A super weather-resistant roof waterproof coating
By using specific group distribution and dispersion technology in polymer cement-based waterproof coatings, a high-density interpenetrating network structure is formed, which solves the problem of insufficient weather resistance of polymer cement-based waterproof coatings in roof applications, and realizes the roof waterproof layer high weather resistance and stability.
Patent Information
- Application Number
- CN202411265977.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polymer cement-based waterproof coatings have poor weather resistance in roof applications and are difficult to waterproof for a long time, especially in wind, sun, rain, snow, frost and dew, and repeated freeze-thawing conditions, water resistance and cracking problems are prone to deterioration and cracking.
Component A and component B are mixed in mass ratio of 10:7 to 20. Component A includes polyacrylate emulsion, rubber-coated nanosilica, modified lignin emulsion and defoaming agent. Component B includes silicon Acid cement and quartz powder, and through specific dispersion and crosslinking agent formulations, a high-density interpenetrating network structure is formed to improve the mechanical properties and weather resistance of the coating.
It significantly improves the low temperature resistance, freeze-thaw resistance and weather resistance of the coating, ensures the long-term stability and weather resistance of the roof waterproof layer, and meets the needs of roof waterproofing.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a super weather-resistant roof waterproof coating, belonging to the technical field of coatings. Background Art
[0002] Roofing was not originally the main market for waterproof coatings. Due to changes in roof design, there are more sloping roofs, and there are also requirements for the shape of sloping roofs, which increases the irregular parts of the roof, making it inconvenient to use waterproof membranes. The convenience of waterproof coatings for easy construction makes them very suitable for roof waterproofing. At present, roof waterproof coatings mainly include polyurethane, modified asphalt, acrylic and JS waterproof coatings. Among the above four types of waterproof coatings, JS waterproof coatings have relatively good performance and are used in large quantities, and have attracted much attention in the building waterproofing industry.
[0003] JS waterproof coating, full name polymer cement-based waterproof coating, is a two-component waterproof coating with water-based polymer emulsion and cement as the main body. The two components are stirred into a uniform and fine slurry at the construction site, brushed or sprayed on the surface of the substrate, and formed into a flexible and high-strength waterproof film after curing. This coating has the advantages of high strength of cement-based cementitious materials and easy adhesion to moist base surfaces, as well as high elasticity and good waterproof properties of polymer coatings. In particular, the water-based system with water as the carrier avoids the disadvantages of asphalt, tar, and organic solvent-based environmental pollution. It is a green and environmentally friendly waterproof coating that is non-toxic, harmless, wet-operable, and easy to construct. Since the end of the 20th century, polymer cement-based waterproof coatings have been listed as 13 recommended waterproof materials by the Ministry of Housing and Urban-Rural Development, and have been widely used in scenes such as building exterior walls, roofs, kitchens, toilets and bathrooms, underground buildings, and bridges. However, in actual applications, when polymer cement waterproof coatings are used for roof waterproofing, they are exposed to harsh natural conditions such as wind, sun, rain, snow, frost, day and night temperature differences, and repeated freezing and thawing for a long time, and their water resistance will gradually deteriorate and cracks will appear. In short, the weather resistance of the current polymer cement waterproof coatings is difficult to guarantee the long-term use effect of roof waterproofing. Therefore, it is urgent to develop JS waterproof coatings with excellent weather resistance to meet the needs of long-term roof waterproofing.
[0004] Chinese patent CN112341878A discloses a polymer cement waterproof coating, a roof waterproof layer and a preparation method thereof. The coating comprises a liquid and a powder in a mass ratio of 1:1 to 1.3; the liquid comprises: 59 to 88% acrylic emulsion, 5 to 30% ethylene-polyvinyl acetate copolymer emulsion, 3 to 5% styrene-butadiene emulsion, 0.1 to 0.7% defoamer and 1 to 5.5% water; the powder comprises: 25 to 35% cement; 32.5 to 44.5% quartz powder; 20 to 30% talc; and 1.5 to 3.5% wollastonite; the roof waterproof layer comprises a coating layer and a base fabric layer made of the aforementioned coating. The technical problem to be solved is to improve the defects of the existing JS waterproof coating, so that the polymer cement waterproof coating has good fluidity and permeability. The polymer cement waterproof coating layer made of it is alternately arranged with the polyester non-woven fabric to form an overall roof waterproof layer, and its tensile strength, heat resistance and UV resistance are significantly improved; under the action of various aging factors, the elongation at break of the roof waterproof layer is reduced, the dimensional stability is enhanced, and the weather resistance is significantly improved, so it is more suitable for practical use. The polymer cement waterproof coating obtained by this patent needs to be used in conjunction with polyester non-woven fabric to achieve good weather resistance, and the convenience of construction is poor. When used for roofs with special designs, the construction process is very difficult.
[0005] Chinese patent CN116004073A discloses a polymer cement waterproof coating, comprising a liquid and a powder; the liquid comprises 100 parts of modified acrylate emulsion by weight; the powder comprises 35 to 60 parts of silicate cement, 10 to 25 parts of filler, and 2 to 15 parts of tannic acid by weight; the modified acrylate emulsion is prepared by reacting methyl acrylate, butyl acrylate, and terminal olefin epoxy resin in a mass ratio of 10: (20 to 30): (5 to 15). The polymer cement waterproof coating of the present application has the advantage of good water resistance. Although the polymer cement waterproof coating prepared by the patent has good water resistance, many bio-based polymer components are added, and the light aging and heat aging effects of these components are not ideal, so the weather resistance is difficult to meet the requirements of roof waterproofing.
