Modified cyanoacrylate adhesive and preparation method thereof
By adding carbazole cross-linked polyacrylate shell core particles with a multi-level spatial cross-linking network structure into cyanoacrylate adhesive, the problem of insufficient toughness and heat resistance of cyanoacrylate adhesive is solved and significantly improved Improved its mechanical properties and impact resistance at high temperatures.
Patent Information
- Application Number
- CN202411025879.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-18
AI Technical Summary
Cyanoacrylate adhesives have poor toughness and heat resistance, poor impact resistance, and are difficult to maintain good mechanical properties in high temperature environments.
Modified cyanoacrylate glue containing carbazole cross-linked polyacrylate shell core particles was used to prepare carbazole cross-linked polyacrylate shell core particles with a multi-level spatial cross-linked network structure through seeded semi-continuous emulsion cross-linking polymerization. , as a toughening agent and impact modifier, it can improve the tensile shear strength and shear impact strength of the adhesive, and improve its heat resistance.
Significantly improves the tensile shear strength and shear impact strength of cyanoacrylate adhesive, enhances its retention rate at high temperatures, improves heat resistance, and ensures that it still has high mechanical strength at high temperatures of 100°C performance.
Smart Images

Figure CN118791995A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a modified cyanoacrylate adhesive and a preparation method thereof. Background Art
[0002] Adhesives are widely used in the fields of construction materials, electrical and electronic, electromechanical engineering, packaging industry, etc. Among them, cyanoacrylate adhesives have the advantages of high activity, fast curing speed, high transparency, low toxicity, etc., and have important applications in medicine, precious metals, precision instruments, etc. However, cyanoacrylate adhesives have poor heat resistance, usually the applicable temperature is below 70-80℃, and the toughness is poor, and the impact resistance is poor. Therefore, it is necessary to improve the toughness, impact resistance, heat resistance and other properties of cyanoacrylate adhesives.
[0003] Adding plasticizers, elastomers, impact modifiers and other additives to cyanoacrylate adhesives can improve their mechanical properties. Such as polyurethane rubber, nitrile rubber, core-shell particles, etc.; polyacrylate core-shell particles are a common impact modifier with good mechanical properties and simple preparation methods. They can improve the toughness and impact resistance of materials and are widely used in adhesives, coatings, plastics and other fields. The present invention aims to improve the comprehensive performance of cyanoacrylate adhesives by using polyacrylate core-shell particles containing carbazole benzyl condensed ring structures. Summary of the invention
[0004] (I) Technical problems solved: The present invention solves the problems of poor toughness and poor heat resistance of cyanoacrylate adhesive.
[0005] (II) Technical solution: A modified cyanoacrylate adhesive, comprising 85-99 parts by weight of cyanoacrylate adhesive and 1-15 parts by weight of carbazole cross-linked polyacrylate core-shell particles.
[0006] The preparation method of carbazole cross-linked polyacrylate core-shell particles is as follows:
[0007] (1) Add deionized water, methyl (meth)acrylate and emulsifier into reaction bottle a and stir evenly to obtain a core emulsion.
[0008] (2) Add deionized water, butyl (meth)acrylate, 1,4-di(2-acrylatecarbazole)benzyl component 1, and an emulsifier to the reaction flask b, stir evenly, and obtain a shell emulsion.
[0009] (3) adding 10-15% by volume of the core emulsion to the reaction flask c, introducing nitrogen, heating to 70-85° C., adding an initiator, carrying out a prepolymerization reaction, and then adding the remaining 85-90% by volume of the core emulsion and adding 1,4-di(2-acrylate carbazole)benzyl component 2 to carry out a core polymerization reaction; finally, adding the shell emulsion and the initiator to carry out a shell polymerization reaction, cooling, adding methanol to break the emulsion, filtering, washing with ethanol, and drying to obtain carbazole cross-linked polyacrylate core-shell particles.
