Acrylic polymer water-based paint and preparation method thereof

By blending modified alkyd resin with water-based acrylic resin and using modified nano-silica, the problems of insufficient hardness, adhesion and antibacterial performance of water-based acrylic paint are solved, and higher paint film hardness and flame retardant properties are achieved.

CN118791920AInactive Publication Date: 2024-10-18JIANGMEN CAIGE ENVIRONMENTAL PROTECTION TECH IND

Patent Information

Application Number
CN202411082997.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing water-based acrylic paints have deficiencies in hardness, adhesion, antibacterial performance and flame retardant properties. The paint film dries slowly, has low hardness, poor adhesion, and poor antibacterial and flame retardant properties.

Method used

By blending modified alkyd resin with water-based acrylic resin and adding modified nano-silica, the modified nano-silica is grafted with anti-bacterial flame retardant to improve the hardness, adhesion and resistance of the paint film. combustion performance.

Benefits of technology

It significantly improves the hardness, adhesion and flame retardant properties of the paint film, enhances the antibacterial properties, and forms good aging resistance and flame retardant properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and discloses an acrylic polymer water-based coating and a preparation method thereof.The acrylic polymer water-based coating is prepared from, by weight, 110-130 parts of water-based acrylic resin, 40-50 parts of modified alkyd resin, 10-25 parts of modified nano-silica, 4-6 parts of dispersing agent, 0.5-2 parts of defoaming agent, 0.5-2 parts of flatting agent and 10-20 parts of water; the modified alkyd resin is epoxy modified castor oil-based waterborne alkyd resin; the modified nano silicon dioxide is antibacterial flame retardant grafted nano silicon dioxide, and the antibacterial flame retardant is a triazine derivative containing benzisothiazolinone and a siloxane structure. By blending the modified alkyd resin and the water-based acrylic resin, the hardness and adhesive force of a paint film are improved, and by adding the modified nano silicon dioxide, the antibacterial property and flame retardant property of the paint film are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to an acrylic polymer water-based coating and a preparation method thereof. Background Art

[0002] In order to avoid metal corrosion, we usually protect the metal by changing the structure of the metal itself, adding a surface protective layer, and using electrochemical principles. The most common method in industry is to apply anti-corrosion and anti-mildew coatings on the surface of steel. Anti-corrosion and anti-mildew coatings have gone through a development process from solvent-based to water-based. Solvent-based coatings have excellent coating performance, but the use of thinners leads to a high content of volatile organic matter, which is harmful to the environment and is not easy to clean. Water-based coatings use water as a diluent, are environmentally friendly and energy-saving, have a high market price, and will gradually replace solvent-based coatings in the future. "Oil retreats and water advances" will be the development trend of the coatings industry. Water-based acrylic anti-corrosion and anti-mildew coatings have attracted widespread attention from researchers due to their good high temperature resistance, water resistance, weather resistance, tensile strength, color retention, and outstanding low cost.

[0003] Waterborne acrylic paint is an acrylic resin paint with an acrylic polymer synthesized from three monomers: methyl methacrylate (MMA), butyl acrylate (BA) and acrylic acid (AA) as the base material and water as the dispersant. It is mainly divided into two categories: thermoplastic and thermosetting resins. The former is used as a topcoat for metal corrosion protection, and the latter is used as a topcoat for glazing various metal surfaces. It has low viscosity, good stability and weather resistance. However, waterborne alkyd resin paint itself also has many performance defects, such as slow drying of the paint film, low hardness and poor adhesion. At the same time, the existing waterborne acrylic paints also have poor antibacterial and flame retardant properties. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide an acrylic polymer water-based paint and a preparation method thereof, by blending modified alkyd resin with water-based acrylic resin, the hardness and adhesion of the paint film are improved, and by adding modified nano-silica, the antibacterial and flame retardant properties of the paint film are improved.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 110-130 parts of water-based acrylic resin, 40-50 parts of modified alkyd resin, 10-25 parts of modified nano-silicon dioxide, 4-6 parts of dispersant, 0.5-2 parts of defoamer, 0.5-2 parts of leveling agent, and 10-20 parts of water, wherein the modified alkyd resin is an epoxy-modified castor oil-based water-based alkyd resin; the modified nano-silicon dioxide is an antibacterial flame retardant grafted nano-silicon dioxide, the antibacterial flame retardant is a triazine derivative containing benzisothiazolinone and siloxane structure, and the structural formula of the antibacterial flame retardant is as follows:

[0007]

[0008] Further preferably, the dispersant is a polyurethane oligomer or a phosphate ester active agent, the defoamer is a polyether defoamer, a silicone defoamer or a polyether siloxane copolymer, and the leveling agent is carboxymethyl cellulose.

[0009] Further preferably, the preparation method of the modified alkyd resin comprises the following steps:

[0010] A. Add castor oil, E-44 epoxy resin and trimethylolpropane into a reactor, heat it to 110-130°C, add LiOH, and then slowly heat it to 230-240°C for full reaction to obtain an alcoholysis product;

[0011] B. Cool the alcoholysis product to 140-160°C, add phthalic anhydride, xylene and benzoic acid, heat to 220-230°C and reflux until the acid value is lower than 10 mgKOH / g, then stop heating to obtain an esterification product;

[0012] C. Vacuum the esterification product to remove xylene, cool it to 150-170°C, add trimellitic anhydride, heat it up for esterification and dehydration, and keep the temperature to react until the acid value reaches 40-60 mgKOH / g, then stop the reaction;

[0013] D. When the system temperature drops to 55-65°C, add a certain proportion of triethylamine to neutralize for 8-10 minutes, then add a certain amount of water, and stir and disperse with a high-speed disperser for 20-40 minutes to obtain the modified alkyd resin.

[0014] More preferably, the mass ratio of castor oil, E-44 epoxy resin, phthalic anhydride and trimellitic anhydride is 40-50:3-5:8-10:12-15.

[0015] Further preferably, the preparation method of modified nano-silicon dioxide comprises the following steps:

[0016] (1) 1,2-benzisothiazol-3-one, potassium carbonate and N,N-dimethylformamide are mixed, and then tribromoneopentyl alcohol is slowly added at room temperature, and the mixture is heated to 70° C. and stirred for reaction for 10 to 12 hours. After the reaction, deionized water is added to dissolve the product, and then the mixed solution is extracted with ethyl acetate. Anhydrous magnesium sulfate is added to the extract to dehydrate the extract, and then the extract is filtered. The ethyl acetate is removed by rotary evaporation of the filtrate, and finally the intermediate A is purified by a chromatographic column;

[0017] (2) Add cyanuric chloride to 1,4-dioxane and triethylamine under a nitrogen atmosphere, stir to dissolve the cyanuric chloride, then uniformly add 3-aminopropyltriethoxysilane, react in an ice bath for 1 to 3 hours after the addition is completed, add intermediate A to the reaction system, then heat up to 40 to 50° C. at a rate of 2 to 4° C. / min, and keep the temperature for 1 to 3 hours. After the reaction is completed, cool and filter to remove triethylamine hydrochloride, remove tetrahydrofuran by vacuum distillation, add ethyl acetate, dry and filter, and vacuum distill the filtrate to obtain an antibacterial flame retardant;

[0018] (3) Add nano-silica powder to a mixture of anhydrous ethanol and deionized water, and ultrasonically disperse for 10 to 15 minutes. Adjust the pH value of the solution to 4 with aqueous hydrochloric acid. Then slowly add the antibacterial flame retardant to the nano-silica solution, and ultrasonically disperse for 5 to 10 minutes. Heat to 60 to 80° C. and keep the temperature for 3 to 5 hours. After cooling, filter, wash, and dry to obtain modified nano-silica.

[0019] More preferably, the molar ratio of 1,2-benzisothiazol-3-one to tribromoneopentyl alcohol is 3:1.

[0020] More preferably, the molar ratio of cyanuric chloride, 3-aminopropyltriethoxysilane and intermediate A is 1:1:2.

