Wide-frequency-domain high-efficiency electromagnetic shielding resin material and preparation method thereof
By dispersing coupling agents and conductive fillers in ethyl acetate and compounding them with thermosetting resins, high-efficiency electromagnetic shielding resin materials in a wide frequency range are prepared, which solves the problems of narrow frequency range and low efficiency of existing electromagnetic shielding materials, and achieves Effective shielding of electromagnetic waves from 2MHz to 40GHz, suitable for a variety of electronic equipment.
Patent Information
- Application Number
- CN202411070547.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing electromagnetic shielding materials have narrow frequency ranges and low efficiency, and cannot effectively cover a wide range of electromagnetic frequency bands, making it difficult to meet the growing demand for electromagnetic shielding.
The coupling agent and conductive filler are ultrasonically dispersed in ethyl acetate. After magnetic stirring and homogenization, a composite of modified conductive filler and thermosetting resin is formed. A curing agent is added for heating and solidification to prepare a high-efficiency electromagnetic shielding resin material in a wide frequency range. .
It achieves effective shielding of electromagnetic waves from 2MHz to 40GHz, improves the mechanical properties and stability of the material, meets a wide range of electromagnetic shielding requirements, and is suitable for electronic equipment, communication equipment, aerospace and other fields.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a wide-band high-efficiency electromagnetic shielding resin material and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, especially the rapid development of electronic technology, more and more electronic devices are being used in our daily life and work. While these devices bring convenience, they also bring a problem that cannot be ignored - electromagnetic radiation. Electromagnetic radiation is everywhere. It comes from the working process of various electronic devices, from smart phones to large communication equipment, from household appliances to industrial equipment, which are constantly generating electromagnetic radiation. The impact of electromagnetic radiation on the human body is complex and subtle. Long-term exposure to electromagnetic radiation may cause health problems such as headaches, insomnia, memory loss, and may even induce more serious diseases. In addition, electromagnetic radiation will also interfere with the electronic equipment itself, affecting its normal operation, and even causing equipment damage or data loss.
[0003] Therefore, how to effectively shield electromagnetic radiation, protect people's health and the safe operation of equipment has become an urgent problem to be solved. The development of high-performance electromagnetic shielding materials has become an important research direction in this field. At present, most electromagnetic shielding materials on the market have problems such as narrow frequency domain and low efficiency. They cannot effectively cover a wide range of electromagnetic frequency bands, and it is difficult to meet the growing demand for electromagnetic shielding. The narrow frequency domain means that the material can only provide effective electromagnetic shielding within a specific frequency band, while the effect is greatly reduced in other frequency bands. Low efficiency means that even within these specific frequency bands, the shielding effect of the material is not satisfactory, and it is difficult to achieve the expected shielding effect. Therefore, the development of an electromagnetic shielding material with wide frequency domain and high efficiency has become an urgent need in this field. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The present invention provides a wide-band high-efficiency electromagnetic shielding resin material and a preparation method thereof, so as to solve the technical problems of narrow frequency range and low efficiency of existing electromagnetic shielding materials.
[0006] (II) Technical solution
[0007] In order to solve the above technical problems, the present invention proposes a method for preparing a wide-band high-efficiency electromagnetic shielding resin material, the preparation method comprising the following steps:
[0008] S1. dispersing the coupling agent in ethyl acetate and ultrasonicating to obtain a coupling agent solution;
[0009] S2. dispersing the conductive filler in the coupling agent solution and stirring magnetically to obtain a suspension;
[0010] S3. The suspension is homogenized, filtered, and dried to obtain a modified conductive filler;
[0011] S4. The modified conductive filler and the thermosetting resin matrix are added to a disperser and stirred to obtain a modified conductive filler / thermosetting resin composite suspension;
[0012] S5. Add a curing agent to the modified conductive filler / thermosetting resin composite suspension, stir, and heat and cure to obtain an electromagnetic shielding resin material.
[0013] Furthermore, the preparation method comprises the following steps:
[0014] S1. Disperse 50 ml of coupling agent in 300 ml of ethyl acetate and ultrasonicate at 500 W for 2 h to obtain a coupling agent solution;
[0015] S2. Disperse 100 g of the conductive filler in the coupling agent solution and stir magnetically for 1 h to obtain a suspension;
[0016] S3. The suspension is added to a homogenizer for homogenization, filtered, and dried to obtain a modified conductive filler;
[0017] S4. The modified conductive filler and the thermosetting resin matrix were added to a disperser and stirred at 800 rpm for 30 min to obtain a modified conductive filler / thermosetting resin composite suspension;
[0018] S5. Add a curing agent to the modified conductive filler / thermosetting resin composite suspension, stir for 1 hour at 23° C., and heat and cure to obtain an electromagnetic shielding resin material.
