Liquid metal ink and preparation method and application thereof
By mixing EGaIn droplets wrapped with conjugated conductive polymers in water cosolvents, the problems of poor wettability and low conductivity of EGaIn in flexible electronics are solved, and stable and efficient liquid metal ink printing is achieved, which is suitable for Manufacturing of flexible electronic devices.
Patent Information
- Application Number
- CN202410967490.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-18
AI Technical Summary
In the existing technology, the application of gallium indium eutectic liquid metal (EGaIn) in flexible electronic products is limited by poor wettability, unstable suspended solids and oxidation problems caused by high surface tension and density, and there are problems during inkjet printing. Problems with viscosity discomfort and low conductivity.
By coating the surface of EGaIn droplets with a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrenesulfonate), the surface tension and density are reduced, and in different proportions of water cosolvents The hybrid, which uses mechanical extrusion to achieve conductive properties, avoids thermal or laser sintering processes and is suitable for common inkjet printers.
The liquid metal ink achieves stable performance and good conductivity, simplifies the printing process, reduces costs and operational complexity, is suitable for the manufacturing of flexible electronic devices, and maintains conductive properties on deformed substrates.
Smart Images

Figure CN118791907A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of 3D printing, and in particular relates to liquid metal ink and a preparation method and application thereof. Background Art
[0002] Gallium-based liquid metal (LM) particles, especially gallium-indium eutectic alloy (EGaIn) composed of 75% gallium and 25% indium, have gained widespread attention in various applications, including stretchable electronics, microfluidics, soft robotics, microelectrodes, circuits, and catalysis, due to their special fluid properties, low toxicity, and metallic conductivity. The inherent fluidity of EGaIn provides significant advantages for the fabrication of flexible circuits. However, the high surface tension and density of EGaIn lead to its poor wettability with the substrate, which makes it challenging to fabricate conductive circuits based on EGaIn. To address these drawbacks, various strategies have been reported, such as using surfactants to reduce surface tension, alloying with other metals, and utilizing advanced printing techniques to improve precision and stability. Current strategies for fabricating LM conductive circuits in flexible electronics involve a range of techniques, such as injection molding, screen printing, soft lithography, selective wetting, reduction patterning, roller ballpoint pen filling metal, 3D printing, and laser patterning. The choice of a specific manufacturing process depends on factors such as molds, dedicated equipment, production scale, material compatibility, and environmental conditions. Although these LM methods are promising, they usually require a large number of manual steps, which makes them time-consuming and labor-intensive. In addition, they involve high costs, complexity and the need for specialized equipment and molds, hindering large-scale production.
[0003] Inkjet printing technology provides a more efficient way to make conductive circuits, allowing direct patterning without molds or extensive equipment, greatly reducing production costs and time. The versatility and precision of inkjet printing allows for efficient production of high-resolution, complex designs on a variety of substrates, making it ideal for the rapidly developing field of flexible electronics. Inkjet printing technology is divided into continuous inkjet (CIJ) and drop-on-demand (DOD) systems based on the droplet ejection method. DOD inkjet is particularly attractive due to its environmentally friendly nature, ejecting droplets only when needed by generating pressure pulses. DOD inkjet printers are further divided into thermal, piezoelectric, electrostatic and acoustic types. Thermal inkjet printers are the most widely used type of DOD inkjet printers, which produce droplets within microseconds by heating the resistive element in the ink chamber to 300-400°C, evaporating the ink and forming bubbles that expel the ink from the nozzle. These printers are cost-effective, can produce small droplet sizes, facilitate multi-layer deposition of multiple materials at different resolutions, and ensure non-contact material processing with minimal waste.
[0004] At present, inkjet printing of EGaIn-based inks faces several challenges, including unstable suspended matter and rapid oxidation in aqueous solution, which hinders the printing process and reduces conductivity. Despite these challenges, aqueous inks have great potential due to their environmental and biosafety compared to organic solvent-based LMs. In related technologies, some scholars have used alginate to achieve LM nano-sizing and developed biocompatible aqueous inks, and some scholars have used elemental sulfur to make liquid metals uniformly dispersed in bulk polymers. However, due to the non-conductive organic materials at the stable interface, processing micro / nano LMs in organic systems usually leads to liquid metal insulation. Therefore, for most LM composites, post-processing methods such as mechanical sintering, laser sintering or chemical treatment are required to restore conductivity. In addition, particle aggregation poses challenges, resulting in inconsistent printing patterns and possible clogging of printhead nozzles. Controlling the viscosity of EGaIn inks is also critical; they are either too viscous, resulting in nozzle clogging; or too thin, resulting in poor resolution. In order to fully utilize the advantages of EGaIn in flexible electronics, it is crucial to develop a liquid metal ink. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the present invention provides a liquid metal ink with stable performance and good conductivity, which is suitable for use in flexible electronic products.
[0006] The invention also provides a method for preparing liquid metal ink.
[0007] The invention also provides a printed circuit.
[0008] The invention also provides a sensor.
[0009] A first aspect of the present invention provides a liquid metal ink, the components of which include liquid metal ink particles, a co-solvent and water, the liquid metal ink particles include EGaIn droplets, the surface of the EGaIn droplets is coated with a polymer, and the polymer is a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate).