[0021] A method for preparing an acrylic polymer water-based paint comprises the following steps: mixing water-based acrylic resin, modified alkyd resin, dispersant, defoamer, leveling agent and water to obtain a mixed liquid; and adding modified nano silicon dioxide into the mixed liquid for high-speed dispersion to obtain a water-based paint.

[0022] Beneficial effects of the present invention:

[0024] The modified nano-silica of the present invention adopts antibacterial flame retardant to graft nano-silica, wherein the antibacterial flame retardant is a triazine derivative containing benzisothiazolinone and siloxane structure, and the siloxane is hydrolyzed and grafted with inorganic nano-silica particles, so that the surface of the nano-silica is grafted with organic groups, so that it can be evenly dispersed in the coating, and at the same time, because the antibacterial flame retardant has multiple benzisothiazolinone groups in the molecular structure, it can give the material excellent antibacterial properties. At the same time, the antibacterial flame retardant molecule has rich N, P, and Si elements, which promotes the dehydration and carbonization of the polymer during thermal cracking, and forms a carbonaceous protective layer of Si-O and Si-C, giving the material good flame retardant properties. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] A method for preparing a modified alkyd resin comprises the following steps:

[0028] A. Add 35.8g castor oil, 4.6g E-44 epoxy resin and 6.1g trimethylolpropane into a reactor, heat to 120°C under nitrogen protection, add 0.5g LiOH, and then slowly heat to 235°C for sufficient reaction to obtain an alcoholysis product;

[0029] B. Cool the alcoholysis product to 150°C, add 7.4g phthalic anhydride, 50ml xylene and 1.1g benzoic acid, heat to 225°C and reflux until the acid value is lower than 10mgKOH / g, then stop heating to obtain an esterification product;

[0030] C. Vacuum the esterification product to remove xylene, cool it to 160°C, add 9.6g of trimellitic anhydride, heat it up for esterification and dehydration, and keep the temperature to react until the acid value reaches 50mgKOH / g, then stop the reaction;

[0031] D. When the system temperature drops to 60°C, add 10 ml of triethylamine for neutralization for 10 minutes, then add a certain amount of water and stir and disperse with a high-speed disperser for 30 minutes to obtain the modified alkyd resin.

[0032] Example 2

[0033] A method for preparing modified nano silicon dioxide comprises the following steps:

[0034] (1) 4.5 g of 1,2-benzisothiazol-3-one, 1.2 g of potassium carbonate and 50 ml of N,N-dimethylformamide were mixed, and then 3.1 g of tribromoneopentyl alcohol was slowly added at room temperature, and the mixture was heated to 70° C. and stirred for 12 h. After the reaction, deionized water was added to dissolve the product, and then the mixed solution was extracted with ethyl acetate. Anhydrous magnesium sulfate was added to the extract to dehydrate it, and then it was filtered. The filtrate was evaporated to remove the ethyl acetate, and finally purified by a chromatographic column to obtain intermediate A;

[0035] (2) Under a nitrogen atmosphere, 3.6 g of cyanuric chloride was added to 30 ml of 1,4-dioxane and 20 ml of triethylamine, and the cyanuric chloride was dissolved by stirring, and then 4.4 g of 3-aminopropyltriethoxysilane was added dropwise at a uniform rate. After the addition was completed, the reaction was carried out in an ice bath for 2 hours. 21.5 g of intermediate A was added to the reaction system, and then the temperature was increased to 45° C. at a rate of 3° C. / min, and the reaction was kept at this temperature for 2 hours. After the reaction was completed, the system was cooled and filtered to remove triethylamine hydrochloride, and tetrahydrofuran was removed by vacuum distillation. Ethyl acetate was added, and the system was dried and filtered. The filtrate was vacuum distilled to obtain an antibacterial flame retardant;

[0036] (3) 7.4 g of nano-silica powder was added to a mixture of 50 ml of anhydrous ethanol and 5 ml of deionized water, and ultrasonically dispersed for 12 min. The pH value of the solution was adjusted to 4 with aqueous hydrochloric acid. Then, 10.5 g of an antibacterial flame retardant was slowly added to the nano-silica solution and ultrasonically dispersed for 8 min. The solution was heated to 70° C. and kept warm for 4 h. After cooling, the solution was filtered, washed, and dried to obtain modified nano-silica.