[0006] From the above, we can see that the current polymer cement-based waterproof coatings still have poor weather resistance and are difficult to be used for roof waterproofing for a long time. Therefore, it is of great practical significance to develop a super weather-resistant roof waterproof coating. Summary of the invention
[0007] In view of the deficiencies in the above-mentioned prior art, the present invention provides a super weather-resistant roof waterproof coating to achieve the following invention objectives: to prepare a super weather-resistant polymer cement waterproof coating for roof waterproofing that is resistant to light aging, heat aging and freeze-thaw cycles.
[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0009] A super weather-resistant roof waterproof coating, the super weather-resistant roof waterproof coating consists of component A and component B, and when used, component A and component B are mixed in a mass ratio of 10:7 to 20;
[0010] The specific formula of the component A is, in parts by weight:
[0011] Polyacrylate emulsion 200 to 300 parts,
[0012] 5 to 20 parts of rubber-coated nano-silicon dioxide,
[0013] 20 to 50 parts of modified lignin emulsion,
[0014] 2 to 6 parts of film-forming aid,
[0015] 3 to 9 parts of plasticizer,
[0016] 1 to 3 parts of defoamer,
[0017] 20 to 50 parts of deionized water;
[0018] The polyacrylate emulsion has a solid content of 45 to 65%, a viscosity of 1000 to 5000 mPa·s, and a pH value of 5.5 to 7;
[0019] The film-forming aid is propylene glycol methyl ether acetate;
[0020] The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol;
[0021] The mass ratio of triacetin to 1,2,6-hexanetriol is 1 to 15:30;
[0022] The defoamer is tributyl phosphate;
[0023] The specific formula of the B component is, in parts by weight:
[0024] 130 to 170 parts of Portland cement,
[0025] 30 to 80 parts of quartz powder,
[0026] 5 to 10 parts of auxiliary crosslinking agent,
[0027] 15 to 30 parts of a cross-linking agent;
[0028] The quartz powder has a particle size of 0.05 to 3 μm;
[0029] The auxiliary cross-linking agent is one of 1,2,3,4-butanetetracarboxylic acid and 1,3,5-pentanetricarboxylic acid;
[0030] The cross-linking agent is one of N-hydroxyethyl acrylamide, N-hydroxymethyl acrylamide, N-(2-hydroxypropyl) methacrylamide and diacetone acrylamide;
[0031] The following are further improvements to the above technical solution:
[0032] Step 1: Preparation of rubber-coated nano-silica
[0033] Add nano silicon dioxide, toluene and triisobutyl phosphate into a high-speed dispersion kettle, control the dispersion rate at 8800 to 10000 rpm, disperse vigorously for 6 to 12 hours, reduce the dispersion rate to 2000 to 4000 rpm, raise the temperature and keep the temperature constant at 60 to 80° C., then add 3-isocyanate propyl triethoxysilane, react for 5 to 9 hours, add liquid rubber, continue to react at a constant temperature for 5 to 11 hours, cool to room temperature, centrifuge, wash the separated solid with ethanol for 2 to 4 times, put it into a vacuum oven, dry it at 30 to 50° C. for 6 to 9 hours, and obtain rubber-coated nano silicon dioxide;
[0034] The particle size of the nano silicon dioxide is 10 to 100 nm;
[0035] The liquid rubber is one of carboxyl-terminated liquid nitrile rubber and carboxyl-terminated liquid polybutadiene rubber;
[0036] The molecular weight of the liquid rubber is 1000 to 9000 g / mol;
[0037] The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 35 to 50: 230 to 350: 3 to 6: 2.5 to 5.5: 8 to 14.
[0038] Step 2: Preparation of modified lignin emulsion
[0039] Add lignin powder and anhydrous ethanol to a reactor, control the temperature at 30 to 50° C., vigorously stir and disperse at 3000 to 5000 rpm for 4 to 8 hours, reduce the stirring rate to 900 to 1500 rpm, add potassium hydroxide to adjust the pH value of the reaction system to 8 to 9, add maleic anhydride, stir and react at constant temperature for 6 to 13 hours, then reduce the temperature to room temperature, add citric acid aqueous solution to adjust the pH value of the reaction system to 3 to 4, continue to stir at room temperature for 2 to 5 hours, fully acidify, centrifuge to obtain maleic anhydride modified lignin, then add the maleic anhydride modified lignin to a high-speed dispersion kettle, add deionized water, control the dispersion rate at 5000 to 9000 rpm, stir and disperse for 6 to 10 hours, then add water-soluble amino silicone oil, continue to disperse and emulsify for 7 to 12 hours, and obtain a uniform and stable emulsion, which is a modified lignin emulsion;
[0040] The particle size of the lignin powder is 0.5 to 6 μm;
[0041] The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 20 to 45:150 to 210:5 to 10;
[0042] The citric acid aqueous solution has a citric acid content of 30 to 50 wt %;
[0043] The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 30 to 55:120 to 220:4 to 8;
[0044] The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 500 to 1200 mPa·s.
[0045] Step 3: Preparation of component A
[0046] According to the specific formula of component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersing kettle, and vigorously dispersed at a speed of 6000 to 9000 rpm for 3 to 6 hours, and then polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added. After continuing to vigorously disperse for 1 to 4 hours, the material is filled into a plastic packaging barrel to obtain component A.
[0047] Step 4: Preparation of component B
[0048] According to the specific formula of component B in parts by weight, silicate cement, quartz powder, auxiliary cross-linking agent and cross-linking agent are placed in a V-shaped powder mixing kettle, the mixing speed is controlled at 90 to 160 rpm, and the mixing is continued for 9 to 14 hours, and then the material is discharged and packed into a moisture-proof packaging bag to obtain component B.