[0010] The ratio of methyl (meth)acrylate, butyl (meth)acrylate, 1,4-di(2-acrylate carbazole)benzyl component a, and 1,4-di(2-acrylate carbazole)benzyl component b is 1 mol:(1.4-2.2) mol:(0.01-0.024):(0.004-0.006) mol.
[0011] Wherein, the emulsifier is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate; and the initiator is ammonium persulfate or potassium persulfate.
[0012] The time of prepolymerization reaction is 10-20 minutes; the time of core polymerization reaction is 40-60 minutes; and the time of shell polymerization reaction is 2-3 hours.
[0013] Wherein, the preparation method of 1,4-di(2-acrylate carbazole)benzyl is:
[0014] S1. Add N,N-dimethylformamide and 2-hydroxycarbazole to a reaction bottle, introduce nitrogen, dropwise add a tetrahydrofuran solution containing sodium hydride, mix well, add 1,4-dichlorobenzyl, wherein the molar ratio of 2-hydroxycarbazole, sodium hydride and 1,4-dichlorobenzyl is (2-2.3):(4.5-5.5):1; heat to 45-60°C, react for 6-12h, add deionized water, extract and wash with dichloromethane, combine the dichloromethane organic phase, rotary evaporate, separate by silica gel column chromatography, and obtain 1,4-di(2-hydroxycarbazole)benzyl.
[0015] S2. Add dichloromethane, pyridine in a molar ratio of (2-2.4):1:(2-2.2), 1,4-di(2-hydroxycarbazole)benzyl and acryloyl chloride into a reaction bottle. After the reaction, rotary evaporate and separate by silica gel column chromatography to obtain 1,4-di(2-acrylatecarbazole)benzyl.
[0016] The reaction temperature in S2 is 25-40°C and the reaction time is 18-24h.
[0017] (III) Technical effect: The present invention uses methyl (meth)acrylate as the core, butyl (meth)acrylate as the shell, and 1,4-di(2-acrylate carbazole)benzyl containing two alkenyl groups as the crosslinking agent. After seed semi-continuous emulsion crosslinking polymerization, carbazole crosslinked polyacrylate core-shell particles with a multi-level spatial crosslinked network structure are obtained. The core-shell particles can be used as toughening agents and impact modifiers. When the adhesive is stretched or impacted by external forces, the spatial crosslinked network structure of the core-shell particles acts as a stress concentrator, which can transfer and buffer stress and inhibit further crack expansion, thereby achieving good toughening and impact resistance effects, and significantly improving the tensile shear strength and shear impact strength of the adhesive.
[0018] The carbazole cross-linked polyacrylate core-shell particles of the present invention contain a large amount of dicarbazole benzyl fused ring structures, have high thermal stability, and good thermal decomposition resistance. When added to cyanoacrylate adhesive, the heat resistance of the adhesive can be improved. After being placed at a high temperature of 100° C., the particles still have high tensile shear strength and shear impact strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the reaction formula for preparing 1,4-di(2-acrylatecarbazole)benzyl. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0021] The cyanoacrylate glue of the present invention is LOCTITE 411.
[0022] Example 1
[0023] S1. Add 2 mL of N,N-dimethylformamide and 9.2 mmol of 2-hydroxycarbazole (CAS No. 86-79-3) to a reaction bottle, introduce nitrogen, dropwise add 15 mL of tetrahydrofuran solution containing 18 mmol of sodium hydride, mix well, add 4 mmol of 1,4-dichlorobenzyl (CAS No. 623-25-6), heat to 60°C, react for 6 hours, add deionized water, extract and wash with dichloromethane, combine the dichloromethane organic phase, rotary evaporate, separate by silica gel column chromatography, and use a solution of dichloromethane and methanol in a volume ratio of 95:5 as the eluent to obtain 1,4-di(2-hydroxycarbazole)benzyl.