[0010] One of the technical solutions of the present invention regarding liquid metal ink has at least the following beneficial effects:
[0011] Usually, the high surface tension and density of EGaIn lead to poor wettability with the substrate. The present invention reduces and changes the surface tension and density of EGaIn by wrapping the EGaIn droplets with a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate), without affecting the contact angle and viscosity of the base material. Furthermore, the present invention mixes EGaIn droplets with conjugated conductive polymers on the surface in different proportions of water co-solvents, without the need for additional lasers or thermal activators, and only requires simple mechanical extrusion to achieve conductive properties, with low cost and easy operation. Liquid metal ink can be printed using a common household inkjet printer without the need for molds and special equipment, and can be printed on polymer substrates (such as polyamide, PVP, etc.) or even pulp paper at room temperature.
[0012] Compared with traditional conductive inks, the liquid metal ink of the present invention provides higher stability, is easier to process, and has better mechanical robustness. The inkjet-printed ink can maintain its line shape without breaking even when the PVA substrate is deformed, and has the prospect of revolutionizing the field of printed electronics.
[0013] The liquid metal ink of the present invention has stable performance and good conductivity. When poly(3,4-ethylenedioxythiophene) (abbreviated as PEDOT) and poly(styrene sulfonate) (abbreviated as PSS) in the ink are coupled with EGaIn, a protective layer (i.e., a polymer that wraps the surface of the EGaIn droplet) is formed around the EGaIn particles to prevent oxidation of the surface Ga. The strong interaction between poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) and EGaIn effectively shields the gallium core and maintains the Ga + The polymer not only stabilizes the ink, but also improves its conductivity by keeping the gallium metal in its state. The ink jet printed on a substrate such as PVA has a resistance of 65kΩ.
[0014] Unlike existing insulating liquid metal inks, the circuits printed by the liquid metal ink of the present invention can be conductive after simple mechanical extrusion without heat or laser sintering treatment. Simply slide the pattern several times (such as 3 times, depending on the thickness of the film and the length and width of the pattern). During the sliding process, the mechanical action destroys the oxide layer on the surface, causing the liquid metal core to condense and form a continuous conductive path, and the solidified ink will produce a shiny metallic color and conductivity.
[0015] The liquid metal ink of the present invention can achieve the desired performance by mixing EGaIn and PEDOT:PSS in different proportions of water (H2O) and co-solvents. By adjusting the proportion of water, the spreadability and stability of the ink on the substrate can be balanced, thereby optimizing the printing quality.
[0016] The liquid metal ink of the present invention can print smooth, stable and conductive patterns, producing printed LM lines with a resistance of 65kΩ on flexible PVA substrates, making them suitable as metal interconnects on hydrophilic substrates. This method greatly simplifies the creation of LM-based circuits, eliminates the need for thin-film metal deposition, and paves the way for more accessible and scalable manufacturing of flexible electronic devices.
[0017] According to some embodiments of the invention, the co-solvent comprises ethylene glycol.
[0018] The role of the co-solvent is to adjust the viscosity and thus the printing process and adhesion to the substrate.
[0019] According to some embodiments of the present invention, the volume ratio of the co-solvent to water is 1:1.5-4.
[0020] If the co-solvent ratio is too high, the viscosity of the ink may be too high, which will cause the ink to flow obstructed inside the nozzle, affecting the stability and accuracy of inkjet printing. The ink may not be able to effectively wet the surface of the substrate during printing, resulting in the ink being unable to be evenly distributed and fixed, affecting the printing quality and conductive properties. Excessive water content will significantly reduce the viscosity of the ink, which may cause the ink to be too fluid and difficult to control during the printing process, or even flow or penetrate into the substrate during printing, affecting the printing quality and accuracy. Furthermore, high water content may dilute the conductive components in the ink, making the printed conductive path not continuous or stable enough. Therefore, the co-solvent and water ratio of 1:1.5 to 4 is an optimized value under the premise of maintaining the stability, conductive properties and printing quality of the liquid metal ink. Adjusting the ratio within this range can balance the fluidity, adhesion and conductive properties of the ink, ensuring that the printed circuit lines are clear and stable, suitable for applications such as flexible electronic devices.
[0021] According to some embodiments of the present invention, the average particle size D50 of the liquid metal ink particles is 100 nm to 200 nm.
[0022] Ink particles that are too small may cause the ink to flow too much, making it difficult to accurately control the printing process, and may cause the printed pattern to be blurred or unclear. Particles that are too small may also make it impossible to form clear lines and patterns during printing, affecting the resolution and detail expression of the print. Particles that are too large will increase the viscosity of the ink, which may cause poor fluidity of the ink inside the print head, affecting the stability and accuracy of inkjet printing. Ink with large particles may be difficult to effectively adhere to the surface of the substrate, resulting in insufficient adhesion of the print, affecting the quality and durability of the print.
[0023] Therefore, the average particle size of liquid metal ink particles is in the range of 100nm to 200nm, which can ensure the resolution and clarity of the printed pattern while maintaining good fluidity and viscosity control. This particle size range also helps to ensure that the printed conductive path is continuous and stable, thereby improving the reliability and performance of the printed circuit.
[0024] According to some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 20 wt %.
[0025] According to some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 10 wt %.
[0026] According to some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 5 wt %.
[0027] Too low a content of conjugated conductive polymer may result in insufficient conductivity of the ink, making the printed conductive path unstable or the resistance value too high, and may also weaken the ability to wrap liquid metal ink particles, which may affect the uniformity and stability of the ink during the printing process. Too high a content of conjugated conductive polymer will significantly increase the viscosity of the ink, which may reduce the fluidity during inkjet printing and even affect the cleaning and maintenance of the nozzle.
[0028] According to some embodiments of the present invention, when the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 20 wt %, the content of the liquid metal ink particles in the liquid metal ink is 50 microliters to 500 microliters.
