Super-hydrophobic cellulose film as well as preparation method and application thereof

By carrying out silanization treatment during the regeneration process of cellulose film, a network of cellulose and long-chain siloxane is formed, which solves the problem of hydrophilicity of cellulose film and prepares highly hydrophobic cellulose film, which is suitable for food packaging and other fields. , achieving the improvement of superhydrophobicity of cellulose films.

CN118791769AInactive Publication Date: 2024-10-18ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202411267799.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The inherent hydrophilicity of cellulose films limits their potential for applications with hydrophobic or superhydrophobic properties, especially in areas such as food packaging.

Method used

A homogeneous cellulose solution is prepared by adding microcrystalline cellulose powder to the ionic liquid co-solvent system, and performs a silanization reaction during the regeneration process. A cellulose film is prepared using a blade coating method to form cellulose and long-chain siloxane. network, improving its hydrophobicity.

Benefits of technology

A superhydrophobic cellulose film with a water contact angle greater than 121.7° is prepared, which has self-cleaning properties and is suitable for food packaging and agricultural mulch films. The process is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791769A_ABST
    Figure CN118791769A_ABST
Patent Text Reader

Abstract

The invention relates to the field of manufacturing of hydrophobic films, in particular to a super-hydrophobic cellulose film as well as a preparation method and application thereof. The preparation method comprises the following steps: firstly, dispersing tetraethyl orthosilicate, hexadecyltrimethoxysilane and ammonia water in an ethanol solution to prepare a cellulose regeneration solution, and carrying out silanization modification on cellulose through hydrolysis and polycondensation of tetraethyl orthosilicate and hexadecyltrimethoxysilane in the process of regenerating cellulose into a film. The water contact angle of the prepared super-hydrophobic cellulose film is 121.7 to 151.8 degrees. The method has the advantages that the operation process is simple, the reaction condition is mild, the used cellulose solvent, silane modifier and regenerated solvent are green and environment-friendly, the prepared cellulose film can be used for packaging materials, and the problems of inherent hydrophilicity and the like of current cellulose-based products are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of manufacturing hydrophobic films, and in particular to a super-hydrophobic cellulose film and a preparation method and application thereof. Background Art

[0002] Cellulose is the most abundant biopolymer on earth and has attracted much attention in recent years due to its availability, biocompatibility, environmental friendliness, non-toxicity, and biodegradability. Cellulose is composed of linear glucose molecules connected by β(1→4) glycosidic bonds, and each glucose unit has three active hydroxyl groups. However, the hydroxyl groups on the cellulose surface can easily establish hydrogen bonds with water molecules, thereby significantly increasing its hydrophilicity. For example, the water contact angle of unmodified regenerated cellulose film is only 41.3°. This inherent property limits its potential in applications that require hydrophobic or superhydrophobic properties.

[0003] To address this limitation, great efforts have been made in molecular structure design, aiming to modify cellulose at the molecular level to enhance its hydrophobicity while retaining its beneficial properties. Therefore, various strategies have been studied to improve the hydrophobic properties of cellulose, including physical surface treatment, plasma treatment, and chemical derivatization. In summary, the progress in the preparation of superhydrophobic cellulose films by different methods highlights its potential for wide application in areas such as food packaging. Nevertheless, further research remains crucial to explore new technologies and enhance the properties of these films to expand the application of cellulose-based products.

[0004] Cellulose dissolution and regeneration into film is an effective method for preparing cellulose film. Cellulose is dissolved to obtain a cellulose solution, and then the cellulose solution is added to a regeneration solvent for precipitation to obtain regenerated cellulose through a dissolution-regeneration process. The regeneration process changes the cellulose chain conformation from cellulose I to cellulose II, resulting in a structure with more amorphous regions, reduced crystallinity, increased chemical reactivity, and a tendency to widely modify the regenerated cellulose product, such as hydrogels, aerogels, cryogels, xerogels, fibers and films. The cellulose solution obtained after cellulose is dissolved in an ionic liquid has the characteristics of a viscous fluid. Therefore, in the process of cellulose regeneration, blade coating is an effective method for preparing cellulose film, and films of different thicknesses can be prepared by controlling the thickness of the solution.

