Application of carbon dioxide-based terpolymer in preparation of pressure-sensitive adhesive
The pressure-sensitive adhesive prepared by copolymerizing carbon dioxide-based terpolymer and Salen-Co catalyst solves the problems of non-degradable and difficult performance control of existing pressure-sensitive adhesives, achieving high-performance, degradable pressure-sensitive adhesives without the need for additional Additives.
Patent Information
- Application Number
- CN202410847905.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing pressure-sensitive adhesives are non-degradable, have complex preparation processes and high costs, and require the addition of additional additives such as tackifiers to improve performance.
Using carbon dioxide-based terpolymer as the raw material of pressure-sensitive adhesive, it is prepared by copolymerization of Salen-Co catalyst and epoxy to form a completely alternating random copolymer with adjustable initial tack, holding force and peel strength. No additional tackifiers or plasticizers are required.
A degradable pressure-sensitive adhesive has been realized with performance comparable to or even exceeding that of commercial pressure-sensitive adhesives. The glass transition temperature of the material can be adjusted by selecting different third monomers to adapt to different environmental needs.
Smart Images

Figure BDA0004916131830000021 
Figure BDA0004916131830000031 
Figure BDA0004916131830000032
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to the application of a carbon dioxide-based terpolymer in the preparation of pressure-sensitive adhesives. Background Art
[0002] Pressure-sensitive adhesive is an adhesive that can produce adhesion with the substrate when a certain pressure is applied to it. It can be widely used in packaging, automotive parts, medical and electronic products and other fields. The viscoelasticity of pressure-sensitive adhesive refers to the ability to adhere and resist shear at the same time. It can reasonably combine these two contradictory properties. The types of adhesive materials currently available on the market mainly include polyacrylate, rubber, silicone, etc. These traditional adhesives are mostly prepared from petrochemical resources and are non-degradable materials. Moreover, they all require the addition of tackifiers, additives, etc. to enhance and improve the viscoelastic properties of pressure-sensitive adhesives. Therefore, the development of sustainable polymer pressure-sensitive adhesives has gradually become the mainstream of current research.
[0003] Carbon dioxide is cheap, widely available and non-toxic, and is also the main source of the greenhouse effect. In recent decades, large-scale emissions of carbon dioxide have caused serious harm to the environment. Therefore, the effective use of carbon dioxide to turn waste into treasure and reduce the emission and concentration of carbon dioxide in the environment has become a global issue affecting the sustainable development of human society. In the past few decades, carbon dioxide has been widely studied as a raw material for the preparation of green chemical products. It has been used in the chemical industry to produce urea, carboxylic acids, methanol, cyclic carbonates and polycarbonates. Among them, the copolymerization of carbon dioxide and epoxides under the action of catalysts to prepare carbon dioxide-based polycarbonates and carbon dioxide-based polyols has become a new way to fix carbon dioxide, which shows potential application prospects in packaging materials, coatings, adhesives and many other fields.
[0004] Due to the high stability and low reactivity of carbon dioxide, a large number of catalytic systems have been explored in the past few decades to catalyze the reaction of carbon dioxide with epoxides, such as organic catalysts and metal-based catalysts, such as K, Mg, Ca, Fe, Cr, Zn, Al and rare earth metals, to try to catalyze the reaction of epoxides with carbon dioxide. In these studies, Salen-Co catalysts (CN105618141A, CN105665022A, CN101940947A, CN101905171A, CN116874390A, CN116726994A, CN115894347A, CN116850904A, CN115028789A, CN114713287A, etc.) have shown excellent performance in the copolymerization of epoxides and carbon dioxide. Catalysts represented by Salen-Co can catalyze the complete alternating random copolymerization of carbon dioxide and epoxide to prepare carbon dioxide-based poly(carbonate-ether). The resulting polymers have different viscoelastic properties depending on the molecular weight and carbonate unit content, and have sustainable capabilities.