[0029] The content of liquid metal ink particles in the liquid metal ink is in the range of 1wt% to 20wt% in order to achieve optimal performance and stability during the printing process. Specifically, too low a content of liquid metal particles in the ink may cause the printed conductive path to be insufficiently continuous or stable, affecting the conductive properties of the circuit. Too low a content may also make the liquid metal ink unstable during storage and printing, making it difficult to ensure print quality and durability. Excessive liquid metal particle content will increase the viscosity of the ink, which may cause difficulty in the flow of ink inside the nozzle, affecting the stability and accuracy of inkjet printing. Liquid metal is relatively expensive, and too high a content will significantly increase the cost of the ink, which is not conducive to large-scale applications and market competitiveness.
[0030] According to some embodiments of the present invention, when the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 5 wt %, the content of the liquid metal ink particles in the liquid metal ink is 100 microliters to 300 microliters.
[0031] The second aspect of the present invention provides a method for preparing the liquid metal ink described in the first aspect of the present invention, the method comprising adding EGaIn, poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) into water containing the co-solvent, and centrifuging after ultrasonic treatment.
[0032] A technical solution in the method for preparing liquid metal ink of the present invention has at least the following beneficial effects:
[0033] The preparation method of the present invention does not require expensive equipment and complex process control, the reaction conditions are not harsh, the raw materials are easily available, the production cost is low, and it is easy to industrialize. There is no need to use expensive or toxic solvents, which meets environmental protection and health and safety requirements. Ultrasonic treatment and centrifugation are relatively simple process steps and do not require complex operating techniques. The controllability and repeatability of production are increased, and production efficiency is improved. In addition, raw materials such as EGaIn, poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) are easy to obtain and the cost is relatively low.
[0034] According to some embodiments of the invention, the ultrasonic treatment is performed by a tip sonicator.
[0035] The sonication was performed by a tip sonicator with the aim of breaking up large EGaIn droplets into small particles by ultrasonic stimulation.
[0036] According to some embodiments of the present invention, the amplitude of the ultrasonic treatment is 10% to 30%.
[0037] According to some embodiments of the present invention, the ultrasonic treatment time is 60 min to 120 min.
[0038] After ultrasonic treatment, centrifugation was performed to collect the concentrated EGaIn ink for later use.
[0039] The third aspect of the present invention provides a printed circuit, which is prepared by the liquid metal ink described in the first aspect of the present invention.
[0040] One of the technical solutions of the present invention regarding printed circuits has at least the following beneficial effects:
[0041] The printed circuit of the present invention uses the liquid metal ink described in the first aspect of the present invention, and thus has all the beneficial effects of the ink. Specifically:
[0042] Excellent conductivity. The ink formed by the encapsulated EGaIn droplets can be printed on a regular household inkjet printer. After printing, a continuous conductive path can be formed by simple mechanical extrusion without the need for complex thermal or laser sintering treatment. Because the conjugated conductive polymer effectively protects the EGaIn droplets from oxidation and maintains their conductive properties, the printed circuit has a stable resistance value (65kΩ).
[0043] Wide applicability. It can be printed on a variety of substrates such as flexible PVA substrates, and is suitable for the manufacture of various flexible electronic devices. The printed LM lines can be used as metal interconnects on hydrophilic substrates, so that they can still maintain stable performance in a humid environment.
[0044] Simplified manufacturing process. The traditional metal deposition and complex heat treatment process are eliminated, greatly simplifying the manufacturing process of LM circuits. Conductive performance can be achieved by simply sliding the pattern a few times, reducing manufacturing costs and operational complexity.
[0045] Environmentally friendly and safe. Using water and ethylene glycol as solvents is more environmentally friendly and safer than traditional organic solvents. No expensive or toxic chemicals are needed, which meets environmental protection and health and safety standards.
[0046] Optimized printing quality. By adjusting the ratio of polymer to EGaIn and the water content, the spreadability and stability of the ink on the substrate can be balanced, thereby optimizing the printing quality. The printed pattern is smooth and stable, and can maintain its conductive properties for a long time, making it suitable for long-term use electronic devices.
[0047] A fourth aspect of the present invention provides a sensor prepared from the liquid metal ink described in the first aspect of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 Schematic diagram of the synthesis and thermal printing process of LM@PEDOT:PSS.
[0049] Figure 2 is the particle size distribution of EGaIn-PEDOT:PSS ink.
[0050] Figure 3 This is a scanning electron microscope image of liquid metal ink.
[0051] Figure 4 This is a transmission electron microscope image of liquid metal ink.
[0052] Figure 5 This is the X-ray photoelectron spectroscopy test result of liquid metal ink.
[0053] Figure 6 These are the contact angle test results of liquid metal ink on different substrates.
[0054] Figure 7 It is a schematic diagram of the activation process of liquid metal ink and scanning electron microscope images of the printed circuit before and after activation.
[0055] Figure 8 Schematic diagram of complex images made with liquid metal ink.
[0056] Fig. 9 This is a graph showing the change in resistance over time when liquid metal ink is printed on PVA film.
[0057] Fig.10 It is a schematic diagram of liquid metal ink printed on PVA film, connected to LED and emitting light.
[0058] Fig.11 This is a graph showing the changes in ΔR / Ro when the electronic skin monitors finger movements.
[0059] Fig.12 This is a graph showing the changes in ΔR / Ro when the electronic skin monitors wrist movement.
[0060] Fig.13 Schematic diagram of EGaIn / PEDOT:PSS lines printed on paper to make origami boxes, showing high stability and good conductivity, and activating LED lights. DETAILED DESCRIPTION
[0061] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0062] In the first aspect, in some embodiments of the present invention, a liquid metal ink is provided, the components of which include liquid metal ink particles, a co-solvent and water, the liquid metal ink particles include EGaIn droplets, the surface of the EGaIn droplets is coated with a polymer, and the polymer is a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate).