[0037] Example 3

[0038] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 110 parts of water-based acrylic resin, 50 parts of modified alkyd resin, 10 parts of modified nano-silicon dioxide, 6 parts of polyurethane oligomer, 0.5 parts of silicone defoamer, 2 parts of carboxymethyl cellulose, and 10 parts of water, wherein the modified alkyd resin is the epoxy-modified castor oil-based water-based alkyd resin prepared in Example 1; and the modified nano-silicon dioxide is the antibacterial flame retardant grafted nano-silicon dioxide prepared in Example 2.

[0039] The preparation method of the acrylic polymer water-based paint comprises the following steps: mixing water-based acrylic resin, modified alkyd resin, dispersant, defoamer, leveling agent and water to obtain a mixed liquid; and then adding modified nano-silicon dioxide into the mixed liquid for high-speed dispersion to obtain a water-based paint.

[0040] Example 4

[0041] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 130 parts of water-based acrylic resin, 40 parts of modified alkyd resin, 25 parts of modified nano-silicon dioxide, 4 parts of phosphate ester active agent, 2 parts of polyether defoamer, 0.5 parts of carboxymethyl cellulose, and 20 parts of water, wherein the modified alkyd resin is the epoxy-modified castor oil-based water-based alkyd resin prepared in Example 1; and the modified nano-silicon dioxide is the antibacterial flame retardant grafted nano-silicon dioxide prepared in Example 2.

[0042] The preparation method of the above acrylic polymer water-based coating is the same as that of Example 3.

[0043] Example 5

[0044] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 120 parts of water-based acrylic resin, 45 parts of modified alkyd resin, 18 parts of modified nano-silica, 5 parts of polyurethane oligomer, 1.2 parts of polyether siloxane copolymer, 1.5 parts of carboxymethyl cellulose, and 15 parts of water, wherein the modified alkyd resin is the epoxy-modified castor oil-based water-based alkyd resin prepared in Example 1; and the modified nano-silica is the antibacterial flame retardant grafted nano-silica prepared in Example 2.

[0045] The preparation method of the above acrylic polymer water-based coating is the same as that of Example 3.

[0046] Comparative Example 1

[0047] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 120 parts of water-based acrylic resin, 18 parts of modified nano-silica, 5 parts of polyurethane oligomer, 1.2 parts of polyether siloxane copolymer, 1.5 parts of carboxymethyl cellulose, and 15 parts of water, wherein the modified nano-silica is the antibacterial flame retardant grafted nano-silica prepared in Example 2.

[0048] The preparation method of the above acrylic polymer water-based coating is the same as that of Example 3.

[0049] Comparative Example 2

[0050] An acrylic polymer water-based paint comprises the following raw materials in parts by weight: 120 parts of water-based acrylic resin, 45 parts of modified alkyd resin, 5 parts of polyurethane oligomer, 1.2 parts of polyether siloxane copolymer, 1.5 parts of carboxymethyl cellulose, and 15 parts of water, wherein the modified alkyd resin is the epoxy-modified castor oil-based water-based alkyd resin prepared in Example 1.

[0051] The preparation method of the above acrylic polymer water-based coating is the same as that of Example 3.

[0052] Performance Testing

[0053] 1. The acrylic polymer water-based coatings prepared in Examples 3 to 5 and Comparative Examples 1 to 2 were tested for pencil hardness of the paint film according to GBT 6739-2022, for impact resistance of the paint film according to GB / T 1732-2020, for adhesion of the paint film according to GB / T 9286-2021, and for abrasion resistance of the paint film according to GB / T 1768-2006, and the data were shown in Table 1 below.