[0005] MW Grinstaff et al. used carbon dioxide / propylene oxide / glycidyl butyrate as comonomers to generate [S,S]-[SalcyCo III DNP] / DNP catalyst synthesized a completely alternating random copolymer, which can be used for pressure-sensitive adhesives and is also biodegradable, but the initial viscosity is better at 37°C, which limits its temperature range of use (Nat. Commun., 2019, 10, 5478). CK Williams et al. prepared a triblock copolymer based on a binuclear catalyst prepared by Robson ligand, and the resulting polymer showed good adhesive properties. However, block polymers have strict requirements for the selection of catalysts, and their adhesive strength range is narrow, making it difficult to significantly regulate performance (Angew. Chem. Int. Ed. 2020, 59, 1–7). HJ Kim et al. used cashew nut shell lactone as raw material and synthesized a new aliphatic polyester polycaprolactone (PPDCL) with long alkyl substituents by ring-opening ester exchange. The resulting polyester has adhesion properties that compete with many common commercial adhesives. This ABA triblock copolymer can be hydrolyzed and degraded, but it needs to be mixed with a renewable tackifier during use to produce sustainable pressure-sensitive adhesive materials (ACS Sustainable Chem. Eng., 2020, 8, 12036-12044).
[0006] In summary, the existing commercially available pressure-sensitive adhesives are non-degradable; degradable pressure-sensitive adhesives still have the following problems: extraction and synthesis of materials are difficult and complicated, the cost is high, and additional tackifiers are required. Summary of the invention
[0007] In view of this, the technical problem to be solved by the present invention is to provide an application of a carbon dioxide-based terpolymer in the preparation of a pressure-sensitive adhesive. The pressure-sensitive adhesive provided by the present invention is degradable and does not require the addition of other additives such as tackifiers and plasticizers. The pressure-sensitive adhesive of the present invention has adjustable initial adhesion, lasting adhesion and peel strength, and exhibits performance comparable to or even exceeding that of commercial pressure-sensitive adhesives.
[0008] The present invention provides an application of a carbon dioxide-based terpolymer in the preparation of a pressure-sensitive adhesive;
[0009] The carbon dioxide-based terpolymer has a structure shown in Formula I;
[0010]
[0011] In formula I, 5≤m≤5000, 5≤n≤5000;
[0012] The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
[0013] Preferably, R1 and R2 are independently selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, allyl or PEG groups.
[0014] Preferably, in the carbon dioxide-based terpolymer having the structure shown in Formula I, the mass content of the carbonate unit is 85% to 99%, and the mass content of the ether segment is 1% to 15%.
[0015] Preferably, the carbon dioxide-based terpolymer having the structure shown in Formula I is prepared by terpolymerization of carbon dioxide and epoxide;
[0016] The epoxides include two of propylene oxide, 1,2-butylene oxide, 2,3-butylene oxide, cyclohexene oxide, 1,2-butylene oxide, 1,2-butylene oxide, 1,2-cyclopentene oxide, epichlorohydrin, glycidyl methacrylate (PEGMA), methyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, styrene oxide, 1,2-epoxy-4-vinylcyclohexane, 2-vinylethylene oxide and 2-[2-(2-methoxyethoxy)ethoxy]ethyl glycidyl ether.
[0017] Preferably, the main catalyst of the ternary copolymerization is a Salen-Co catalyst having a structure shown in Formula II;
[0018]
[0019] Preferably, the co-catalyst for the ternary copolymerization is bis(triphenylphosphorane)trifluoroammonium acetate (PPNTFA), having the structure shown in Formula III;
[0020]
[0021] Preferably, the molar ratio of the co-catalyst to the main catalyst is 0 to 2:1;
[0022] The molar ratio of the main catalyst to the epoxide is 1:1000-5000.
[0023] Preferably, the carbon dioxide pressure of the ternary copolymerization is 0 to 20 MPa, and is not zero.