[0063] It should be noted that the high surface tension and density of EGaIn usually lead to poor wettability with the substrate. The present invention reduces and changes the surface tension and density of EGaIn by wrapping EGaIn droplets with a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate), without affecting the contact angle and viscosity of the base material. Furthermore, the present invention mixes EGaIn droplets with conjugated conductive polymers on the surface in water co-solvents of different proportions, without the need for additional lasers or thermal activators, and only requires simple mechanical extrusion to achieve conductive properties, with low cost and easy operation. Liquid metal ink can be printed by a common household inkjet printer, without the need for molds and special equipment, and can be printed on polymer substrates (such as polyamide, PVP, etc.) or even pulp paper at room temperature.
[0064] It should also be noted that compared with traditional conductive inks, the liquid metal ink of the present invention provides higher stability, is easier to process, and has better mechanical robustness. The inkjet-printed ink can maintain its line shape without breaking even when the PVA substrate is deformed, and has the prospect of completely changing the field of printed electronics.
[0065] The liquid metal ink of the present invention has stable performance and good conductivity. When poly(3,4-ethylenedioxythiophene) (abbreviated as PEDOT) and poly(styrene sulfonate) (abbreviated as PSS) in the ink are coupled with EGaIn, a protective layer (i.e., a polymer that wraps the surface of the EGaIn droplet) is formed around the EGaIn particles to prevent oxidation of the surface Ga. The strong interaction between poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) and EGaIn effectively shields the gallium core and maintains the Ga + The polymer not only stabilizes the ink, but also improves its conductivity by keeping the gallium metal in its state. The ink jet printed on a substrate such as PVA has a resistance of 65kΩ.
[0066] It can be understood that, unlike the existing insulating liquid metal ink, the circuit printed by the liquid metal ink of the present invention can be conductive by simple mechanical extrusion without heat or laser sintering treatment. Simply slide the pattern several times (such as 3 times, depending on the thickness of the film and the length and width of the pattern). During the sliding process, the mechanical action destroys the oxide layer on the surface, causing the liquid metal core to condense and form a continuous conductive path, and the solidified ink will produce a shiny metallic color and conductivity.
[0067] Furthermore, the liquid metal ink of the present invention can achieve the desired performance by mixing EGaIn and PEDOT:PSS in different proportions of water (H2O) and co-solvents. By adjusting the proportion of water, the spreadability and stability of the ink on the substrate can be balanced, thereby optimizing the printing quality.
[0068] The liquid metal ink of the present invention can print smooth, stable and conductive patterns, producing printed LM lines with a resistance of 65kΩ on flexible PVA substrates, making them suitable as metal interconnects on hydrophilic substrates. This method greatly simplifies the creation of LM-based circuits, eliminates the need for thin-film metal deposition, and paves the way for more accessible and scalable manufacturing of flexible electronic devices.
[0069] In combination with the first aspect, in some embodiments of the present invention, the co-solvent includes ethylene glycol.
[0070] The role of the co-solvent is to adjust the viscosity and thus the printing process and adhesion to the substrate.
[0071] In combination with the first aspect, in some embodiments of the present invention, the volume ratio of the co-solvent to water is 1:1.5-4.
[0072] If the co-solvent ratio is too low, the viscosity of the ink may be too high, which will cause the ink to flow obstructed inside the nozzle, affecting the stability and accuracy of inkjet printing. The ink may not be able to effectively wet the surface of the substrate during printing, resulting in the ink being unable to be evenly distributed and fixed, affecting the printing quality and conductive properties. Excessive water content will significantly reduce the viscosity of the ink, which may cause the ink to be too fluid and difficult to control during the printing process, or even to flow or penetrate into the substrate during printing, affecting the printing quality and accuracy. Furthermore, high water content may dilute the conductive components in the ink, making the printed conductive path not continuous or stable enough. Therefore, the co-solvent and water ratio of 1:1.5 to 4 is an optimized value under the premise of maintaining the stability, conductive properties and printing quality of the liquid metal ink. Adjusting the ratio within this range can balance the fluidity, adhesion and conductive properties of the ink, ensuring that the printed circuit lines are clear and stable, suitable for applications such as flexible electronic devices.
[0073] In combination with the first aspect, in some embodiments of the present invention, the average particle size D50 of the liquid metal ink particles is 100 nm to 200 nm.
[0074] Ink particles that are too small may cause the ink to flow too much, making it difficult to accurately control the printing process, and may cause the printed pattern to be blurred or unclear. Particles that are too small may also make it impossible to form clear lines and patterns during printing, affecting the resolution and detail expression of the print. Particles that are too large will increase the viscosity of the ink, which may cause poor fluidity of the ink inside the print head, affecting the stability and accuracy of inkjet printing. Ink with large particles may be difficult to effectively adhere to the surface of the substrate, resulting in insufficient adhesion of the print, affecting the quality and durability of the print.
[0075] Therefore, the average particle size of liquid metal ink particles is in the range of 100nm to 200nm, which can ensure the resolution and clarity of the printed pattern while maintaining good fluidity and viscosity control. This particle size range also helps to ensure that the printed conductive path is continuous and stable, thereby improving the reliability and performance of the printed circuit.
[0076] In combination with the first aspect, in some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 20 wt %.
[0077] In combination with the first aspect, in some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 10 wt %.
[0078] In combination with the first aspect, in some embodiments of the present invention, the content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 5 wt %.