[0019] Furthermore, the coupling agent is a titanate coupling agent or an aluminate coupling agent.
[0020] Furthermore, the conductive filler is one or more of silver-plated glass beads, nickel-plated glass beads, silver-plated glass powder, nickel-plated glass powder, nickel-plated graphite sheets, and stainless steel fibers.
[0021] Furthermore, in step S3, the homogenization conditions in the homogenizer are a working pressure of 200 to 400 bar and a homogenization treatment time of 20 to 50 seconds.
[0022] Furthermore, the thermosetting resin is one of epoxy resin, cast polyurethane and unsaturated resin.
[0023] Furthermore, the curing agent is one of pentaethylenetetramine, 4,4'-methylenebis(2-chloroaniline), and di-tert-butyl peroxide.
[0024] Furthermore, the temperature-raising curing condition is a gradient heating, and the temperature range is 150-220°C.
[0025] In addition, the present invention also proposes a broadband high-performance electromagnetic shielding resin material, which is prepared by the above method.
[0026] Furthermore, the wide-band high-efficiency electromagnetic shielding resin material has a shielding effect on electromagnetic waves of 2 MHz to 40 GHz.
[0027] (III) Beneficial effects
[0028] The present invention proposes a wide-band high-efficiency electromagnetic shielding resin material and a preparation method thereof. Conductive particles are used as conductive fillers, and the additives are coated on the surface of the conductive particles through specific additives and production processes to form a microsphere structure with a core and a shell tightly combined. This structure can improve the dispersibility and bonding strength of the conductive filler in the resin matrix, improve the mechanical properties and stability of the material, and make the composite material have wide-band and high-efficiency characteristics, which meets the current growing demand for electromagnetic shielding, has a good shielding effect on electromagnetic waves of 2MHz to 40GHz, and can be widely used in electronic equipment, communication equipment, aerospace and other fields. DETAILED DESCRIPTION
[0029] In order to make the purpose, content and advantages of the present invention more clear, the specific implementation methods of the present invention are further described in detail below in conjunction with embodiments.
[0030] Example 1
[0031] S1. Disperse 50 ml of titanate coupling agent NDZ-311 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0032] S2. Disperse 100 g of nickel-plated glass beads in the coupling agent solution and stir magnetically for 1 h to obtain a suspension;
[0033] S3. The suspension was added to a homogenizer, homogenized for 50 seconds at a working pressure of 200 bar, filtered, and dried to obtain a modified conductive filler;
[0034] S4. The modified conductive filler and 400g of epoxy resin were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / epoxy resin composite suspension;
[0035] S5. Add 20 g of pentaethylenetetramine curing agent to the modified conductive filler / epoxy resin composite suspension, stir for 1 hour at 23°C, and perform temperature curing according to the temperature rising conditions (150°C / 1h; 170°C / 1h; 190°C / 2h) to obtain an electromagnetic shielding resin material.
[0036] The volume resistivity and shielding performance tests were conducted on the prepared electromagnetic shielding resin material. The volume resistivity test was conducted in accordance with GB / T 15662-1995 Conductive and antistatic plastic volume resistivity test method to test the volume resistivity of electromagnetic shielding composite materials. The shielding performance test used a waveguide mold of a vector network analyzer (Agilent PNAN5244A) to test the electromagnetic shielding performance of the electromagnetic shielding composite material. The test frequency range was 2MHz to 40GHz. The volume resistivity of the prepared electromagnetic shielding resin material was 2.7×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -20dB, and the shielding effectiveness peak is -45.2dB.
[0037] Example 2
[0038] S1. Disperse 50 ml of titanate coupling agent NDZ-311 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0039] S2. 100 g of silver-plated glass beads and nickel-plated glass powder (silver-plated glass beads: nickel-plated glass powder = 1:1) were dispersed in the coupling agent solution and magnetically stirred for 1 h to obtain a suspension;
[0040] S3. The suspension was added to a homogenizer, homogenized for 35 seconds at a working pressure of 300 bar, filtered, and dried to obtain a modified conductive filler;
[0041] S4. The modified conductive filler and 400g of epoxy resin were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / epoxy resin composite suspension;
[0042] S5. Add 16 g of 4,4'-methylenebis(2-chloroaniline) curing agent to the modified conductive filler / epoxy resin composite suspension, stir for 1 hour at 23°C, and perform temperature curing according to the temperature increase conditions (170°C / 1h; 190°C / 1h; 210°C / 2h) to obtain an electromagnetic shielding resin material.