[0024] Preferably, the temperature of the terpolymerization is 20 to 30° C., and the time is 6 to 72 hours.
[0025] The present invention also provides a pressure-sensitive adhesive, which is prepared from a carbon dioxide-based terpolymer;
[0026] The carbon dioxide-based terpolymer has a structure shown in Formula I;
[0027]
[0028] In formula I, 5≤m≤5000, 5≤n≤5000;
[0029] The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
[0030] The present invention provides an application of a carbon dioxide-based terpolymer in the preparation of a pressure-sensitive adhesive; the carbon dioxide-based terpolymer has a structure shown in Formula I;
[0031]
[0032] In formula I, 5≤m≤5000, 5≤n≤5000;
[0033] The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
[0034] In the present invention, the carbon dioxide-based terpolymer uses carbon dioxide as a raw material to alleviate the greenhouse effect, which meets the needs of sustainable development. At the same time, the obtained carbon dioxide-based polycarbonate has degradability. The carbon dioxide-based terpolymer can be directly used as a pressure-sensitive adhesive without the need for additional tackifiers, plasticizers and other additives. The pressure-sensitive adhesive provided by the present invention has adjustable initial adhesion, lasting adhesion and peel strength, showing performance comparable to or even exceeding that of commercial pressure-sensitive adhesives. The carbon dioxide-based terpolymer can produce different adjustments to the synthesized pressure-sensitive adhesive by selecting different types of third monomers, which can reduce the glass transition temperature of the obtained material, meet the use environment requirements of the pressure-sensitive adhesive, and adjust the performance of the pressure-sensitive adhesive. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the H NMR spectrum of the polymer prepared in Example 1 of the present invention;
[0036] Figure 2 This is the GPC spectrum of the polymer prepared in Example 5 of the present invention;
[0037] Figure 3 180° peeling test curve of the pressure-sensitive adhesive prepared from PPC5 of the present invention;
[0038] Figure 4 This is a DSC schematic diagram of the pressure-sensitive adhesive prepared by PPC5 of the present invention;
[0039] Figure 5 It is a schematic diagram of thermal decomposition of the pressure-sensitive adhesive prepared by PPC5 of the present invention;
[0040] Figure 6 Schematic diagram of the rheology of the pressure-sensitive adhesive prepared by PPC5 of the present invention;
[0041] Figure 7 is the 180° peel strength curve of the 3M Scotch tape in Comparative Example 1;
[0042] Figure 8 This is the 180° peel strength curve of the Japanese Nitto tape in Comparative Example 2. DETAILED DESCRIPTION
[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The invention provides an application of a carbon dioxide-based terpolymer in the preparation of a pressure-sensitive adhesive; specifically, the terpolymer can be used as a raw material component for preparing the pressure-sensitive adhesive; and can also be directly used as the pressure-sensitive adhesive.
[0045] The carbon dioxide-based terpolymer has a structure shown in Formula I;
[0046]
[0047] In formula I, 5≤m≤5000, 5≤n≤5000;
[0048] The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
[0049] The carbon dioxide-based terpolymer in the present invention is polycarbonate, which has a completely alternating structure.
[0050] In certain embodiments of the present invention, R1 and R2 are independently selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, allyl or PEG groups.
[0051] In certain embodiments of the present invention, in the carbon dioxide-based terpolymer having the structure shown in Formula I, the mass content of the carbonate unit is 85% to 99%, and the mass content of the ether segment is 1% to 15%.
[0052] In certain embodiments of the present invention, the carbon dioxide-based terpolymer having the structure shown in formula I has the structure shown in formula (1):
[0053]
[0054] Among them, 5≤m≤5000, 5≤n≤5000.