[0079] Too low a content of conjugated conductive polymer may result in insufficient conductivity of the ink, making the printed conductive path unstable or the resistance value too high, and may also weaken the ability to wrap liquid metal ink particles, which may affect the uniformity and stability of the ink during the printing process. Too high a content of conjugated conductive polymer will significantly increase the viscosity of the ink, which may reduce the fluidity during inkjet printing and even affect the cleaning and maintenance of the nozzle.
[0080] In combination with the first aspect, in some embodiments of the present invention, when the content of the conjugated conductive polymer in the liquid metal ink is 1 wt% to 20 wt%, the content of the liquid metal ink particles in the liquid metal ink is 50 microliters to 500 microliters.
[0081] The content of liquid metal ink particles in the liquid metal ink is in the range of 1wt% to 20wt% in order to achieve optimal performance and stability during the printing process. Specifically, too low a content of liquid metal particles in the ink may cause the printed conductive path to be insufficiently continuous or stable, affecting the conductive properties of the circuit. Too low a content may also make the liquid metal ink unstable during storage and printing, making it difficult to ensure print quality and durability. Excessive liquid metal particle content will increase the viscosity of the ink, which may cause difficulty in the flow of ink inside the nozzle, affecting the stability and accuracy of inkjet printing. Liquid metal is relatively expensive, and too high a content will significantly increase the cost of the ink, which is not conducive to large-scale applications and market competitiveness.
[0082] In combination with the first aspect, in some embodiments of the present invention, when the content of the conjugated conductive polymer in the liquid metal ink is 1 wt% to 5 wt%, the content of the liquid metal ink particles in the liquid metal ink is 100 microliters to 300 microliters.
[0083] In combination with the first aspect, in some embodiments of the present invention, the conjugated conductive polymer can be directly purchased from commercial poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS, which can be dispersed in water at a concentration of 1.5 wt.%).
[0084] In a second aspect, in some embodiments of the present invention, a method for preparing the liquid metal ink described in the first aspect of the present invention is provided, the method comprising adding EGaIn, poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) to water containing the co-solvent, and centrifuging after ultrasonic treatment.
[0085] It can be understood that the preparation method of the present invention does not require expensive equipment and complex process control, the reaction conditions are not harsh, the raw materials are easily available, the production cost is low, and it is easy to industrialize. There is no need to use expensive or toxic solvents, which meets environmental protection and health and safety requirements. Ultrasonic treatment and centrifugation are relatively simple process steps and do not require complex operating techniques. The controllability and repeatability of production are increased, and production efficiency is improved. In addition, raw materials such as EGaIn, poly (3,4-ethylenedioxythiophene) and poly (styrene sulfonate) are easy to obtain and the cost is relatively low.
[0086] In conjunction with the second aspect, in some embodiments of the present invention, the ultrasonic treatment is performed by a tip sonicator.
[0087] The sonication was performed by a tip sonicator with the aim of breaking up large EGaIn droplets into small particles by ultrasonic stimulation.
[0088] In conjunction with the second aspect, in some embodiments of the present invention, the amplitude of the ultrasonic treatment is 10% to 30%.
[0089] In combination with the second aspect, in some embodiments of the present invention, the ultrasonic treatment time is 60 min to 120 min.
[0090] After ultrasonic treatment, centrifugation was performed to collect the concentrated EGaIn ink for later use.
[0091] In a third aspect, some embodiments of the present invention provide a printed circuit, which is prepared by the liquid metal ink described in the first aspect of the present invention.
[0092] It can be understood that the printed circuit of the present invention, because it uses the liquid metal ink described in the first aspect of the present invention, has all the beneficial effects of the ink. Specifically:
[0093] Excellent conductivity. The ink formed by the encapsulated EGaIn droplets can be printed on a regular household inkjet printer. After printing, a continuous conductive path can be formed by simple mechanical extrusion without the need for complex thermal or laser sintering treatment. Because the conjugated conductive polymer effectively protects the EGaIn droplets from oxidation and maintains their conductive properties, the printed circuit has a stable resistance value (65kΩ).
[0094] Wide applicability. It can be printed on a variety of substrates such as flexible PVA substrates, and is suitable for the manufacture of various flexible electronic devices. The printed LM lines can be used as metal interconnects on hydrophilic substrates, so that they can still maintain stable performance in a humid environment.
[0095] Simplified manufacturing process. The traditional metal deposition and complex heat treatment process are eliminated, greatly simplifying the manufacturing process of LM circuits. Conductive performance can be achieved by simply sliding the pattern a few times, reducing manufacturing costs and operational complexity.
[0096] Environmentally friendly and safe. Using water and ethylene glycol as solvents is more environmentally friendly and safer than traditional organic solvents. No expensive or toxic chemicals are needed, which meets environmental protection and health and safety standards.
[0097] Optimized printing quality. By adjusting the ratio of polymer to EGaIn and the water content, the spreadability and stability of the ink on the substrate can be balanced, thereby optimizing the printing quality. The printed pattern is smooth and stable, and can maintain its conductive properties for a long time, making it suitable for long-term use electronic devices.
[0098] In a fourth aspect, some embodiments of the present invention provide a sensor prepared from the liquid metal ink described in the first aspect of the present invention.
[0099] In conjunction with the fourth aspect, in some embodiments of the present invention, the sensor includes patches for monitoring various movements of the human body. By sticking these patches to different parts of the body, such as fingers, wrists, and head, motion sensors with high response rates can be developed. When the electronic tape is attached to the skin, it forms a conductive path that can detect changes in resistance (ΔR / Ro) when the body moves. As the tape area moves, the tension on the conductive ink changes, thereby changing its resistance. These changes in resistance are then measured and analyzed to monitor and quantify specific movements of body parts.