[0049] Compared with the prior art, the present invention achieves the following beneficial effects:
[0050] 1. The present invention uses triisobutyl phosphate as a dispersant, and firstly disperses nano-silica uniformly in a toluene solution. After the nano-scale dispersed nano-silica is modified by 3-isocyanate propyl triethoxysilane, the surface is covered with isocyanate functional groups or ethoxysilane functional groups. After adding carboxyl-terminated liquid nitrile rubber or carboxyl-terminated liquid polybutadiene rubber, the isocyanate functional groups or ethoxysilane react with the carboxyl groups, and the surface of the nano-silica is uniformly wrapped with rubber molecular chains. The wrapped rubber polymers still have unreacted carboxyl groups at the ends, which retains the polarity of the nano-silica and makes it easy to obtain in an aqueous system. After the rubber-wrapped nano-silica is evenly dispersed and solidified in the coating, the rubber layer on the surface is in close contact with the inorganic particles in the polymer cement coating and is closely complexed with the calcium ions in the cement through the carboxyl group and finally forms an ionic bond, forming a rubber inorganic particle transition layer with very good flexibility and elasticity. Because the carboxyl-terminated liquid nitrile rubber and the carboxyl-terminated liquid polybutadiene rubber have very excellent low temperature resistance, flexibility and weather resistance, the above-mentioned organic-inorganic transition structure plays a very key role in improving the low temperature resistance, freeze-thaw resistance and weather resistance of the polymer cement waterproof coating.
[0051] 2. In the present invention, maleic anhydride is used to modify lignin in a strong base reaction system constructed by an ethanol solution of potassium hydroxide. The phenolic hydroxyl groups in the lignin react to form carboxyl hydroxyl structures. After the acidification treatment with citric acid, these carboxyl hydroxyl groups can maintain a terminal carboxyl state with high activity. Then, these lignin particles with high-activity terminal carboxyl groups are emulsified with water-soluble amino silicone oil to become stable microemulsion droplets suspended in the liquid system. In addition, a certain degree of neutralization reaction occurs between the high-activity terminal carboxyl groups on the surface of the lignin particles and the terminal amino groups of the amino silicone oil, so that the amino silicone oil tightly wraps the lignin particles, which further improves the stability of the modified lignin emulsion. After the modified lignin emulsion is added to the polymer cement waterproof coating formula, the coating is sprayed During the curing process of the coating, as the water escapes, the modified lignin emulsion breaks the emulsion, and due to the low surface tension of the amino silicone oil, it will migrate to the coating surface more quickly, so that the lignin particles wrapped by the amino silicone oil will also migrate to the coating surface. After the coating is cured, the lignin content on the coating surface will be significantly higher than the lignin content inside the coating. Lignin itself has very good weather resistance. After the coating surface is cured, it will give the coating extremely excellent weather resistance. In addition, there are still a lot of terminal carboxyl groups on the surface of the lignin particles. These carboxyl groups and calcium ions in the cement are combined with ionic bonds to form a denser cross-linked cured layer, which further enhances the cross-linking degree on the surface and inside of the coating, and greatly improves the mechanical properties and weather resistance of the coating.
[0052] 3. The present invention adds a highly reactive cross-linking agent such as N-hydroxyethyl acrylamide, N-hydroxymethyl acrylamide, N-(2-hydroxypropyl) methacrylamide, diacetone acrylamide, etc., and also adds a multi-carboxyl small molecule that can react with calcium ions to produce an ionic bond, 1,2,3,4-butanetetracarboxylic acid or 1,3,5-pentanetricarboxylic acid. The cross-linking agent and the polyacrylate emulsion undergo a chemical cross-linking reaction to form a dense polymer film with a high cross-linking density. The auxiliary cross-linking agent can catalyze the cross-linking reaction between the cross-linking agent and the polyacrylate emulsion. In addition, the auxiliary cross-linking agent itself also undergoes an ionic bond cross-linking reaction with calcium ions. The above two cross-linking reactions will form an interpenetrating network polymer structure to a certain extent. This highly dense interpenetrating cross-linked network can greatly improve the overall density of the coating, and endow the coating with very excellent mechanical properties and excellent weather resistance;
[0053] 4. The super weather-resistant roof waterproof coating obtained by the present invention has a surface drying time of 0.8 to 1.3 hours, a practical drying time of 2.2 to 2.7 hours, and is impermeable under the conditions of 0.3MPa and 30min. The tensile strength is 3.46 to 3.69MPa without treatment, 92 to 96% after heat treatment, 90 to 94% after alkali treatment, 95 to 99% after immersion treatment, and 90 to 94% after ultraviolet treatment; the elongation at break is 361 to 382% without treatment, and 90 to 9 4%, the retention rate of alkali treatment is 87 to 92%, the retention rate of immersion treatment is 95 to 99%, and the retention rate of UV treatment is 85 to 91%; Adhesion strength: no treatment is 1.53 to 1.66MPa, the retention rate of moist base is 90 to 94%, the retention rate of alkali treatment is 82 to 86%, the retention rate of immersion treatment is 93 to 98%, and the retention rate of UV treatment is 85 to 88%; Low temperature flexibility is -36 to -42℃, resistance to freeze-thaw destructiveness is 38 to 43 times, and the time without abnormality in resistance to artificial climate aging is 4394 to 4659 hours. DETAILED DESCRIPTION
[0054] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0055] Example 1: A super weather-resistant roof waterproof coating
[0056] Step 1: Preparation of rubber-coated nano-silica
[0057] Add nano-silica, toluene and triisobutyl phosphate into a high-speed dispersion kettle, control the dispersion rate at 9600 rpm, disperse vigorously for 8 hours, reduce the dispersion rate to 2900 rpm, raise the temperature and keep it constant at 75°C, then add 3-isocyanate propyl triethoxysilane, react for 6 hours, add liquid rubber, continue to react at constant temperature for 10 hours, cool to room temperature, centrifuge, wash the separated solid with ethanol for 3 times, put it into a vacuum oven, dry it at 39°C for 7 hours, and obtain rubber-coated nano-silica;
[0058] The particle size of the nano silicon dioxide is 60nm;
[0059] The liquid rubber is a carboxyl-terminated liquid nitrile rubber;
[0060] The molecular weight of the liquid rubber is 6500 g / mol;
[0061] The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 40:300:5:4:12.