[0055] In certain embodiments of the present invention, the carbon dioxide-based terpolymer having the structure shown in Formula I is prepared by terpolymerization of carbon dioxide and epoxide; the epoxide is selected from two of propylene oxide, 1,2-butylene oxide, 2,3-butylene oxide, cyclohexene oxide, 1,2-epoxyhexane, 1,2-epoxyhexane, 1,2-epoxycyclopentane, epichlorohydrin, methacrylic acid glycidyl ether (PEGMA), methyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, styrene oxide, 1,2-epoxy-4-vinylcyclohexane, 2-vinyl ethylene oxide and 2-[2-(2-methoxyethoxy)ethoxy]ethyl glycidyl ether (ME3GE).
[0056] The main catalyst of the ternary copolymerization is a Salen-Co catalyst having a structure shown in Formula II;
[0057]
[0058] The present invention has no special restriction on the source of the Salen-Co catalyst, and a conventional preparation method can be adopted, or the catalyst can be prepared according to the method disclosed in patent documents CN105618141A, CN105665022A, CN101940947A, CN101905171A, CN116874390A, CN116726994A, CN115894347A, CN116850904A, CN115028789A, and CN114713287A.
[0059] The co-catalyst for the ternary copolymerization is bis(triphenylphosphorane)ammonium trifluoroacetate (PPNTFA), having the structure shown in Formula III;
[0060]
[0061] In certain embodiments of the present invention, the method for preparing bis(triphenylphosphorane)ammonium trifluoroacetate (PPNTFA) comprises the following steps:
[0062] The aqueous solution of NaX is mixed with PPNCl, and reacted at 45-55°C. The obtained turbid liquid is filtered while hot, and the filter residue is recrystallized in dichloromethane to obtain the product PPNX; wherein X = TFA;
[0063]
[0064] The molar ratio of NaX to PPNCl is 1:1. The reaction temperature is 50°C and the reaction time is 1 to 3 hours, such as 2 hours. The number of recrystallizations is 3 times.
[0065] The molar ratio of the co-catalyst to the main catalyst is 0 to 2:1, such as 1:1.
[0066] The molar ratio of the main catalyst to the epoxide is 1:1000-5000, such as 1:2000.
[0067] The carbon dioxide pressure of the ternary copolymerization is 0-20 MPa, and is not 0; for example, 2 MPa, 4 MPa, 6 MPa.
[0068] The temperature of the terpolymerization is 20-30°C, such as 25°C, and the time is 6-72h, such as 24h. The terpolymerization is carried out under stirring, and the stirring rate is 50-1000rpm, such as 500rpm.
[0069] After the ternary copolymerization is completed, the method further comprises: cooling in an ice water bath.
[0070] The carbonate unit content and the ether segment content of the polycarbonate can be adjusted by the co-catalyst and the carbon dioxide pressure.
[0071] The present invention also provides a pressure-sensitive adhesive, which is prepared from a carbon dioxide-based terpolymer;
[0072] The carbon dioxide-based terpolymer is the carbon dioxide-based terpolymer described above.
[0073] In certain embodiments of the present invention, the method for preparing the pressure-sensitive adhesive comprises the following steps:
[0074] A) mixing the carbon dioxide-based terpolymer with a solvent to obtain a polymer solution;
[0075] B) uniformly coating the polymer solution on a substrate and removing the solvent to obtain a pressure-sensitive adhesive;
[0076] The carbon dioxide-based terpolymer is the carbon dioxide-based terpolymer described above.
[0077] In step A):
[0078] In certain embodiments of the present invention, the solvent is acetone.
[0079] In certain embodiments of the present invention, the concentration of the polymer solution is 0.2-0.6 mg / mL; for example, 0.2 mg / mL, 0.4 mg / mL, 0.6 mg / mL.
[0080] In step B):
[0081] In certain embodiments of the present invention, the coating is performed using a wire rod coater with a specification of 50 μm.
[0082] In some embodiments of the present invention, the substrate is a PET film, specifically a PET film with a size of A4 paper and a thickness of 50 μm.