[0100] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0101] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0102] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.
[0103] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.
[0104] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0105] The abbreviation PP stands for conjugated conducting polymer. PEDOT:PSS stands for poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate). LM@PEDOT:PSS stands for liquid metal ink.
[0106] In the embodiment, the conjugated conductive polymer is commercial poly(3,4-ethylenedioxythiophene) and polystyrene sulfonate (PEDOT:PSS) purchased directly, and supplied by Macklin (Shanghai) Chemical Technology Co., Ltd.
[0107] Example
[0108] In this embodiment, a liquid metal ink is first prepared, and then a polyvinyl alcohol polymer film is prepared by itself. The prepared ink is then used to print on the film, and a series of characterizations are performed.
[0109] The components of the liquid metal ink are liquid metal ink particles, a co-solvent and water. The liquid metal ink particles include EGaIn droplets, and the surface of the EGaIn droplets is coated with a polymer, which is a conjugated conductive polymer formed by poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate).
[0110] in:
[0111] The cosolvent is ethylene glycol, with a content of 70:30 (water: EG, volume ratio).
[0112] The content of the EGaIn droplets was 5 wt%.
[0113] The content of the conjugated conductive polymer was 5 wt %.
[0114] The balance is water.
[0115] The preparation method of liquid metal ink is:
[0116] Liquid metal ink was prepared by adding 5wt.% EGaIn and 5wt.% PEDOT:PSS (i.e., conjugated conductive polymer) to H2O:EG solution according to the ratio. Ultrasonication was performed for 90 min at 20% amplitude in a cold water bath using a tip sonicator (1 / 16 inch micro-tip probe). After ultrasonication, the ink was centrifuged at 2000 rpm for 5 minutes to remove larger nanoparticles.
[0117] Preparation of polyvinyl alcohol (PVA) polymer film
[0118] PVA was prepared in a solution (5 wt.% PVA dissolved in water) by mixing at 80°C for 2 h and spinning at 400 rpm. After the PVA was completely dissolved, the solution was poured into a mold and dried in an oven at 40°C for 6 h. Then, to ensure uniform layer distribution, it was kept at room temperature until completely dry.
[0119] Printing process
[0120] After the ink was prepared, it was loaded into a nominal 10mL capacity cartridge (XL-805) with a print width of 0.57 inches (14.48mm). The liquid metal ink on the PVA film was directly inkjet printed using an hp1200 printer with a thermal print head. The optimized printing conditions were: droplet double drop weight of 7 and 3ng, print head resolution of 1200×600dpi, and substrate room temperature (25°C). A PVA film dried at 70°C for 10 minutes was used; this is the optimal temperature for solvent evaporation.
[0121] The flexible patch is based on EGaIn-PEDOT:PSS ink on a PVA substrate and is designed for testing electric motion sensing devices.
[0122] PVA films were made, each of which was printed with EGaIn-PEDOT:PSS ink to form patterned lines 80 mm long and 5 mm wide. These PVA films were securely attached to the experimenter's finger and wrist joints to ensure that the film would stretch and deform synchronously with the movement of the joints. The ends of the wires were clamped with alligator clips and connected to a digital multimeter. By repeatedly bending and straightening the fingers or wrists, the real-time changes in the wire resistance were measured using a digital multimeter throughout the process.
[0123] Characterization methods
[0124] It should be noted that the ultrasound was performed by an ultrasound instrument (Branson SFX550 digital ultrasonic cell destroyer).
[0125] The SEM images were taken using a SU8220 (Hitachi, Japan) measuring instrument. 10 μL of the LM nanoparticle ink suspension diluted two times was dropped on a silicon wafer and dried in the environment.
[0126] Transmission Electron Microscopy (TEM) (JEOL JSM-7500FA) As the EGaIn / PEDOT:PSS ink is dark in color with a high concentration of LM nanoparticles, the suspension was therefore diluted with EtOH and then dropped onto a TEM copper grid and dried under ambient conditions.
[0127] Dynamic light scattering (DLS) measurements were performed using a Malvern Zetasizer Nano series at 25° C. Before each measurement, the ink was diluted to 1 μL in EtOH.
[0128] Electromechanical coupling measurements; Conductive traces (length: 40 mm; width: 20 mm) were used for electromechanical testing as per the manufacturing process.
[0129] After being treated with LM nanoparticle ink, the PVA with conductive traces was cut into dog-bone shapes (length: 60 mm) using a laser cutter (VLS 3.50, Universal laser Systems, Inc.).
[0130] These dogbones with conductive traces were subjected to uniaxial tensile loading in a universal bread frame (Instron) when the printed circuit was precisely positioned in the middle of the dogbone shape. Simultaneously, the change in the resistance of the sample was measured with a multimeter. The tensile specimens were used to determine the maximum electromechanical strength at a displacement rate of 10 mm / min.
[0131] All resistance measurements were performed using a digital multimeter (Kitthley DMM6500 digital multimeter). X-ray photoelectron spectroscopy (XPS) analysis was performed using a PHI 5000 VersaProbe III (ULVAC PHI, Japan).
[0132] The contact angle of LM nanoparticles was measured using a DSA25 contact angle meter (Kruss, Germany).
[0133] Optical microscope SOPTOP (SZN71TR, China).
[0134] To measure the viscosity, a Pinkevich glass capillary viscometer was used.