[0062] Step 2: Preparation of modified lignin emulsion
[0063] Add lignin powder and anhydrous ethanol to a reactor, control the temperature to 45°C, vigorously stir and disperse at 4500 rpm for 5 hours, reduce the stirring rate to 1100 rpm, then add potassium hydroxide to adjust the pH value of the reaction system to 8.7, add maleic anhydride, stir and react at constant temperature for 8 hours, then reduce the temperature to room temperature, add citric acid aqueous solution to adjust the pH of the reaction system to 3.7, continue to stir at room temperature for 4 hours, fully acidify, centrifuge to obtain maleic anhydride modified lignin, then add the maleic anhydride modified lignin to a high-speed dispersion kettle, add deionized water, control the dispersion rate to 8000 rpm, stir and disperse for 9 hours, then add water-soluble amino silicone oil, continue to disperse and emulsify for 11 hours, and obtain a uniform and stable emulsion, which is a modified lignin emulsion;
[0064] The particle size of the lignin powder is 4 μm;
[0065] The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 40:180:7;
[0066] The citric acid aqueous solution has a citric acid content of 45wt%;
[0067] The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 45:190:7;
[0068] The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 1100 mPa·s.
[0069] Step 3: Preparation of component A
[0070] The specific formula of the component A is, in parts by weight:
[0071] Polyacrylate emulsion 260 parts,
[0072] Rubber coated nano silicon dioxide 13 parts,
[0073] 35 parts of modified lignin emulsion,
[0074] 5 parts of film-forming aid,
[0075] 7 parts of plasticizer,
[0076] 2 parts of defoamer,
[0077] Deionized water 29 parts;
[0078] The polyacrylate emulsion has a solid content of 49%, a viscosity of 1800 mPa·s, and a pH value of 6;
[0079] The film-forming aid is propylene glycol methyl ether acetate;
[0080] The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol;
[0081] The mass ratio of triacetin to 1,2,6-hexanetriol is 10:30;
[0082] The defoamer is tributyl phosphate;
[0083] According to the specific formula of component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersing kettle. After intensive dispersion at a speed of 7500 rpm for 5 hours, polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added. After continuing to intensively disperse for 2 hours, the material is filled into a plastic packaging barrel to obtain component A.
[0084] Step 4: Preparation of component B
[0085] The specific formula of the B component is, in parts by weight:
[0086] 160 parts of Portland cement,
[0087] 60 parts of quartz powder,
[0088] 8 parts of cross-linking agent,
[0089] 25 parts of cross-linking agent;
[0090] The quartz powder has a particle size of 2 μm;
[0091] The auxiliary cross-linking agent is 1,2,3,4-butanetetracarboxylic acid;
[0092] The cross-linking agent is N-hydroxyethyl acrylamide;
[0093] According to the specific formula of component B in parts by weight, silicate cement, quartz powder, auxiliary cross-linking agent and cross-linking agent are put into a V-shaped powder mixing kettle, the mixing speed is controlled at 130 rpm, and the mixing is continued for 11 hours, and then the material is discharged and packed into a moisture-proof packaging bag to obtain component B.
[0094] Example 2: A super weather-resistant roof waterproof coating
[0095] Step 1: Preparation of rubber-coated nano-silica
[0096] Add nano-silica, toluene and triisobutyl phosphate into a high-speed dispersion kettle, control the dispersion rate to 8800 rpm, and after intensive dispersion for 6 hours, reduce the dispersion rate to 2000 rpm, and raise the temperature and keep it constant at 60°C, then add 3-isocyanate propyl triethoxysilane, react for 5 hours, add liquid rubber, continue to react at a constant temperature for 5 hours, cool to room temperature, centrifuge, wash the separated solid with ethanol twice, put it into a vacuum oven, and dry it at 30°C for 6 hours to obtain rubber-coated nano-silica;
[0097] The particle size of the nano silicon dioxide is 10 nm;
[0098] The liquid rubber is carboxyl-terminated liquid polybutadiene rubber;
[0099] The molecular weight of the liquid rubber is 1000 g / mol;
[0100] The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 35:230:3:2.5:8.
[0101] Step 2: Preparation of modified lignin emulsion
[0102] Add lignin powder and anhydrous ethanol to a reactor, control the temperature at 30°C, vigorously stir and disperse at 3000 rpm for 4 hours, reduce the stirring rate to 900 rpm, then add potassium hydroxide to adjust the pH value of the reaction system to 8, add maleic anhydride, stir and react at constant temperature for 6 hours, then reduce the temperature to room temperature, add citric acid aqueous solution to adjust the pH of the reaction system to 3, continue to stir at room temperature for 2 hours, fully acidify, centrifuge to obtain maleic anhydride modified lignin, then add maleic anhydride modified lignin to a high-speed dispersion kettle, add deionized water, control the dispersion rate at 5000 rpm, stir and disperse for 6 hours, then add water-soluble amino silicone oil, continue to disperse and emulsify for 7 hours, and obtain a uniform and stable emulsion, which is a modified lignin emulsion;
[0103] The particle size of the lignin powder is 0.5 μm;
[0104] The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 20:150:5;
[0105] The citric acid aqueous solution has a citric acid content of 30 wt %;
[0106] The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 30:120:4;
[0107] The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 500 mPa·s.