[0005] Superhydrophobicity is a phenomenon in which the water contact angle is greater than 150° and the rolling angle is less than 10°. It has attracted widespread attention in the fields of self-cleaning and oil-water separation due to its excellent water repellency. Superhydrophobic surfaces mainly rely on micro-nano rough surfaces and low surface energy. Therefore, surface grafting with a small amount of organic matter with low surface energy is an efficient and convenient method to form superhydrophobic surfaces. In addition, organosilicon compounds can increase the surface roughness of cellulose. Moreover, organosilicon compounds have many good properties, including environmental protection, non-toxicity, antioxidant, high temperature resistance and corrosion resistance. Long-chain alkanes can provide low surface energy. Therefore, in the process of cellulose regeneration, the hydroxyl groups of cellulose and the hydrolyzate of silane compounds are polycondensed to achieve silanization of cellulose, and the hydrophobicity of cellulose is achieved by grafting silane compounds to achieve rough surface and low surface energy. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a super-hydrophobic cellulose film and a preparation method and application thereof.

[0007] The first object of the present invention is to provide a method for preparing a super-hydrophobic cellulose film, comprising the following steps: (1) adding microcrystalline cellulose powder into an ionic liquid co-solvent system to prepare a homogeneous cellulose solution having viscous fluid properties; (2) pouring the cellulose solution obtained in step (1) onto the substrate, and controlling the thickness of the cellulose solution by a doctor blade coating method; (3) subjecting the cellulose solution in step (2) to a silanization reaction in a regeneration solution to obtain a cellulose film; (4) The cellulose film prepared in step (3) is washed with a solvent and dried to obtain a superhydrophobic cellulose film.

[0008] The second object of the present invention is to provide a super-hydrophobic cellulose film prepared by the above-mentioned preparation method.

[0009] The third object of the present invention is to provide a super-hydrophobic cellulose film for use in preparing food packaging products.

[0010] The beneficial effects of the present invention are: (1) The present invention prepares a super-hydrophobic cellulose film by first dissolving cellulose and then modifying the cellulose during the regeneration process.

[0011] (2) The present invention adopts a blade coating method to prepare the film. The blade coating method can be used to prepare films of different thicknesses on a large area, and has the advantages of simple operation and easy industrialization.

[0012] (3) The super-hydrophobic cellulose film prepared in the present invention is a film in which cellulose and a long-chain siloxane network are linked by chemical bonds.

[0013] (4) The present invention can adjust the hydrophobicity of the cellulose film by adjusting the mass ratio of the long-chain silane compound. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0015] Figure 1 Schematic diagram of the preparation of superhydrophobic cellulose film.

[0016] Figure 2 It is the infrared spectra of comparative example and embodiment 1.

[0017] Figure 3 It is the X-ray photoelectron spectrum diagram of comparative example and embodiment 1.

[0018] Figure 4 This is the EDS spectrum of Example 1.

[0019] Figure 5 This is a scanning electron microscope image of Example 1.

[0020] Figure 6 2D morphology image of the comparative example.

[0021] Figure 7 This is the 2D morphology image of Example 1.

[0022] Figure 8 The water contact angle diagrams of the comparative example and embodiments 1, 2, 3, and 4 are shown.

[0023] Fig. 9 The stress-strain curves of the comparative example and embodiments 1, 2, 3, and 4 are shown in FIG. DETAILED DESCRIPTION