[0024] S2. Add 25 mL of dichloromethane, 10 mmol of pyridine, 5 mmol of 4-di(2-hydroxycarbazole)benzyl and 10 mmol of acryloyl chloride to the reaction bottle, react at 40°C for 18 h, rotary evaporate, separate by silica gel column chromatography, and use a solution of dichloromethane and methanol in a volume ratio of 90:10 as the eluent to obtain 1,4-di(2-acrylatecarbazole)benzyl.
[0025] Example 2
[0026] S1. Add 1.5 mL of N,N-dimethylformamide and 8 mmol of 2-hydroxycarbazole to a reaction bottle, introduce nitrogen, dropwise add 20 mL of a tetrahydrofuran solution containing 22 mmol of sodium hydride, mix well, add 4 mmol of 1,4-dichlorobenzyl, heat to 45°C, react for 12 h, add deionized water, extract and wash with dichloromethane, combine the dichloromethane organic phases, rotary evaporate, separate by silica gel column chromatography, and use a solution of dichloromethane and methanol in a volume ratio of 95:5 as the eluent to obtain 1,4-di(2-hydroxycarbazole)benzyl.
[0027] S2. Add 30 mL of dichloromethane, 12 mmol of pyridine, 5 mmol of 4-di(2-hydroxycarbazole)benzyl and 11 mmol of acryloyl chloride to the reaction bottle, react at 20°C for 24 h, rotary evaporate, separate by silica gel column chromatography, and use a solution of dichloromethane and methanol in a volume ratio of 90:10 as eluent to obtain 1,4-di(2-acrylatecarbazole)benzyl.
[0028] Example 3
[0029] (1) Prepare 1,4-di(2-acrylatecarbazole)benzyl according to the method of Example 2.
[0030] (2) Add 8 mL of deionized water, 50 mmol of methyl acrylate, and 0.021 g of emulsifier sodium dodecyl sulfate to reaction bottle a and stir evenly to obtain a core emulsion.
[0031] (3) Add 20 mL of deionized water, 70 mmol of butyl acrylate, 0.5 mmol of 1,4-di(2-acrylatecarbazole)benzyl, and 0.036 g of emulsifier sodium dodecyl sulfate to the reaction flask b, and stir evenly to obtain a shell emulsion.
[0032] (4) Add 15% of the core emulsion by volume to the reaction bottle c, introduce nitrogen, heat to 75° C., add 0.03 g of initiator ammonium persulfate, and perform prepolymerization for 20 min. Then add the remaining 85% of the core emulsion by volume, and add 0.2 mmol 1,4-di(2-acrylate carbazole)benzyl, and perform core polymerization for 60 min. Finally, add the shell emulsion and 0.052 g of initiator ammonium persulfate, and perform shell polymerization for 2 h. After cooling, add methanol to break the emulsion, filter, wash with ethanol, and dry to obtain carbazole cross-linked polyacrylate core-shell particles.
[0033] Example 4
[0034] (1) Prepare 1,4-di(2-acrylatecarbazole)benzyl according to the method of Example 2.
[0035] (2) Add 10 mL of deionized water, 50 mmol of methyl methacrylate, and 0.034 g of emulsifier sodium dodecylbenzene sulfonate to reaction bottle a and stir evenly to obtain a core emulsion.
[0036] (3) Add 25 mL of deionized water, 90 mmol of butyl methacrylate, 0.8 mmol of 1,4-di(2-acrylatecarbazole)benzyl, and 0.045 g of an emulsifier, sodium dodecylbenzenesulfonate or sodium dodecyl sulfate, to the reaction flask b, and stir evenly to obtain a shell emulsion.
[0037] (4) Add 10% of the core emulsion by volume to the reaction flask c, introduce nitrogen, raise the temperature to 70° C., add 0.035 g of initiator potassium persulfate, and perform a prepolymerization reaction for 20 min. Then add the remaining 90% of the core emulsion by volume, and add 0.25 mmol 1,4-di(2-acrylate carbazole)benzyl, and perform a core polymerization reaction for 60 min. Finally, add the shell emulsion and 0.06 g of initiator potassium persulfate, and perform a shell polymerization reaction for 3 h. After cooling, add methanol to break the emulsion, filter, wash with ethanol, and dry to obtain carbazole cross-linked polyacrylate core-shell particles.