[0108] Step 3: Preparation of component A
[0109] The specific formula of the component A is, in parts by weight:
[0110] 200 parts of polyacrylate emulsion,
[0111] 5 parts of rubber-coated nano-silicon dioxide,
[0112] 20 parts of modified lignin emulsion,
[0113] 2 parts of film-forming aid,
[0114] 3 parts of plasticizer,
[0115] 1 part defoamer,
[0116] 20 parts of deionized water;
[0117] The polyacrylate emulsion has a solid content of 45%, a viscosity of 1000 mPa·s, and a pH value of 5.5;
[0118] The film-forming aid is propylene glycol methyl ether acetate;
[0119] The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol;
[0120] The mass ratio of triacetin to 1,2,6-hexanetriol is 1:30;
[0121] The defoamer is tributyl phosphate;
[0122] According to the specific formula of component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersing kettle, and vigorously dispersed for 3 hours at a speed of 6000 rpm. Then, polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added. After continuing to vigorously disperse for 1 hour, the material is filled into a plastic packaging barrel to obtain component A.
[0123] Step 4: Preparation of component B
[0124] The specific formula of the B component is, in parts by weight:
[0125] 130 parts of Portland cement,
[0126] 30 parts of quartz powder,
[0127] 5 parts of cross-linking agent,
[0128] 15 parts of cross-linking agent;
[0129] The particle size of the quartz powder is 0.05 μm;
[0130] The auxiliary cross-linking agent is 1,3,5-pentanetricarboxylic acid;
[0131] The cross-linking agent is N-hydroxymethyl acrylamide;
[0132] According to the specific formula of component B in parts by weight, silicate cement, quartz powder, auxiliary cross-linking agent and cross-linking agent are put into a V-shaped powder mixing kettle, the mixing speed is controlled at 90 rpm, and the mixing is continued for 9 hours, and then the material is discharged and packed into a moisture-proof packaging bag to obtain component B.
[0133] Example 3: A super weather-resistant roof waterproof coating
[0134] Step 1: Preparation of rubber-coated nano-silica
[0135] Add nano-silica, toluene and triisobutyl phosphate into a high-speed dispersion kettle, control the dispersion rate at 10,000 rpm, disperse vigorously for 12 hours, reduce the dispersion rate to 4,000 rpm, raise the temperature and keep it constant at 80°C, then add 3-isocyanate propyl triethoxysilane, react for 9 hours, add liquid rubber, continue to react at a constant temperature for 11 hours, cool to room temperature, centrifuge, wash the separated solid with ethanol for 4 times, put it into a vacuum oven, dry it at 50°C for 9 hours, and obtain rubber-coated nano-silica;
[0136] The particle size of the nano silicon dioxide is 100 nm;
[0137] The liquid rubber is carboxyl-terminated liquid polybutadiene rubber;
[0138] The molecular weight of the liquid rubber is 9000 g / mol;
[0139] The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 50:350:6:5.5:14.
[0140] Step 2: Preparation of modified lignin emulsion
[0141] Add lignin powder and anhydrous ethanol to a reactor, control the temperature to 50°C, vigorously stir and disperse at 5000 rpm for 8 hours, reduce the stirring rate to 1500 rpm, then add potassium hydroxide to adjust the pH value of the reaction system to 9, add maleic anhydride, stir and react at constant temperature for 13 hours, then reduce the temperature to room temperature, add citric acid aqueous solution to adjust the pH of the reaction system to 4, continue to stir at room temperature for 5 hours, fully acidify, centrifuge to obtain maleic anhydride modified lignin, then add maleic anhydride modified lignin to a high-speed dispersion kettle, add deionized water, control the dispersion rate to 9000 rpm, stir and disperse for 10 hours, then add water-soluble amino silicone oil, continue to disperse and emulsify for 12 hours, and obtain a uniform and stable emulsion, which is a modified lignin emulsion;
[0142] The particle size of the lignin powder is 6 μm;
[0143] The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 45:10:10;
[0144] The citric acid aqueous solution has a citric acid content of 50wt%;
[0145] The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 55:220:8;
[0146] The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 1200 mPa·s.
[0147] Step 3: Preparation of component A
[0148] The specific formula of the component A is, in parts by weight:
[0149] 300 parts of polyacrylate emulsion,
[0150] 20 parts of rubber-coated nano-silicon dioxide,
[0151] 50 parts of modified lignin emulsion,
[0152] 6 parts of film-forming aid,
[0153] Plasticizer 9 parts,
[0154] 3 parts of defoamer,
[0155] 50 parts of deionized water;
[0156] The polyacrylate emulsion has a solid content of 65%, a viscosity of 5000 mPa·s, and a pH value of 7;
[0157] The film-forming aid is propylene glycol methyl ether acetate;
[0158] The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol;
[0159] The mass ratio of triacetin to 1,2,6-hexanetriol is 15:30;
[0160] The defoamer is tributyl phosphate;
[0161] According to the specific formula of component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersing kettle. After intensive dispersion at a speed of 9000 rpm for 6 hours, polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added. After continuing to intensively disperse for 4 hours, the material is filled into a plastic packaging barrel to obtain component A.