[0043] The volume resistivity of the prepared electromagnetic shielding resin material was 1.2×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -20dB, and the shielding effectiveness peak is -51.4dB.
[0044] Example 3
[0045] S1. Disperse 50 ml of aluminate coupling agent LD-B-1 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0046] S2. 100 g of silver-coated glass powder and nickel-coated graphite sheet (silver-coated glass powder: nickel-coated graphite sheet = 1:1) were dispersed in the coupling agent solution and magnetically stirred for 1 h to obtain a suspension;
[0047] S3. The suspension was added to a homogenizer, homogenized for 25 seconds at a working pressure of 300 bar, filtered, and dried to obtain a modified conductive filler;
[0048] S4. The modified conductive filler and 400g cast polyurethane were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / cast polyurethane composite suspension;
[0049] S5. Add 16g of 4,4'-methylenebis(2-chloroaniline) curing agent to the modified conductive filler / cast polyurethane composite suspension, stir for 1h at 23°C, and perform temperature curing according to the temperature rising conditions (80°C / 2h; 110°C / 12h) to obtain an electromagnetic shielding resin material.
[0050] The volume resistivity of the prepared electromagnetic shielding resin material was 7.5×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is not less than -15dB, and the peak shielding effectiveness is -31.9dB.
[0051] Example 4
[0052] S1. Disperse 50 ml of aluminate coupling agent LD-B-1 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0053] S2. Disperse 100 g of nickel-plated glass powder in the coupling agent solution and stir magnetically for 1 h to obtain a suspension;
[0054] S3. The suspension was added to a homogenizer, homogenized for 20 seconds at a working pressure of 400 bar, filtered, and dried to obtain a modified conductive filler;
[0055] S4. The modified conductive filler and 400g cast polyurethane were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / cast polyurethane composite suspension;
[0056] S5. Add 16g of 4,4'-methylenebis(2-chloroaniline) curing agent to the modified conductive filler / cast polyurethane composite suspension, stir for 1h at 23°C, and perform temperature curing according to the temperature rising conditions (80°C / 2h; 110°C / 12h) to obtain an electromagnetic shielding resin material.
[0057] The volume resistivity of the prepared electromagnetic shielding resin material was 6.8×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -15dB, and the peak shielding effectiveness is -35.6dB.
[0058] Example 5
[0059] S1. Disperse 50 ml of aluminate coupling agent LD-B-1 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0060] S2. 100 g of stainless steel fiber and nickel-plated graphite sheet (stainless steel fiber: nickel-plated graphite sheet = 1:1) were dispersed in the coupling agent solution and magnetically stirred for 1 h to obtain a suspension;
[0061] S3. The suspension was added to a homogenizer, homogenized for 20 seconds at a working pressure of 400 bar, filtered, and dried to obtain a modified conductive filler;
[0062] S4. The modified conductive filler and 400g of unsaturated resin were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / unsaturated resin composite suspension;
[0063] S5. Add 16 g of di-tert-butyl peroxide curing agent to the modified conductive filler / unsaturated resin composite suspension, stir for 1 h at 23 ° C, and heat cure according to the heating conditions (60 ° C / 1 h; 85 ° C / 4 h) to obtain an electromagnetic shielding resin material
[0064] The volume resistivity of the prepared electromagnetic shielding resin material was 1.7×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -15dB, and the shielding effectiveness peak is -48.6dB.
[0065] Example 6
[0066] S1. Disperse 50 ml of aluminate coupling agent LD-B-1 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0067] S2. 100 g of nickel-plated glass beads and silver-plated glass beads (nickel-plated glass beads: silver-plated glass beads = 1:1) were dispersed in the coupling agent solution and magnetically stirred for 1 h to obtain a suspension;
[0068] S3. The suspension was added to a homogenizer, homogenized for 50 seconds at a working pressure of 200 bar, filtered, and dried to obtain a modified conductive filler;
[0069] S4. The modified conductive filler and 100g of unsaturated resin were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / unsaturated resin composite suspension;
[0070] S5. Add 16 g of di-tert-butyl peroxide curing agent to the modified conductive filler / unsaturated resin composite suspension, stir for 1 hour at 23°C, and perform temperature curing according to the temperature increase conditions (60°C / 1h; 85°C / 4h) to obtain an electromagnetic shielding resin material.
[0071] The volume resistivity of the prepared electromagnetic shielding resin material is 3.8×10 -2 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -20dB, and the peak shielding effectiveness is -41.6dB.