[0024] The present application dissolves a certain amount of cellulose in an ionic liquid co-solvent system to obtain a homogeneous cellulose solution with viscous fluid properties. Dissolving the cellulose will increase the accessibility of the cellulose, causing the cellulose to expose a large number of hydroxyl groups on its surface, which is beneficial to the silanization process. The cellulose is modified by silanization through hydrolysis and polycondensation reactions during the cellulose regeneration process. The present application has the advantages of a simple operating process, and the cellulose solvent, silane modifier, and regeneration solvent used are all green and environmentally friendly. Cellulose films with different degrees of hydrophobicity can be prepared by controlling the mass ratio of the silane compound in the regeneration solution. The prepared super-hydrophobic cellulose film can be used as a packaging material, and can solve the problems of the inherent hydrophilicity of current cellulose-based products. The present application specifically includes the following steps, see Figure 1 : Step (1), adding microcrystalline cellulose powder into an ionic liquid co-solvent system to prepare a homogeneous cellulose solution having viscous fluid properties; Step (2), pouring the cellulose solution obtained in step (1) onto the substrate, and controlling the thickness of the cellulose solution by a doctor blade coating method; Step (3), subjecting the cellulose solution in step (2) to a silanization reaction in a regeneration solution to obtain a cellulose film; Step (4), washing the cellulose film in step (3) with a solvent and drying it to obtain a super-hydrophobic cellulose film.

[0025] The ionic liquid co-solvent system in step (1) is specifically a mixture of 1-butyl-3-methylimidazolium chloride and dimethyl sulfoxide, with a mass ratio of 3:1.

[0026] Through the above technical solution, the addition of a certain amount of dimethyl sulfoxide helps to disperse the cellulose powder, thereby increasing the dissolution rate of cellulose, and also helps to reduce the viscosity of the ionic liquid.

[0027] In the step (1), the mass ratio of cellulose powder to ionic liquid co-solvent system is 1:39, the cellulose is microcrystalline cellulose with a degree of polymerization of 280, the dissolution temperature of the cellulose in the ionic liquid co-solvent system is 80° C., and the reaction time is 1 hour.

[0028] In order to obtain more homogeneous cellulose solution through the above technical solution, more cellulose should be dissolved. If too much cellulose is added, the viscosity of the ionic liquid will increase, and the cellulose will not be fully dissolved, so the obtained cellulose solution contains undissolved cellulose.

[0029] In the step (2), the cellulose solution is coated by a doctor blade with a thickness of 1000 μm and an area of ​​10 cm×8 cm.

[0030] Through the above technical solution, the thickness of the cellulose solution is directly related to the thickness of the film. If the solution is too thin, the film will be too thin, and the strength of the obtained cellulose film will be too low. In addition, the blade coating method can prepare a large-area uniform film.

[0031] The regeneration solution in step (3) is a mixed solution of ethanol, tetraethyl orthosilicate, hexadecyltrimethoxysilane and ammonia water, with a mass ratio of 20:0.25:(0.7-1):2, a reaction temperature of 25°C and a reaction time of 12h.

[0032] Through the above technical scheme, tetraethyl orthosilicate is pre-hydrolyzed under alkaline conditions and condensed with the hydrolysis product of hexadecyltrimethoxysilane to form a siloxane network, which is further condensed with the hydroxyl groups on the surface of cellulose, and finally the siloxane network is grafted on the surface of cellulose, and the hydrophobicity of cellulose is improved by long-chain alkanes.

[0033] The solvent in step (4) is an anhydrous ethanol solution.

[0034] Through the above technical solution, the siloxane compounds attached to the surface of the cellulose membrane that have not been successfully grafted are removed.

[0035] The water contact angle of the super-hydrophobic cellulose film is 121.7-151.8°, and it has certain self-cleaning properties, and can be applied to the fields of food packaging films and agricultural mulch films.

[0036] In order to further understand the present invention, the embodiments of the present invention will be further described in detail below in combination with comparative examples and examples, but the embodiments of the present invention are not limited thereto.

[0037] Comparative Example (1) Weigh 1 g of microcrystalline cellulose and disperse it in 13 g of dimethyl sulfoxide by ultrasonic. Add the dispersed cellulose dispersion into 39 g of 1-butyl-3-methylimidazolium chloride solution and react at 80°C for 1 h to obtain a homogeneous cellulose solution with viscous fluid properties.

[0038] (2) Pour the cellulose solution onto a glass plate and scrape out a solution with a thickness of 1000 μm using a doctor blade.