[0162] Step 4: Preparation of component B
[0163] The specific formula of the B component is, in parts by weight:
[0164] 170 parts of Portland cement,
[0165] 80 parts of quartz powder,
[0166] 10 parts of cross-linking agent,
[0167] 30 parts of cross-linking agent;
[0168] The quartz powder has a particle size of 3 μm;
[0169] The auxiliary cross-linking agent is 1,3,5-pentanetricarboxylic acid;
[0170] The cross-linking agent is N-(2-hydroxypropyl) methacrylamide;
[0171] According to the specific formula of component B in parts by weight, silicate cement, quartz powder, auxiliary cross-linking agent and cross-linking agent are placed in a V-shaped powder mixing kettle. The mixing speed is controlled at 160 rpm. After continuous mixing for 14 hours, the material is discharged and packed into a moisture-proof packaging bag to obtain component B.
[0172] Example 4: A super weather-resistant roof waterproof coating
[0173] Step 1: Preparation of rubber-coated nano-silica
[0174] Add nano-silica, toluene and triisobutyl phosphate into a high-speed dispersion kettle, control the dispersion rate at 10,000 rpm, disperse vigorously for 6 hours, reduce the dispersion rate to 4,000 rpm, raise the temperature and keep it constant at 60°C, then add 3-isocyanate propyl triethoxysilane, react for 9 hours, add liquid rubber, continue to react at a constant temperature for 11 hours, cool to room temperature, centrifuge, wash the separated solid with ethanol for 4 times, put it into a vacuum oven, dry it at 50°C for 9 hours, and obtain rubber-coated nano-silica;
[0175] The particle size of the nano silicon dioxide is 10 nm;
[0176] The liquid rubber is carboxyl-terminated liquid polybutadiene rubber;
[0177] The molecular weight of the liquid rubber is 1000 g / mol;
[0178] The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 50:350:6:2.5:8.
[0179] Step 2: Preparation of modified lignin emulsion
[0180] Add lignin powder and anhydrous ethanol to a reactor, control the temperature at 30°C, vigorously stir and disperse at 5000 rpm for 4 hours, reduce the stirring rate to 1500 rpm, then add potassium hydroxide to adjust the pH value of the reaction system to 9, add maleic anhydride, stir and react at constant temperature for 13 hours, then reduce the temperature to room temperature, add citric acid aqueous solution to adjust the pH of the reaction system to 3, continue to stir at room temperature for 5 hours, fully acidify, centrifuge to obtain maleic anhydride modified lignin, then add maleic anhydride modified lignin to a high-speed dispersion kettle, add deionized water, control the dispersion rate at 9000 rpm, stir and disperse for 10 hours, then add water-soluble amino silicone oil, continue to disperse and emulsify for 12 hours, and obtain a uniform and stable emulsion, which is a modified lignin emulsion;
[0181] The particle size of the lignin powder is 0.5 μm;
[0182] The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 20:150:5;
[0183] The citric acid aqueous solution has a citric acid content of 30 wt %;
[0184] The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 55:220:8;
[0185] The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 1200 mPa·s.
[0186] Step 3: Preparation of component A
[0187] The specific formula of the component A is, in parts by weight:
[0188] 300 parts of polyacrylate emulsion,
[0189] 20 parts of rubber-coated nano-silicon dioxide,
[0190] 50 parts of modified lignin emulsion,
[0191] 6 parts of film-forming aid,
[0192] Plasticizer 9 parts,
[0193] 3 parts of defoamer,
[0194] 50 parts of deionized water;
[0195] The polyacrylate emulsion has a solid content of 65%, a viscosity of 1000 mPa·s, and a pH value of 5.5;
[0196] The film-forming aid is propylene glycol methyl ether acetate;
[0197] The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol;
[0198] The mass ratio of triacetin to 1,2,6-hexanetriol is 1:30;
[0199] The defoamer is tributyl phosphate;
[0200] According to the specific formula of component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersing kettle, and vigorously dispersed at a speed of 9000 rpm for 6 hours. Then, polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added. After continuing to vigorously disperse for 1 hour, the material is filled into a plastic packaging barrel to obtain component A.
[0201] Step 4: Preparation of component B
[0202] The specific formula of the B component is, in parts by weight:
[0203] 130 parts of Portland cement,
[0204] 80 parts of quartz powder,
[0205] 5 parts of cross-linking agent,
[0206] 30 parts of cross-linking agent;
[0207] The quartz powder has a particle size of 3 μm;
[0208] The auxiliary cross-linking agent is 1,2,3,4-butanetetracarboxylic acid;
[0209] The cross-linking agent is diacetone acrylamide;
[0210] According to the specific formula of component B in parts by weight, silicate cement, quartz powder, auxiliary cross-linking agent and cross-linking agent are placed in a V-shaped powder mixing kettle. The mixing speed is controlled at 160 rpm. After continuous mixing for 9 hours, the material is discharged and packed into a moisture-proof packaging bag to obtain component B.
[0211] Comparative Example 1: Based on Example 1, step 1, preparation of rubber-coated nano-silicon dioxide, is not performed. In step 3, preparation of component A, 13 parts of rubber-coated nano-silicon dioxide are replaced by 13 parts of nano-silicon dioxide. The specific operation is as follows:
[0212] Step 1, preparation of rubber-coated nano-silica is not performed;
[0213] The operation of step 2 is the same as that of embodiment 1;
[0214] Step 3: Preparation of component A
[0215] 13 parts of rubber-coated nano-silicon dioxide were replaced by 13 parts of nano-silicon dioxide, and the other operations were the same as in Example 1;
[0216] The particle size of the nano silicon dioxide is 60nm;
[0217] The operation of step 4 is the same as that of embodiment 1.