[0038] Example 5
[0039] (1) Prepare 1,4-di(2-acrylatecarbazole)benzyl according to the method of Example 2.
[0040] (2) Add 10 mL of deionized water, 50 mmol of methyl acrylate, and 0.034 g of emulsifier sodium dodecylbenzene sulfonate to reaction bottle a and stir evenly to obtain a core emulsion.
[0041] (3) Add 30 mL of deionized water, 110 mmol of butyl acrylate, 1.2 mmol of 1,4-di(2-acrylatecarbazole)benzyl, and 0.052 g of emulsifier sodium dodecylbenzenesulfonate to the reaction flask b, and stir evenly to obtain a shell emulsion.
[0042] (4) Add 15% of the core emulsion by volume to the reaction flask c, introduce nitrogen, heat to 85° C., add 0.037 g of initiator potassium persulfate, and perform prepolymerization for 20 min. Then add the remaining 85% of the core emulsion by volume, and add 0.3 mmol 1,4-di(2-acrylate carbazole)benzyl, and perform core polymerization for 40 min. Finally, add the shell emulsion and 0.065 g of initiator potassium persulfate, and perform shell polymerization for 2 h. After cooling, add methanol to break the emulsion, filter, wash with ethanol, and dry to obtain carbazole cross-linked polyacrylate core-shell particles.
[0043] Comparative Example 1
[0044] (1) Add 8 mL of deionized water, 50 mmol of methyl acrylate, and 0.021 g of emulsifier sodium dodecyl sulfate to a reaction bottle a and stir evenly to obtain a core emulsion.
[0045] (3) Add 20 mL of deionized water, 70 mmol of butyl acrylate, and 0.036 g of emulsifier sodium dodecyl sulfate to the reaction flask b, and stir evenly to obtain a shell emulsion.
[0046] (4) Add 15% of the volume of the core emulsion to the reaction bottle c, introduce nitrogen, heat to 75°C, add 0.03g of initiator ammonium persulfate, carry out prepolymerization for 20 minutes, then add the remaining 85% of the volume of the core emulsion, carry out core polymerization for 60 minutes; finally, add the shell emulsion, 0.052g of initiator ammonium persulfate, carry out shell polymerization for 2 hours, cool, add methanol to break the emulsion, filter, wash with ethanol and dry to obtain polyacrylate core-shell particles.
[0047] Comparative Example 2
[0048] (1) Add 8 mL of deionized water, 50 mmol of methyl acrylate, and 0.021 g of emulsifier sodium dodecyl sulfate to a reaction bottle a and stir evenly to obtain a core emulsion.
[0049] (2) Add 20 mL of deionized water, 70 mmol of butyl acrylate, and 0.5 mmol of N-vinyl carbazole (CAS No. 1484-13-5, structural formula: ), 0.036 g of emulsifier sodium dodecyl sulfate, stir evenly to obtain a shell emulsion.
[0050] (3) Add 15% of the core emulsion by volume to the reaction bottle c, introduce nitrogen, raise the temperature to 75°C, add 0.03g of initiator ammonium persulfate, and carry out prepolymerization for 20 minutes, then add the remaining 85% of the core emulsion by volume, and add 0.2mmol N-vinylcarbazole, and carry out core polymerization for 60 minutes; finally, add the shell emulsion and 0.052g of initiator ammonium persulfate, and carry out shell polymerization for 2 hours. After cooling, add methanol to break the emulsion, filter, wash with ethanol and dry to obtain carbazole-based polyacrylate core-shell particles.
[0051] To 990 g of cyanoacrylate glue, the polyacrylate core-shell particles (10 g) of the example and the comparative example were added respectively, and the mixture was mixed to obtain modified cyanoacrylate glue.