[0072] Comparative Example 1
[0073] S1. 100 g of unmodified nickel-plated glass beads and 400 g of epoxy resin were added to a high-speed disperser and stirred at 800 rpm for 30 min to obtain a conductive filler / epoxy resin composite suspension;
[0074] S2. Add 20 g of pentaethylenetetramine curing agent to the conductive filler / epoxy resin composite suspension, stir for 1 hour at 23°C, and perform temperature curing according to the temperature increase conditions (150°C / 1h; 170°C / 1h; 190°C / 2h) to obtain an electromagnetic shielding resin material.
[0075] The volume resistivity of the prepared electromagnetic shielding resin material is 3.5×10 -1 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is not less than -5dB, and the peak shielding effectiveness is -28.6dB.
[0076] Comparative Example 2
[0077] S1. Disperse 50 ml of silane coupling agent KH550 in 300 ml of ethyl acetate and ultrasonicate for 2 h at a power of 500 W to obtain a coupling agent solution;
[0078] S2. 100 g of silver-coated glass powder and nickel-coated graphite sheet (silver-coated glass powder: nickel-coated graphite sheet = 1:1) were dispersed in the coupling agent solution and magnetically stirred for 1 h to obtain a suspension;
[0079] S3. The modified conductive filler and 400g cast polyurethane were added to a high-speed disperser and stirred at 800rpm for 30min to obtain a modified conductive filler / cast polyurethane composite suspension;
[0080] S4. Add 16g of 4,4'-methylenebis(2-chloroaniline) curing agent to the modified conductive filler / cast polyurethane composite suspension, stir for 1h at 23°C, and perform temperature curing according to the temperature rising conditions (80°C / 2h; 110°C / 12h) to obtain an electromagnetic shielding resin material.
[0081] The volume resistivity of the prepared electromagnetic shielding resin material is 8.7×10 -1 Ω.m; the electromagnetic shielding efficiency from 2MHz to 40GHz is no less than -5dB, and the peak shielding effectiveness is -24.9dB.
[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a wide-band high-performance electromagnetic shielding resin material, characterized in that: The preparation method comprises the following steps: S1. dispersing the coupling agent in ethyl acetate and ultrasonicating to obtain a coupling agent solution; S2. dispersing the conductive filler in the coupling agent solution and stirring magnetically to obtain a suspension; S3. The suspension is homogenized, filtered, and dried to obtain a modified conductive filler; S4. The modified conductive filler and the thermosetting resin matrix are added to a disperser and stirred to obtain a modified conductive filler / thermosetting resin composite suspension; S5. Add a curing agent to the modified conductive filler / thermosetting resin composite suspension, stir, and heat and cure to obtain an electromagnetic shielding resin material.
2. The method for preparing a wide-band high-performance electromagnetic shielding resin material according to claim 1, characterized in that: The preparation method comprises the following steps: S1. Disperse 50 ml of coupling agent in 300 ml of ethyl acetate and ultrasonicate at 500 W for 2 h to obtain a coupling agent solution; S2. Disperse 100 g of the conductive filler in the coupling agent solution and stir magnetically for 1 h to obtain a suspension; S3. The suspension is added to a homogenizer for homogenization, filtered, and dried to obtain a modified conductive filler; S4. The modified conductive filler and the thermosetting resin matrix were added to a disperser and stirred at 800 rpm for 30 min to obtain a modified conductive filler / thermosetting resin composite suspension; S5. Add a curing agent to the modified conductive filler / thermosetting resin composite suspension, stir for 1 hour at 23° C., and heat and cure to obtain an electromagnetic shielding resin material.
3. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: The coupling agent is a titanate coupling agent or an aluminate coupling agent.
4. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: The conductive filler is one or more of silver-plated glass microbeads, nickel-plated glass microbeads, silver-plated glass powder, nickel-plated glass powder, nickel-plated graphite sheets, and stainless steel fibers.
5. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: In step S3, the homogenization conditions in the homogenizer are a working pressure of 200 to 400 bar and a homogenization time of 20 to 50 seconds.
6. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: The thermosetting resin is one of epoxy resin, cast polyurethane and unsaturated resin.
7. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: The curing agent is one of pentaethylenetetramine, 4,4'-methylenebis(2-chloroaniline) and di-tert-butyl peroxide.
8. The method for preparing a wide-band high-efficiency electromagnetic shielding resin material according to claim 1 or 2, characterized in that: The temperature rise curing condition is a gradient temperature rise, and the temperature range is 150-220°C.
9. A wide-band high-performance electromagnetic shielding resin material, characterized in that: The electromagnetic shielding resin material is prepared by the method according to any one of claims 1 to 8.
10. The wide-band high-efficiency electromagnetic shielding resin material according to claim 9, characterized in that: The wide-band high-efficiency electromagnetic shielding resin material has a shielding effect on electromagnetic waves of 2 MHz to 40 GHz.