[0054] Table 1 Physical and chemical properties of acrylic polymer water-based coatings

[0055]

[0056] It can be seen from the data in Table 1 that the acrylic polymer water-based coatings prepared in Examples 3 to 5 and Comparative Example 1 have good pencil hardness, impact resistance and wear resistance after curing. In Comparative Example 1, no modified alkyd resin is added, and its paint film adhesion slightly decreases. In Comparative Example 2, no modified nano-silicon dioxide is added, and the pencil hardness and wear resistance of the paint film decrease more significantly. The present invention utilizes modified alkyd resin and water-based acrylic resin to blend, and the modified alkyd resin adopts epoxy groups and polyols to undergo ring-opening reaction to generate ether alcohol, and then alcoholyzes castor oil to obtain a clear, transparent, epoxy-modified water-based alkyd resin with excellent comprehensive performance. On the basis of maintaining the original excellent performance of the alkyd resin, the epoxy resin can be introduced into the alkyd resin structure, and the heat resistance, water resistance and corrosion resistance of the alkyd resin are improved to a certain extent, and the hardness and its adhesion on the substrate are improved at the same time, and the modified nano-silicon dioxide can significantly improve the mechanical properties and wear resistance of the material.

[0057] 2. Aging resistance test

[0058] The acrylic polymer water-based coatings prepared in Examples 3 to 6 and Comparative Examples 1 to 2 were tested for antibacterial properties according to GB T1741-2007, and the vertical burning grade (UL94) was tested according to ASTM3801. The data obtained are shown in Table 2 below.

[0059] Table 2 Aging resistance of acrylic polymer water-based coatings

[0060]

[0061] It can be seen from the data in Table 2 that the acrylic polymer water-based coatings in Examples 3 to 4 and Comparative Example 1 have good aging resistance and flame retardant properties after curing, while the modified nano-silicon dioxide is added in Comparative Example 2, and the antibacterial and flame retardant properties of the coating film are significantly reduced. The modified nano-silicon dioxide of the present invention uses an antibacterial flame retardant to graft nano-silicon dioxide, wherein the antibacterial flame retardant is a triazine derivative containing benzisothiazolinone and a siloxane structure, and the siloxane is hydrolyzed and grafted with inorganic nano-silicon dioxide particles, so that the surface of the nano-silicon dioxide is grafted with an organic group, so that it can be evenly dispersed in the coating, and at the same time, because the antibacterial flame retardant has multiple benzisothiazolinone groups in the molecular structure, it can give the material excellent antibacterial properties. At the same time, the antibacterial flame retardant molecule has rich N, P, and Si elements, which promote the dehydration and carbonization of the polymer during thermal cracking, and form a carbonaceous protective layer of Si-O and Si-C, giving the material good flame retardant properties.

[0062] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0063] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. An acrylic polymer water-based paint, characterized in that: The invention comprises the following raw materials in parts by weight: 110-130 parts of water-based acrylic resin, 40-50 parts of modified alkyd resin, 10-25 parts of modified nano-silicon dioxide, 4-6 parts of dispersant, 0.5-2 parts of defoamer, 0.5-2 parts of leveling agent, and 10-20 parts of water. The modified alkyd resin is an epoxy-modified castor oil-based water-based alkyd resin; the modified nano-silicon dioxide is an antibacterial flame retardant grafted nano-silicon dioxide, the antibacterial flame retardant is a triazine derivative containing benzisothiazolinone and siloxane structure, and the structural formula of the antibacterial flame retardant is as follows:

2. The acrylic polymer water-based paint according to claim 1, characterized in that: The dispersant is a polyurethane oligomer or a phosphate ester active agent, the defoamer is a polyether defoamer, an organosilicon defoamer or a polyether siloxane copolymer, and the leveling agent is carboxymethyl cellulose.

3. The acrylic polymer water-based paint according to claim 1, characterized in that: The preparation method of the modified alkyd resin comprises the following steps: A. Add castor oil, E-44 epoxy resin and trimethylolpropane into a reactor, heat it to 110-130°C, add LiOH, and then slowly heat it to 230-240°C for full reaction to obtain an alcoholysis product; B. Cool the alcoholysis product to 140-160°C, add phthalic anhydride, xylene and benzoic acid, heat to 220-230°C and reflux until the acid value is lower than 10 mgKOH / g, then stop heating to obtain an esterification product; C. Vacuum the esterification product to remove xylene, cool it to 150-170°C, add trimellitic anhydride, heat it up for esterification and dehydration, and keep the temperature to react until the acid value reaches 40-60 mgKOH / g, then stop the reaction; D. When the system temperature drops to 55-65°C, add a certain proportion of triethylamine for neutralization for 8-10 minutes, then add a certain amount of water, and stir and disperse with a high-speed disperser for 30 minutes to obtain the modified alkyd resin.