[0052] The tensile shear strength and shear impact strength were tested according to GB T 7124-2008 and GB / T 6328-2021 methods. The test substrate was carbon steel-carbon steel, and the coating was cured and overlapped at 25°C. The specimens were then placed at 25°C, 70°C, and 100°C for 24 hours before testing. The test results are shown in the table below.
[0053]
[0054] Comparative Example 3 is cyanoacrylate glue without adding polyacrylate core-shell particles.
[0055]
[0056]
[0057] After testing, comparative example 3 is unmodified cyanoacrylate glue without adding polyacrylate core-shell particles. After being placed at 25°C for 24 hours, the tensile shear strength is 10.9 MPa and the shear impact strength is 9.2 kJ / m 2 However, after being placed at 100°C for 24 hours, the tensile shear strength was only 3.1MPa, with a retention rate of 28.4%, and the shear impact strength was only 2.8kJ / m 2 The retention rate is 30.4%, the mechanical properties are poor, and the high temperature resistance is poor.
[0058] In Example 3-5, methyl (meth)acrylate is used as the core, butyl (meth)acrylate is used as the shell layer, and 1,4-di(2-acrylate carbazole)benzyl containing two alkenyl groups is used as a crosslinking agent. After seed semi-continuous emulsion crosslinking polymerization, carbazole crosslinked polyacrylate core-shell particles with a multi-level spatial crosslinked network structure are obtained. The core-shell particles can be used as a toughening agent and an impact modifier. When the adhesive is stretched or impacted by an external force, the spatial crosslinked network structure of the core-shell particles acts as a stress concentrator, which can transfer and buffer stress and inhibit further crack expansion, thereby achieving a good toughening and impact resistance effect, and significantly improving the tensile shear strength and shear impact strength of the adhesive to 13.9-16.4MPa and 17.5-19.7kJ / m 2 In addition, the carbazole cross-linked polyacrylate core-shell particles contain a large amount of dicarbazole benzyl fused ring structures. It has high thermal stability and good resistance to thermal decomposition. When added to cyanoacrylate glue, the heat resistance of the adhesive can be improved. After being placed at a high temperature of 100°C, it still has high tensile shear strength and shear impact strength. The tensile shear strength retention rate of Example 3 is 52.9% (8.1÷15.3), and the shear impact strength retention rate is 53.1% (9.3÷17.5).
[0059] The difference between Comparative Example 1 and Example 3 is that 1,4-di(2-acrylate carbazole)benzyl crosslinking agent is not added, and the obtained polyacrylate core-shell particles do not contain a multi-layered spatial crosslinked network structure, and the toughening and impact modification effects on cyanoacrylate adhesive are not good, and the tensile shear strength and shear impact strength are lower than those in Example 1. In addition, the polyacrylate core-shell particles do not contain a dicarbazole benzyl fused ring structure, and the thermal stability and thermal decomposition resistance are poor, resulting in a large decrease in the tensile shear strength and shear impact strength of the adhesive after being placed at high temperature, and a low retention rate.
[0060] The difference between Comparative Example 2 and Example 3 is that N-vinyl carbazole is used instead of 1,4-di(2-acrylate carbazole)benzyl, and N-vinyl carbazole contains only one olefinic group and cannot undergo crosslinking polymerization reaction. The obtained polyacrylate core-shell particles do not contain a multi-layered spatial crosslinked network structure, and the toughening and impact modification effects are lower than those of Example 3. After high-temperature placement, the tensile shear strength and shear impact strength retention rates are higher than those of Comparative Examples 1 and 3, but higher than those of Example 3.
[0061] 10-150 g of polyacrylate core-shell particles (prepared in Example 4) were added to 850-990 g of cyanoacrylate glue, and mixed to obtain modified cyanoacrylate glue. The mass ratio of cyanoacrylate glue to polyacrylate core-shell particles was A
[0062] The tensile shear strength and shear impact strength were tested according to GB T 7124-2008 and GB / T 6328-2021 methods. The test substrate was carbon steel-carbon steel. The coating was cured and overlapped at 25°C, and then the sample was placed at 25°C for 24 hours. The test results are shown in the table below.