[0135] Figure 1 The synthesis of LM@PEDOT:PSS and the subsequent thermal printing process are demonstrated. Figure 1 In the figure, part a shows the ink preparation process, part b shows the use of a thermal inkjet printer to load the ink into the ink cartridge and perform printing, and part c shows a schematic diagram of the ink being printed on the PVA film.
[0136] The process of achieving the properties of the conductive LM@PEDOT:PSS printing ink consists of four steps:
[0137] (i) preparing EGaIn ink;
[0138] (ii) Print using specific parameters;
[0139] (iii) drying the film at about 70 °C for about 10 min to evaporate the solvent and ensure mechanical stability and adhesion to the substrate, although the film is still non-conductive at this stage;
[0140] (iv) Further drying at room temperature for 24 h, which gives the films a shiny metallic color and electrical conductivity, depending on their thickness.
[0141] The solution containing EGaIn droplets was probe-ultrasonicated for 1.5 h. During this process, the ultrasonic stimulation broke the large EGaIn droplets into small particle sizes. At the same time, these particles were stabilized by coating the conjugated polymer PEDOT:PSS on their surface. The surface of these particles became stable due to the coating of the conjugated polymer PEDOT:PSS. After the centrifugation step, the concentrated liquid metal ink was collected and loaded into the ink cartridge (XL-805) with a 0.57-inch (14.48 mm) printing tape.
[0142] The liquid metal ink on the PVA film was directly printed by inkjet printing using an HP 1200 thermal print head. The optimized printing conditions were: double drop weight of 7 and 3 ng, print head resolution of 1200×600 dpi, and substrate at room temperature (25°C). Figure 1 In the experiment, the liquid metal ink on the PVA film with circuits and lines is very stable and uniform, and does not affect its operation as a conductive line after stretching and twisting.
[0143] The stability, dispersion, and size of nanoparticles (NPs) are critical to liquid metal ink systems because larger particles or aggregated NPs can clog printer nozzles. In addition, NPs should have a narrow size distribution and be evenly dispersed throughout the ink vehicle to ensure optimal jetting performance.
[0144] The particle size distribution of EGaIn-PEDOT:PSS ink was characterized by dynamic light scattering (DLS). Figure 2 The average particle size of the prepared LM ink is 164 nm.
[0145] Figure 3 A scanning electron microscope (SEM) image of the liquid metal ink is shown, in which EGaIn NPs with a smooth core-shell spherical structure are uniformly stacked together.
[0146] Figure 4 Transmission electron microscopy (TEM) images of the liquid metal ink showed that the EGaIn NPs formed under continuous ultrasound were spherically isolated with clear boundaries and rounded shapes.
[0147] In addition, viscosity and contact angle are key to the performance of inks. For example, thermal inkjet printing technology uses high temperatures to generate bubbles to eject ink from the nozzle, so the ink must contain an aqueous solution and be able to withstand these temperatures. Aqueous solvents often face challenges with poor dispersibility and poor adhesion in most conductive compounds, so binders or surfactants are required to achieve high-quality ink uniformity. The unbalanced ink composition leads to a series of problems such as printed pattern distortion, surface cracking, and coffee ring effect during the printing process, which has become a serious obstacle to inkjet printing. In order to obtain the best printing effect, EG is used as a high-boiling point co-solvent to reduce the evaporation rate of the solvent and provide suitable viscosity and contact angle values for the printing process.
[0148] X-ray photoelectron spectroscopy (XPS) analysis of the ink revealed the chemical composition of its core and shell. Figure 5 As shown, the measured spectrum XPS shows that the main elements are Ga 2p, Ga 3d and carbon, corresponding to LM@PEDOT:PSS. The XPS results refer to the C1s peak with a binding energy of 284.6 eV.
[0149] Further, such as Figure 6 As shown, the contact angle test showed different values, with sample H-3 showing 110.9°C and 86.8°C on paper and PVA substrates, respectively. It is worth noting that the low contact angle (less than 90°C) of the EGaIn ink droplet on the PVA film indicates excellent wettability. The contact angles of H-1 and H-3 were compared with the baseline H-2 ink. While the contact angle on paper remained essentially unchanged, the contact angle of the H-3 sample on the PVA film increased to 112.8°C. The high contact angle on the PVA film can be attributed to the higher EG content. The higher the EG content, the higher the viscosity of the ink, the lower the surface tension, the smaller the diffusion, and the larger the contact angle. However, the inks with lower EG content (H-1 and H-2) maintain a balance, allowing better diffusion and lower contact angles.
[0150] As a polymer binder for LM NPs, the embodiment selected the conductive polymer PEDOT:PSS, which is a conjugated polymer that is easily processed with aqueous solvents. This ensures its applicability in liquid metal ink applications without adversely affecting the viscosity or contact angle properties of the ink. The content of PEDOT:PSS and EGaIn has a significant impact on the stability and performance of the liquid metal ink.
[0151] The present invention first evaluated different doses of EGaIn NPs to determine the optimal concentration for printing. It was determined that 200 microliters was the maximum suitable amount of LM, because higher concentrations would make it difficult to maintain uniform and stable nanoparticles in the solution, increasing the possibility of nozzle clogging. Low concentrations of low-metal nanoparticles, below 200 microliters, showed poor conductivity. Using 200 microliters of EGaIn NPs, the PEDOT:PSS concentration was changed to 1, 3, 5 and 10wt.% for testing.
[0152] The results showed that inks containing 1 and 3 wt.% PEDOT:PSS were unstable and had poor conductivity. In addition, higher concentrations of PEDOT:PSS (such as 10 wt.%) resulted in unclear images due to poor printability. Finally, the concentrations of PEDOT:PSS and EGaIn NPs were adjusted to prepare the ink, a condition that achieved a good compromise between stability and conductivity. In addition, the present invention also attempted to use other surfactant polymers such as polystyrene pyrrolidone (PVP), PVA, and polystyrene sulfonate (PSS) in the aqueous ink system. However, after loading these inks into the ink cartridge, the printer failed to print, indicating that there was a problem with the ink.