[0039] (3) Place the glass plate with the cellulose solution into anhydrous ethanol and react at 25°C for 12 hours to obtain a cellulose film.

[0040] (4) The cellulose film was washed by soaking in anhydrous ethanol for 5 times and dried at room temperature.

[0041] Example 1 (1) Weigh 1 g of microcrystalline cellulose and disperse it in 13 g of dimethyl sulfoxide by ultrasonication. Add the dispersed cellulose dispersion into 39 g of 1-butyl-3-methylimidazolium chloride solution and react at 80°C for 1 h to obtain a homogeneous cellulose solution with viscous fluid properties.

[0042] (2) Pour the cellulose solution onto a glass plate and scrape out a solution with a thickness of 1000 μm using a doctor blade.

[0043] (3) Add 0.25 g of tetraethyl orthosilicate, 1 g of hexadecyltrimethoxysilane, and 2 mL of aqueous ammonia to 20 mL of anhydrous ethanol to prepare a regeneration solution.

[0044] (4) Place the glass plate with the cellulose solution into the regeneration solution and react at 25°C for 12 hours to obtain a cellulose film.

[0045] (5) The cellulose film was washed by soaking in anhydrous ethanol for 5 times and dried at room temperature to obtain a superhydrophobic cellulose film.

[0046] according to Figure 2 It can be seen that Example 1 has -1 The peaks at 1467 cm-1 correspond to the stretching vibrations of the symmetric and asymmetric forms of the long-chain alkyl (C–H) with low surface energy. -1 The peak at 1045cm is caused by the bending vibration of –CH2. -1 The peaks at 795 and 440 cm are due to the overlap of the typical absorption peaks of C–O of cellulose and the characteristic absorption peaks of Si–O–Si in siloxane compounds. -1 The peaks at are the stretching vibrations of Si–O and –CH3. The infrared spectrum data show that the silanization of the cellulose film is successful.

[0047] according to Figure 3 It can be seen that the C content of Example 1 increases, the O content decreases, and two new peaks of Si 2p and Si 2s appear. X-ray photoelectron spectroscopy data show that long-chain alkanes and siloxane groups have been successfully grafted onto the cellulose film.

[0048] Example 2 (1) Weigh 1 g of microcrystalline cellulose and disperse it in 13 g of dimethyl sulfoxide by ultrasonication. Add the dispersed cellulose dispersion into 39 g of 1-butyl-3-methylimidazolium chloride solution and react at 80°C for 1 h to obtain a homogeneous cellulose solution with viscous fluid properties.

[0049] (2) Pour the cellulose solution onto a glass plate and scrape out a solution with a thickness of 1000 μm using a doctor blade.

[0050] (3) Add 0.25 g of tetraethyl orthosilicate, 0.9 g of hexadecyltrimethoxysilane, and 2 mL of aqueous ammonia to 20 mL of anhydrous ethanol to prepare a regeneration solution.

[0051] (4) Place the glass plate with the cellulose solution into the regeneration solution and react at 25°C for 12 hours to obtain a cellulose film.

[0052] (5) The cellulose film was washed by soaking in anhydrous ethanol for 5 times and dried at room temperature to obtain a superhydrophobic cellulose film.

[0053] Example 3 (1) Weigh 1 g of microcrystalline cellulose and disperse it in 13 g of dimethyl sulfoxide by ultrasonic. Add the dispersed cellulose dispersion into 39 g of 1-butyl-3-methylimidazolium chloride solution and react at 80°C for 1 h to obtain a homogeneous cellulose solution with viscous fluid properties.

[0054] (2) Pour the cellulose solution onto a glass plate and scrape out a solution with a thickness of 1000 μm using a doctor blade.

[0055] (3) Add 0.25 g of tetraethyl orthosilicate, 0.8 g of hexadecyltrimethoxysilane, and 2 mL of aqueous ammonia to 20 mL of anhydrous ethanol to prepare a regeneration solution.