4. The acrylic polymer water-based paint according to claim 3, characterized in that: The mass ratio of the castor oil, E-44 epoxy resin, phthalic anhydride and trimellitic anhydride is 40-50:3-5:8-10:12-15.

5. The acrylic polymer water-based paint according to claim 1, characterized in that: The preparation method of the modified nano silicon dioxide comprises the following steps: (1) 1,2-benzisothiazol-3-one, potassium carbonate and N,N-dimethylformamide are mixed, and then tribromoneopentyl alcohol is slowly added at room temperature, and the mixture is heated to 70° C. and stirred for reaction for 10 to 12 hours. After the reaction, deionized water is added to dissolve the product, and then the mixed solution is extracted with ethyl acetate. Anhydrous magnesium sulfate is added to the extract to dehydrate the extract, and then the extract is filtered. The ethyl acetate is removed by rotary evaporation of the filtrate, and finally the intermediate A is purified by a chromatographic column; (2) Add cyanuric chloride to 1,4-dioxane and triethylamine under a nitrogen atmosphere, stir to dissolve the cyanuric chloride, then uniformly add 3-aminopropyltriethoxysilane, react in an ice bath for 1 to 3 hours after the addition is completed, add intermediate A to the reaction system, then heat up to 40 to 50° C. at a rate of 2 to 4° C. / min, and keep the temperature for 1 to 3 hours. After the reaction is completed, cool and filter to remove triethylamine hydrochloride, remove tetrahydrofuran by vacuum distillation, add ethyl acetate, dry and filter, and vacuum distill the filtrate to obtain an antibacterial flame retardant; (3) Add nano-silica powder to a mixture of anhydrous ethanol and deionized water, and ultrasonically disperse for 10 to 15 minutes. Adjust the pH value of the solution to 4 with aqueous hydrochloric acid. Then slowly add the antibacterial flame retardant to the nano-silica solution, and ultrasonically disperse for 5 to 10 minutes. Heat to 60 to 80° C. and keep the temperature for 3 to 5 hours. After cooling, filter, wash, and dry to obtain modified nano-silica.

6. The acrylic polymer water-based paint according to claim 5, characterized in that: The molar ratio of the 1,2-benzisothiazol-3-one to tribromoneopentyl alcohol is 3:

1.

7. The acrylic polymer water-based paint according to claim 5, characterized in that: The molar ratio of the cyanuric chloride, 3-aminopropyltriethoxysilane and intermediate A is 1:1:

2.

8. A method for preparing an acrylic polymer water-based coating as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: A water-based acrylic resin, a modified alkyd resin, a dispersant, a defoamer, a leveling agent and water are mixed to obtain a mixed liquid; then the modified nano-silicon dioxide is added to the mixed liquid and dispersed at a high speed to obtain a water-based coating.

Citation Information

Patent Citations

  • Triazine type siloxane surface modifier and preparation method thereof

    CN102952158A

  • Triazine ring-containing phosphorus-nitrogen-silicon compound and preparation method thereof

    CN103980315A

  • Epoxy-modified water-based alkyd resin and water-based alkyd amino stoving varnish and preparation method of epoxy-modified water-based alkyd resin and water-based alkyd amino stoving varnish.

    CN104072742A

  • Resin composition for water-based high-performance color gloss coating and preparation method of resin composition

    CN104293134A

  • Nano-silica modified macromolecular flame-retardant charring agent and preparation method thereof

    CN112321895A

Cited By

  • Water-based acrylic modified alkyd resin and preparation method thereof

    CN119119506A

  • A kind of waterborne acrylic acid modified alkyd resin and preparation method thereof

    CN119119506B

  • Environment-friendly sponge and application thereof

    CN119463110A

  • Water-based color-changing paint for ceramic surface layer and preparation method of water-based color-changing paint

    CN121022184A