[0218] Comparative Example 2: Based on Example 1, step 2, preparation of modified lignin emulsion, was not performed. In step 3, preparation of component A, 35 parts of modified lignin emulsion were replaced by 35 parts of polyacrylate emulsion. The specific operation was as follows:
[0219] The operation of step 1 is the same as that of embodiment 1;
[0220] Step 2, preparation of modified lignin emulsion is not performed;
[0221] Step 3: Preparation of component A
[0222] 35 parts of modified lignin emulsion were replaced by 35 parts of polyacrylate emulsion, and other operations were the same as in Example 1;
[0223] The operation of step 4 is the same as that of embodiment 1.
[0224] Comparative Example 3: Based on Example 1, in step 4, in the preparation of component B, no auxiliary cross-linking agent is added, and 8 parts of the auxiliary cross-linking agent are replaced by 8 parts of Portland cement in equal amounts. The specific operation is as follows:
[0225] The operations of steps 1, 2, and 3 are the same as those of Example 1;
[0226] Step 4: Preparation of component B
[0227] 8 parts of the auxiliary cross-linking agent were replaced by 8 parts of silicate cement, and the other operations were the same as in Example 1.
[0228] The super weather-resistant roof waterproof coatings obtained in Examples 1, 2, 3, 4 and Comparative Examples 1, 2, 3, component A and component B were mixed in a mass ratio of 1:1 for spraying, and the surface drying time, actual drying time, tensile strength, elongation at break, bonding strength, low-temperature flexibility, freeze-thaw damage resistance, resistance to artificial weathering and other performance indicators were tested with reference to GB / T23445-2009 "Polymer Cement Waterproof Coatings", JC / T 894-2001 "Polymer Cement Waterproof Coatings", and GB / T 1865-2009 "Artificial Weathering and Artificial Radiation Exposure to Filtered Xenon Arc Radiation of Paints and Varnishes". The specific test data are shown in Table 1;
[0229] Table 1
[0230]
[0231] From the data in Table 1, it can be seen that in Comparative Example 1, in which nano-silica is directly added without rubber coating, the surface drying time and the actual drying time are slightly different from those of the embodiments, and the tensile strength, elongation at break, and bonding strength are all significantly less than those of the four embodiments. Moreover, after heat treatment, alkali treatment, water immersion treatment, and UV treatment, the retention rate of mechanical properties is greatly reduced, and the low-temperature flexibility is reduced to the worst, only -19°C, and the freeze-thaw resistance and artificial aging resistance are also sharply reduced. This shows that nano-silica is not coated with rubber, and it is difficult to obtain a good dispersion in the coating body. It may be due to agglomeration that it is difficult to play the role of nano-silica in strengthening and toughening the coating and improving weather resistance. On the contrary, excessive agglomeration may hinder the normal curing of the coating, resulting in a comprehensive decline in mechanical properties and weather resistance. On the other hand, the carboxyl-terminated liquid nitrile rubber and carboxyl-terminated liquid polybutadiene rubber coated with nano-silica have very good low-temperature flexibility and weather resistance. It may also be due to the lack of coating of these two liquid rubbers that the mechanical properties of the coating, especially the low-temperature resistance, are greatly reduced, and the weather resistance is also significantly reduced. In Comparative Example 2, in which the modified lignin emulsion is not added, the surface drying time and the actual drying time are greatly extended. The three mechanical properties of tensile strength, elongation at break, and bonding strength are improved after heat treatment, alkali treatment, immersion treatment, and UV treatment compared with Example 2. , all of which have greatly decreased, among which the mechanical properties after heat treatment and UV treatment decreased significantly, which shows that the modified lignin emulsion can not only improve the curing rate, but also greatly improve the heat aging and light aging resistance of the coating. In addition, the low-temperature flexibility and freeze-thaw damage resistance of Comparative Example 2 are also significantly reduced, especially the artificial weathering aging resistance, which is reduced to the lowest value of all embodiments and comparative examples. This shows that the modified lignin emulsion not only plays a vital role in improving the weather resistance of the coating, but also plays a very significant role in the low-temperature resistance of the coating; in Comparative Example 3 without adding a co-crosslinking agent, the surface drying time and actual drying time are greatly increased, which shows that the co-crosslinking agent can accelerate the surface drying of the coating. The curing rates of the surface and interior are similar to those of Comparative Example 1, and the tensile strength, elongation at break and bonding strength are significantly reduced, but the reduction is less than that of Comparative Example 1. The retention rates after heat treatment, alkali treatment, water immersion and UV treatment are also similar to those of Comparative Example 1, but the reduction is generally less than that of Comparative Example 1, which shows that the co-crosslinking agent plays a very significant positive role in improving the various mechanical properties of the coating, and the low-temperature flexibility, freeze-thaw resistance and artificial climate aging resistance are significantly reduced, which shows that the co-crosslinking agent can effectively improve the low-temperature resistance and weather resistance of the coating, which may be because the co-crosslinking agent improves the cross-linking density of the coating, thereby improving the low-temperature resistance and weather resistance of the coating.The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A super weather-resistant