[0063] A(g / g) Tensile shear strength (MPa) <![CDATA[Shearing impact strength (kJ / m 2 )]]> 990 / 10 16.4 19.7 960 / 40 27.7 26.1 920 / 80 24.0 35.6 880 / 120 21.2 39.8 850 / 150 17.9 33.8
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A modified cyanoacrylate adhesive, characterized in that: The modified cyanoacrylate glue comprises 85-99 parts by weight of cyanoacrylate glue and 1-15 parts by weight of carbazole cross-linked polyacrylate core-shell particles; The preparation method of the carbazole cross-linked polyacrylate core-shell particles is as follows: (1) adding deionized water, methyl (meth)acrylate and emulsifier into reaction bottle a and stirring evenly to obtain a core emulsion; (2) adding deionized water, butyl (meth)acrylate, 1,4-di(2-acrylatecarbazole)benzyl component 1, and an emulsifier to the reaction flask b, stirring evenly to obtain a shell emulsion; (3) adding part of the core emulsion to the reaction bottle c, introducing nitrogen, heating to 70-85° C., adding an initiator, carrying out a prepolymerization reaction, and then adding the remaining core emulsion and 1,4-di(2-acrylate carbazole)benzyl component 2 to carry out a core polymerization reaction; finally, adding the shell emulsion and initiator to carry out a shell polymerization reaction, breaking the emulsion after cooling, filtering, washing and drying to obtain carbazole cross-linked polyacrylate core-shell particles.
2. The modified cyanoacrylate adhesive according to claim 1, characterized in that: The ratio of the methyl (meth)acrylate, butyl (meth)acrylate, 1,4-di(2-acrylate carbazole)benzyl component a, and 1,4-di(2-acrylate carbazole)benzyl component b is 1 mol:(1.4-2.2) mol:(0.01-0.024):(0.004-0.006) mol.
3. The modified cyanoacrylate adhesive according to claim 1, characterized in that: The emulsifier is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate; the initiator is ammonium persulfate or potassium persulfate.
4. The modified cyanoacrylate adhesive according to claim 1, characterized in that: The time of the prepolymerization reaction is 10-20 minutes; the time of the core polymerization reaction is 40-60 minutes; and the time of the shell polymerization reaction is 2-3 hours.
5. The modified cyanoacrylate adhesive according to claim 1, characterized in that: The preparation method of 1,4-di(2-acrylate carbazole)benzyl is as follows: S1. Add N,N-dimethylformamide and 2-hydroxycarbazole to a reaction bottle, introduce nitrogen, dropwise add a tetrahydrofuran solution containing sodium hydride, mix well, add 1,4-dichlorobenzyl, raise the temperature to 45-60° C., react for 6-12 hours, extract, separate by silica gel column chromatography, and obtain 1,4-di(2-hydroxycarbazole)benzyl; S2. Add dichloromethane, pyridine, 1,4-di(2-hydroxycarbazole)benzyl and acryloyl chloride into a reaction bottle. After the reaction, separate by silica gel column chromatography to obtain 1,4-di(2-acrylatecarbazole)benzyl.
6. The modified cyanoacrylate adhesive according to claim 5, characterized in that: In the S1, the molar ratio of 2-hydroxycarbazole, sodium hydride and 1,4-dichlorobenzyl is (2-2.3):(4.5-5.5):
1.
7. The modified cyanoacrylate adhesive according to claim 5, characterized in that: In S2, the molar ratio of pyridine, 1,4-di(2-hydroxycarbazole)benzyl and acryloyl chloride is (2-2.4):1:(2-2.2).
8. The modified cyanoacrylate adhesive according to claim 5, characterized in that: The reaction temperature in S2 is 25-40°C and the reaction time is 18-24h.