[0153] In addition, the wetting properties of the EGaIn-PEDOT:PSS ink on the PVA film were observed, where the ink exhibited a relatively hydrophilic property, allowing the ink to spread and maximize contact due to its special affinity for water. This caused the printed droplets to shrink into islands on the hydrophobic surface.
[0154] Figure 7 shows the activation process of the conductive LM nanoparticle ink. By sliding the pattern 3-4 times, the cured ink develops a shiny metallic color and conductivity, depending on the thickness of the film and the length and width of the pattern. During the sliding process, the mechanical action breaks up the oxide layer on the surface, allowing the liquid metal core to condense and form a continuous conductive path. Repeated sliding ensures that the oxide layer is adequately broken up, promoting the formation of a uniform conductive metal film. This activation process highlights the importance of mechanical activation in achieving the desired conductive properties of LM nanoparticle inks, promoting the production of high-quality conductive films that are easily activated. Figure 7 In the SEM image, before activation, the pattern shows that after 3-5 prints, the ink shrinks into an island shape and is densely packed with each other; after activation, the pattern presents another effect, the ink is continuous and linear, and has conductivity. The interconnected hollow spaces indicate good conduction in both the lateral and vertical directions.
[0155] Different circuits and complex images were printed on PVA films to verify that the ink can produce complex images, such as Figure 8 shown.
[0156] The stability of the LM@PEDOT:PSS ink was evaluated by printing square patterns on PVA film with the same ink cartridge on consecutive days and measuring the change in its conductivity after curing under optimal conditions, e.g. Fig. 9 As shown. The conductivity of LM@PEDOT:PSS patterns printed with the same ink cartridge remained constant for 7 consecutive days and then decreased. During this period, frequent nozzle clogging was observed, requiring multiple cleaning steps to maintain functionality. This behavior could be due to the onset of nanoparticle deposition or agglomeration. After 14 days, the ink cartridge was no longer jettable. This study suggests that the stability of LM@PEDOT:PSS inks can be improved by exploring other surfactants or binders.
[0157] exist Fig.10 In the paper, a printed circuit was used to confirm the conductivity of the EGaIn-PEDOT:PSS ink on the PVA film. An LED was connected to the circuit and it emitted light with an amplitude of 3.05V, verifying that the pattern had good conductivity.
[0158] Furthermore, the liquid metal ink LM@PEDOT:PSS of the present invention can be used to make electronic patches for monitoring various movements of the human body. By sticking these patches to different parts of the body, such as fingers and wrists, motion sensors with high response rates can be developed. When the electronic tape is attached to the skin, it forms a conductive path that can detect changes in resistance (ΔR / Ro) when the body moves. As the tape area moves, the tension on the liquid metal ink changes, thereby changing its resistance. These changes in resistance are then measured and analyzed to monitor and quantify specific movements of body parts.
[0159] Fig.11 and Fig.12 The electronic skin shows the change in ΔR / Ro when monitoring finger and wrist movements, respectively. For example, when a finger is bent, the tape stretches, causing a change in resistance detected by the sensor. Similarly, movements of the wrist and head cause corresponding changes in the resistance of the electronic patch, providing real-time monitoring of these movements. The use of LM@PEDOT:PSS ink in electronic patches shows its potential to create flexible wearable sensors that can accurately monitor and respond to human movements, paving the way for advances in wearable technology and health monitoring systems.
[0160] Fig.13 The cube origami is made by using EGaIn / PEDOT:PSS along the lines printed on the paper. The process of energizing the printed EGaIn / PEDOT:PSS lines to activate the LED light source is shown, showing high stability and good conductivity.
[0161] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A liquid metal ink, characterized in that: The components include liquid metal ink particles, a co-solvent and water. The liquid metal ink particles include EGaIn droplets. The surface of the EGaIn droplets is coated with a polymer. The polymer is a conjugated conductive polymer formed by poly (3, 4-ethylenedioxythiophene) and poly (styrene sulfonate).
2. The liquid metal ink according to claim 1, characterized in that: The co-solvent includes ethylene glycol.
3. The liquid metal ink according to claim 1, characterized in that: The volume ratio of the co-solvent to water is 1:1.5-4.
4. The liquid metal ink according to any one of claims 1 to 3, characterized in that: The average particle size D50 of the liquid metal ink particles is 100 nm to 200 nm.
5. The liquid metal ink according to any one of claims 1 to 3, characterized in that: The content of the conjugated conductive polymer in the liquid metal ink is 1 wt % to 20 wt %.
6. The liquid metal ink according to claim 5, characterized in that: The content of the liquid metal ink particles in the liquid metal ink is 50 microliters to 500 microliters.
7. A method for preparing the liquid metal ink according to any one of claims 1 to 6, characterized in that: The method comprises adding EGaIn, poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) into water containing the co-solvent, and performing ultrasonic treatment followed by centrifugation.
8. The method according to claim 7, characterized in that The ultrasonic treatment is performed by a tip ultrasonicator; and / or the amplitude of the ultrasonic treatment is 10% to 30%; and / or the time of the ultrasonic treatment is 60 min to 120 min.
9. A printed circuit, characterized in that: Prepared from the liquid metal ink according to any one of claims 1 to 6.
10. A sensor, characterized in that: Prepared from the liquid metal ink according to any one of claims 1 to 6.