[0083] In certain embodiments of the present invention, the method for removing the solvent comprises:
[0084] At room temperature, place in a fume hood for 10 to 14 hours to evaporate the solvent.
[0085] Beneficial effects:
[0086] 1) The carbon dioxide-based terpolymer uses carbon dioxide as a raw material, which alleviates the greenhouse effect and meets the needs of sustainable development. At the same time, the obtained carbon dioxide-based polycarbonate has degradability.
[0087] 2) The carbon dioxide-based terpolymer can be used directly as a pressure-sensitive adhesive without the need for additional tackifiers, plasticizers and other additives, and has good and adjustable peel strength performance (0.05-5N / cm). Its molecular weight is between 5kg / mol and 200kg / mol, and the mass content of carbonate units is between 85% and 99%. It has a fairly strong peel strength (0.4-18N / cm), and exhibits adjustable initial adhesion (between balls 1 and 7) and high lasting adhesion (up to 100h).
[0088] 3) The pressure-sensitive adhesive prepared by the present invention has adjustable initial adhesion, sustained adhesion and peel strength, and exhibits performance comparable to or even exceeding that of commercial pressure-sensitive adhesives.
[0089] 4) The carbon dioxide-based terpolymer can produce different adjustments to the synthesized pressure-sensitive adhesive by selecting different types of third monomers, which can reduce the glass transition temperature of the obtained material, meet the use environment requirements of the pressure-sensitive adhesive, and adjust the performance of the pressure-sensitive adhesive.
[0090] The present invention has no particular limitation on the sources of the raw materials used above, and they can be generally commercially available.
[0091] In order to further illustrate the present invention, the application of a carbon dioxide-based terpolymer provided by the present invention in the preparation of a pressure-sensitive adhesive is described in detail below in conjunction with examples, but it should not be construed as limiting the scope of protection of the present invention.
[0092] Preparation of Salen-Co catalyst having the structure shown in Formula II:
[0093]
[0094] The ligand Ln (0.01 mol) was dissolved in a three-necked flask containing 150 mL of dichloromethane and stirred at room temperature. After the ligand was completely dissolved, an anhydrous ethanol solution containing 0.012 mol of Co(OAc)2 was added and stirred for 1 h. After the reaction was completed, it was cooled to room temperature and filtered. The filter cake was repeatedly washed with anhydrous ethanol solution to obtain a red solid for standby use. The red solid (0.01 mmol) and CF3COOH (0.01 mmol) were dissolved in 20 mL of dichloromethane, oxygen was introduced, and stirred at room temperature in the dark for 2 h. After the reaction was complete, the crude product was filtered and the solvent in the filtrate was removed by rotary evaporation to obtain the crude product. The crude product was recombinated with ether and n-hexane to obtain the product. Then, after dissolving with dichloromethane, 1 mL of trifluoroacetic acid was immediately added dropwise and stirred at room temperature in air overnight. The solvent was then evaporated to dryness at 20-25°C. The solid was dissolved with dichloromethane and then recrystallized with n-hexane. Finally, the solid was filtered out, which was the final product (Salen-Co catalyst with the structure shown in Formula II).
[0095] ME3GE has the structure shown in Formula IV;
[0096]
[0097] Preparation of the ME3GE:
[0098] Epichlorohydrin (92.5 g, 1.0 mol) and sodium hydroxide (60.0 g, 1.5 mmol) were added into a round-bottom flask. While stirring at room temperature, 1.0 mol of triethylene glycol monomethyl ether (TGE) was added dropwise. After the addition was completed, the mixture was stirred at room temperature for 3 h. After the stirring was completed, the reaction mixture was filtered to remove excess NaOH and the formed NaCl. The remaining liquid was colorless and transparent, or with a little yellow transparent liquid; it was then dried with MgSO4, and the product was further dried with CaH2 vacuum distillation.