[0056] (4) Place the glass plate with the cellulose solution into the regeneration solution and react at 25°C for 12 hours to obtain a cellulose film.

[0057] (5) The cellulose film was washed by soaking in anhydrous ethanol for 5 times and dried at room temperature to obtain a superhydrophobic cellulose film.

[0058] Example 4 (1) Weigh 1 g of microcrystalline cellulose and disperse it in 13 g of dimethyl sulfoxide by ultrasonic. Add the dispersed cellulose dispersion into 39 g of 1-butyl-3-methylimidazolium chloride solution and react at 80°C for 1 h to obtain a homogeneous cellulose solution with viscous fluid properties.

[0059] (2) Pour the cellulose solution onto a glass plate and scrape out a solution with a thickness of 1000 μm using a doctor blade.

[0060] (3) Add 0.25 g of tetraethyl orthosilicate, 0.7 g of hexadecyltrimethoxysilane, and 2 mL of aqueous ammonia to 20 mL of anhydrous ethanol to prepare a regeneration solution.

[0061] (4) Place the glass plate with the cellulose solution into the regeneration solution and react at 25°C for 12 hours to obtain a cellulose film.

[0062] (5) The cellulose film was washed by soaking in anhydrous ethanol for 5 times and dried at room temperature to obtain a superhydrophobic cellulose film.

[0063] The specific performance test is as follows: (1) Thickness measurement: According to GB / T 6672-2001, the thickness of the film is measured by an electronic thickness gauge. Three points of the sample are taken for each test and the arithmetic mean is taken.

[0064] (2) Water contact angle measurement: According to GB / T 30693-2014, the water contact angle of the film was measured by a contact angle meter. The experiment was carried out at 25°C. 5.0 μL of deionized water was dropped on the surface of the film and kept for 5 seconds. Three points were tested for each group of samples and the arithmetic mean was calculated. The larger the water contact angle, the more hydrophobic the material is. When the water contact angle is greater than 150°, the material is super hydrophobic.

[0065] (3) Tensile property determination: According to the test method for tensile properties of plastics and films GB / T 13022-1991, an EJAVantage10 24″ tensile testing machine was used. The rectangular specimen size was 30 mm × 10 mm. The thickness was determined by the performance test (1). The test process was carried out at 25°C and 10 mm / min. -1 The tensile rate is tested five times for each group of samples and the arithmetic mean is calculated. The greater the elongation at break, the better the ductility of the film. The tensile elastic modulus is calculated from the initial straight line part of the stress-strain curve. The elastic modulus reflects the stiffness and elasticity of the material, that is, when the material is subjected to external force, its ability to resist deformation and restore its original state. The larger the elastic modulus, the higher the stiffness of the material.

[0066] The following is a further description of the accompanying drawings: according to Figure 4 It can be seen that C, O, and Si elements are evenly distributed on the surface of the cellulose film, indicating that the siloxane groups are successfully grafted on the cellulose surface.

[0067] according to Figure 5 It can be seen that the surface of the unmodified cellulose film is slightly uneven, while the surface of the modified cellulose film has petal-like unevenness and obvious cavities. From the surface morphology of the sample, it can be seen that the surface of the modified cellulose film is more rough and uneven.

[0068] according to Figure 6 and Figure 7 It can be seen that the root mean square roughness of Example 1 is much greater than that of the comparative example. The surface roughness will increase the effective contact area of ​​the solid surface, which means that the actual contact line length of the water droplet in contact with the solid surface will increase. On a surface with higher roughness, the water droplet must overcome a greater force to further penetrate and spread, thereby forming a larger contact angle.

[0069] Figure 8 The contact angles of the comparative example and examples 1, 2, 3, and 4. As can be seen from the data in the figure, the contact angles of examples 1, 2, 3, and 4 are all greater than those of the comparative example, indicating that the hydrophobicity of the modified cellulose film is better than that of the unmodified cellulose film, and the size of the contact angle, i.e., the degree of hydrophobicity, can be changed by adjusting the mass ratio of the long-chain alkane, because the long-chain alkane has a lower surface energy.