roof waterproof coating, characterized in that: The super weather-resistant roof waterproof coating consists of component A and component B, which are mixed in a mass ratio of 10:7 to 20 during use; The specific formula of the component A is, in parts by weight: Polyacrylate emulsion 200 to 300 parts, 5 to 20 parts of rubber-coated nano-silicon dioxide, 20 to 50 parts of modified lignin emulsion, 2 to 6 parts of film-forming aid, 3 to 9 parts of plasticizer, 1 to 3 parts of defoamer, 20 to 50 parts of deionized water; The polyacrylate emulsion has a solid content of 45 to 65%, a viscosity of 1000 to 5000 mPa·s, and a pH value of 5.5 to 7; The film-forming aid is propylene glycol methyl ether acetate; The plasticizer is a mixture of triacetin and 1,2,6-hexanetriol; The mass ratio of triacetin to 1,2,6-hexanetriol is 1 to 15:30; The defoamer is tributyl phosphate; The specific formula of the B component is, in parts by weight: 130 to 170 parts of Portland cement, 30 to 80 parts of quartz powder, 5 to 10 parts of auxiliary crosslinking agent, 15 to 30 parts of a cross-linking agent; The quartz powder has a particle size of 0.05 to 3 μm; The auxiliary cross-linking agent is one of 1,2,3,4-butanetetracarboxylic acid and 1,3,5-pentanetricarboxylic acid; The cross-linking agent is one of N-hydroxyethyl acrylamide, N-hydroxymethyl acrylamide, N-(2-hydroxypropyl) methacrylamide and diacetone acrylamide; The rubber-coated nano-silica is prepared by: adding nano-silica, toluene and triisobutyl phosphate to a high-speed dispersion kettle, controlling the dispersion rate to 8800 to 10000 rpm, dispersing vigorously for 6 to 12 hours, reducing the dispersion rate to 2000 to 4000 rpm, and simultaneously raising the temperature and keeping the temperature constant at 60 to 80° C., then adding 3-isocyanate propyl triethoxysilane, reacting for 5 to 9 hours, adding liquid rubber, continuing the constant temperature reaction for 5 to 11 hours, cooling to room temperature, centrifuging, washing the separated solid with ethanol for 2 to 4 times, putting it in a vacuum oven, and drying it at 30 to 50° C. for 6 to 9 hours to obtain the rubber-coated nano-silica; The liquid rubber is one of carboxyl-terminated liquid nitrile rubber and carboxyl-terminated liquid polybutadiene rubber; The modified lignin emulsion has a preparation method comprising: adding lignin powder and anhydrous ethanol to a reaction kettle, controlling the temperature at 30 to 50°C, vigorously stirring and dispersing at 3000 to 5000 rpm for 4 to 8 hours, reducing the stirring rate to 900 to 1500 rpm, adding potassium hydroxide to adjust the pH value of the reaction system to 8 to 9, adding maleic anhydride, stirring and reacting at a constant temperature for 6 to 13 hours, then reducing the temperature to room temperature, adding citric acid aqueous solution to adjust the pH value of the reaction system to 3 to 4, continuing to stir at room temperature for 2 to 5 hours, and after sufficient acidification, centrifugation to obtain maleic anhydride modified lignin, then adding the maleic anhydride modified lignin to a high-speed dispersion kettle, adding deionized water, controlling the dispersion rate at 5000 to 9000 rpm, stirring and dispersing for 6 to 10 hours, then adding water-soluble amino silicone oil, continuing to disperse and emulsify for 7 to 12 hours, and obtaining a uniform and stable emulsion, namely the modified lignin emulsion.
2. The super weather-resistant roofing waterproof coating according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 10 to 100 nm; The molecular weight of the liquid rubber is 1000 to 9000 g / mol; The mass ratio of the nano-silicon dioxide, toluene, triisobutyl phosphate, 3-isocyanate propyl triethoxysilane and liquid rubber is 35 to 50: 230 to 350: 3 to 6: 2.5 to 5.5: 8 to 14.
3. The super weather-resistant roof waterproof coating according to claim 1, characterized in that: The particle size of the lignin powder is 0.5 to 6 μm; The mass ratio of the lignin powder, anhydrous ethanol and maleic anhydride is 20 to 45:150 to 210:5 to 10; The citric acid aqueous solution has a citric acid content of 30 to 50 wt %; The mass ratio of maleic anhydride modified lignin, deionized water and water-soluble amino silicone oil is 30 to 55:120 to 220:4 to 8; The water-soluble amino silicone oil is amino polyether modified dimethyl silicone oil, and its viscosity at 25° C. is 500 to 1200 mPa·s.
4. The super weather-resistant roofing waterproof coating according to claim 1, characterized in that: The preparation method of the component A is as follows: according to the specific formula of the component A in parts by weight, deionized water, rubber-coated nano-silica and defoaming agent are first put into a high-speed dispersion kettle, and vigorously dispersed at a speed of 6000 to 9000 rpm for 3 to 6 hours, and then polyacrylate emulsion, modified lignin emulsion, film-forming aid and plasticizer are added, and after continuing to vigorously disperse for 1 to 4 hours, the material is filled into a plastic packaging barrel to obtain the component A.
5. The super weather-resistant roof waterproof coating according to claim 1, characterized in that: The preparation method of the component B is as follows: according to the specific formula of the component B in parts by weight, silicate cement, quartz powder, auxiliary crosslinking agent and crosslinking agent are placed in a V-shaped powder mixing kettle, the mixing speed is controlled at 90 to 160 rpm, and the mixing is continued for 9 to 14 hours, and then the material is discharged and packed into a moisture-proof packaging bag to obtain the component B.
Citation Information
Patent Citations
Polymer cement waterproof coating, roof waterproof layer and preparation method of roof waterproof layer
CN112341878A
Polymer cement waterproof coating
CN116004073A
Preparation method of low-shrinkage high-strength sealant
CN108975823A
Anti-skid surface layer of asphalt pavement and construction method of anti-skid surface layer
CN116640455A
Coating material and method for coating using the same
JP1996120192A