extensive blistering and increased corrosion. However, the water-based one-component light-duty anti-corrosion coating of the present invention has excellent salt spray resistance, maintaining a good gloss for more than 500 hours within 22 days, with no obvious corrosion.

[0070] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A method for preparing a silica sol-modified versatate vinyl carbonate / acrylate copolymer, characterized in that: The following steps are involved: i) Preparation of silane-modified nano-silica sol: Inject the nano-silica sol into a reaction container, then slowly add the first co-solvent, and disperse it in an ultrasonic disperser for a period of time; The reaction container is heated to a first temperature, and an excess of γ-glycidyloxypropyltrimethoxysilane is slowly added under mechanical stirring. After a period of constant temperature stirring, the reaction is performed by centrifugation to filter out excess γ-glycidyloxypropyltrimethoxysilane to obtain a silane-modified nano-silica sol; ii) Preparation of silica sol modified versatate vinyl carbonate / acrylate copolymer: Weighing monomers methyl methacrylate, butyl acrylate, methacrylic acid, monomer VeoVa10 and an emulsifier aqueous solution, adding them into a pre-emulsification kettle equipped with a mechanical stirrer, heating to a second temperature and stirring at a high speed to obtain a pre-emulsion; Add water, an emulsifier, and a mixed aqueous solution of an initiator and a buffer, and heat to a third temperature under controlled low-speed stirring, then transfer part of the pre-emulsion to a reaction kettle, heat to the reaction temperature, and keep the temperature for a period of time after blue light appears to obtain a seed emulsion; After the insulation is completed, the reactor is charged with materials in two stages, as follows: The first stage of feeding: the remaining pre-emulsion and the mixed aqueous solution of the initiator and the buffer are simultaneously added dropwise to the reactor. After a period of time from the start of the addition, the silane-modified nano-silica sol prepared in step i) is simultaneously added dropwise to the reactor; Second stage of feeding: after the first stage of feeding, add the diacetone acrylamide aqueous solution; After the addition is completed, the temperature is kept at the reaction temperature for a period of time, then the temperature is lowered to the fourth temperature, a small amount of oxidizing agent tert-butyl hydroperoxide and reducing agent sodium formaldehyde sulfoxylate solution are added twice, and the temperature is kept for a period of time; The temperature is further lowered to the fifth temperature, ammonia water is added to adjust the pH value to be weakly alkaline, adipic acid dihydrazide aqueous solution is added, and finally the material is filtered out to remove insoluble matter to obtain a silica sol-modified versatate vinyl carbonate / acrylate copolymer emulsion; Among them, the temperature range of the first temperature is 60-70°C, the temperature range of the second temperature is 35-45°C, the temperature range of the third temperature is 71-78°C, the temperature range of the reaction temperature is 80-90°C, the temperature range of the fourth temperature is 71-78°C, and the temperature range of the fifth temperature is 28-35°C.

2. The method for preparing the silica sol-modified versatate vinyl carbonate / acrylate copolymer according to claim 1, characterized in that: In the versatate vinyl ester / acrylate copolymer, the content of versatate carbonic acid is 30-50%.

3. The method for preparing the silica sol modified versatate vinyl carbonate / acrylate copolymer according to claim 1, characterized in that: The mass ratio of the diacetone acrylamide to adipic acid dihydrazide is 1.5-2.5:

1.

4. The method for preparing the silica sol modified versatate vinyl carbonate / acrylate copolymer according to claim 1, characterized in that: Transfer 15-25% of the pre-emulsion to the reactor to prepare the seed emulsion.

5. The method for preparing the silica sol modified versatate vinyl carbonate / acrylate copolymer according to claim 1, characterized in that: In the first stage of feeding, the remaining pre-emulsion and initiator buffer aqueous solution are added dropwise for 15-25 minutes, and then the silane-modified nano-silica sol is added dropwise, and the simultaneous addition time is 35-55 minutes; During the second stage of adding, the diacetone acrylamide aqueous solution is added dropwise for 60-120 minutes.

6. A water-based one-component quick-drying light anti-corrosion coating, characterized in that: Includes the following components: 2-8 parts of cosolvent, pH regulator, 0.5-2 parts of dispersant, 0.1-0.5 parts of defoamer, 0.1-1 parts of leveling agent, 5-15 parts of rust inhibitor, 5-15 parts of filler, 5-15 parts of pigment, 10-20 parts of deionized water, 1-3 parts of thickener, 0.5-2 parts of anti-flash rust agent and 35-60 parts of silica sol modified versatate vinyl carbonate / acrylate copolymer emulsion prepared according to any one of claims 1-5.

7. A method for preparing the water-based one-component quick-drying light anticorrosive coating according to claim 6, characterized in that: The following steps are involved: Weigh each component according to the ratio; add a certain amount of deionized water into the sand mill, add dispersant, part of defoamer, filler, pigment, corrosion inhibitor, and co-solvent in sequence at 500-1000rpm, and disperse for 10-20min; Replace the sand grinding disc, add grinding balls, grind and disperse at 2000-3000rpm high-speed stirring for 30-60min until the fineness is less than 15um, and then filter to obtain slurry; Add silica sol modified versatate vinyl carbonate / acrylate copolymer emulsion into a stirring container, control the rotation speed to 800-1500rpm, add the above slurry under stirring, add the second co-solvent and water, adjust the pH, add defoamer, leveling agent and anti-flash rust agent; after fully mixing, filter and package to obtain a single-component water-based quick-drying light anti-corrosion coating.

8. The method for preparing the water-based one-component quick-drying light anticorrosive coating according to claim 7, characterized in that: The second auxiliary solvent is an alcohol ether solvent, including one or a mixture of alcohol ester dodecanedione, ethylene glycol butyl ether, dipropylene glycol methyl ether, dipropylene glycol butyl ether, and propylene glycol.

9. The method for preparing the water-based one-component quick-drying light anticorrosive coating according to claim 7, characterized in that: The pH regulator is one or a combination of ammonia water, triethylamine, AMP-95 and DMEA.

10. The method for preparing the water-based one-component quick-drying light anticorrosive coating according to claim 7, characterized in that: The dispersant is anionic, nonionic or a combination thereof.