[0070] Fig. 9 The stress-strain curves of the comparative example and embodiments 1, 2, 3, and 4 are shown in FIG. It can be clearly seen from the curves in the figure that the elongation at break of embodiments 1, 2, 3, and 4 is higher than that of the comparative example, and the elastic modulus of embodiments 1, 2, 3, and 4 is lower than that of the comparative example. Cellulose is a high molecular polymer formed by cellulose molecular chains through hydrogen bonds and covalent bonds, and has high strength and rigidity. The elastic modulus of the cellulose film after silane modification will decrease, but the polysiloxane network structure on the cellulose surface helps to improve the ductility of the cellulose film.

[0071] In summary, in the process of cellulose regeneration, the present invention successfully silanizes cellulose through the hydrolysis and polycondensation of tetraethyl orthosilicate and hexadecyltrimethoxysilane, and the prepared cellulose film has high roughness and low surface energy. The preparation process is mild, environmentally friendly and easy to operate.

[0072] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the described specific embodiments or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above implementations based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a super-hydrophobic cellulose film, characterized in that: The following steps are involved: Step (1), adding microcrystalline cellulose powder into an ionic liquid co-solvent system to prepare a homogeneous cellulose solution having viscous fluid properties; Step (2), pouring the cellulose solution obtained in step (1) onto the substrate, and controlling the thickness of the cellulose solution by a doctor blade coating method; Step (3), subjecting the cellulose solution in step (2) to a silanization reaction in a regeneration solution to obtain a cellulose film; Step (4), washing the cellulose film in step (3) with a solvent and drying it to obtain a super-hydrophobic cellulose film; in: In step (1), the ionic liquid co-solvent system is specifically a mixture of 1-butyl-3-methylimidazolium chloride and dimethyl sulfoxide, with a mass ratio of 3:1; In step (1), the mass ratio of microcrystalline cellulose powder to ionic liquid co-solvent system is 1:39, and the degree of polymerization of the microcrystalline cellulose is 280.

2. The preparation method according to claim 1, characterized in that: The dissolution temperature of the microcrystalline cellulose in the ionic liquid co-solvent system is 80° C., and the reaction time is 1 h.

3. The preparation method according to claim 1, characterized in that: In step (2), the cellulose solution is coated by a doctor blade with a thickness of 1000 μm and an area of ​​10 cm×8 cm.

4. The preparation method according to claim 1, characterized in that: In step (3), the regeneration solution is a mixed solution of anhydrous ethanol solution, tetraethyl orthosilicate, hexadecyltrimethoxysilane and ammonia water, with a mass ratio of 20:0.25:(0.7-1):2; the silanization reaction temperature is 25°C and the reaction time is 12 h.

5. The preparation method according to claim 1, characterized in that: In step (4), the solvent is an anhydrous ethanol solution. After soaking and washing for several times, the super-hydrophobic cellulose film is naturally dried at room temperature.

6. A super-hydrophobic cellulose film, characterized in that: The method is prepared according to any one of claims 1 to 5.

7. The super-hydrophobic cellulose film according to claim 6, characterized in that: The water contact angle of the superhydrophobic cellulose film is 121.7-151.8°.

8. Use of the super-hydrophobic cellulose film as claimed in claim 6 or 7 in preparing food packaging products.

Citation Information

Patent Citations

  • Cellulose dissolving liquid as well as preparation method and application thereof

    CN103937011A

  • Preparation method and application of super-hydrophobic cellulose acetate fiber@silicon dioxide hybrid membrane

    CN106589439A

  • Preparation method of regenerated cellulose membrane material and application of cellulose membrane

    CN109796614A

  • Preparation method of microfibrillated cellulose-based super-hydrophobic protective composite material

    CN114920969A

Cited By

  • Preparation method and application of oil-water separation membrane with super-affinity in medium

    CN117105330A

  • Preparation method of oil-water separation membrane with super-philic property in medium and application thereof

    CN117105330B

  • Method for preparing composite film from biomass cellulose and composite film

    CN119350682A