[0099] Preparation of PPNTFA:
[0100] NaX (10 mmol) was dissolved in 10 mL of deionized water, and then PPNCl (5.74 g, 10 mmol) was added, and the mixture was reacted at 50° C. for 2 h. The obtained turbid solution was filtered while hot, and the residue was recrystallized from dichloromethane three times to obtain the product PPNX; wherein X = TFA;
[0101]
[0102] Preparation Example 1
[0103] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 200 eq. of ME3GE, 1.1 eq. of Salen-Co catalyst and 1.1 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0104] The reactor was placed in a 25°C water bath and filled with 2MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000):
[0105]
[0106] Figure 1 This is the hydrogen NMR spectrum of the polymer prepared in Example 1 of the present invention.
[0107] GPC test showed that its molecular weight was 70.8 kg / mol and its molecular weight distribution was 1.35; NMR test showed that its conversion rate was 95%, carbonate unit content was 99%, and polymer selectivity was 99%. It was recorded as PPC1.
[0108] Preparation Example 2
[0109] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 200 eq. of ME3GE, 1.1 eq. of Salen-Co catalyst and 1.1 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0110] The reactor was placed in a 25°C water bath and filled with 4MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid (to remove the catalyst in the polymer). The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0111] GPC test showed that its molecular weight was 71.9 kg / mol and its molecular weight distribution was 1.33; NMR test showed that its conversion rate was 97%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC2.
[0112] Preparation Example 3
[0113] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 200 eq. of ME3GE, 1.1 eq. of Salen-Co catalyst and 1.1 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0114] The reactor was placed in a 25°C water bath and filled with 6MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0115] GPC test showed that its molecular weight was 71.2 kg / mol and its molecular weight distribution was 1.35; NMR test showed that its conversion rate was 94%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC3.
[0116] Preparation Example 4
[0117] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 4000 eq. of propylene oxide, 500 eq. of ME3GE, 2.25 eq. of Salen-Co catalyst and 2.25 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0118] The reactor was placed in a 25°C water bath and filled with 6MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0119] GPC test showed that its molecular weight was 67.4 kg / mol and its molecular weight distribution was 1.31; NMR test showed that its conversion rate was 96%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC4.
[0120] Preparation Example 5
[0121] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 3000 eq. of propylene oxide, 500 eq. of ME3GE, 1.75 eq. of Salen-Co catalyst and 1.75 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0122] The reactor was placed in a 25°C water bath and filled with 6MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0123] Figure 2 This is the GPC spectrum of the polymer prepared in Example 5 of the present invention.
[0124] GPC test showed that its molecular weight was 62.2 kg / mol and its molecular weight distribution was 1.36; NMR test showed that its conversion rate was 93%, carbonate unit content was 94%, and polymer selectivity was 99%. It was recorded as PPC5.
[0125] Preparation Example 6
[0126] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 400 eq. of ME3GE, 1.2 eq. of Salen-Co catalyst and 1.2 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0127] The reactor was placed in a 25°C water bath and filled with 6MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0128] GPC test showed that its molecular weight was 56.1 kg / mol and its molecular weight distribution was 1.31; NMR test showed that its conversion rate was 94%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC6.
[0129] Preparation Example 7
[0130] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 500 eq. of ME3GE, 1.25 eq. of Salen-Co catalyst and 1.25 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0131] The reactor was placed in a 25°C water bath and filled with 6MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0132] GPC test showed that its molecular weight was 46.3 kg / mol and its molecular weight distribution was 1.37; NMR test showed that its conversion rate was 96%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC7.
[0133] Preparation Example 8
[0134] Using a Salen-Co catalyst having a structure shown in Formula II as a main catalyst, using a PPNTFA having a structure shown in Formula III as a co-catalyst, using propylene oxide PO as an epoxy monomer, 2000 eq. of propylene oxide, 1000 eq. of ME3GE, 1.5 eq. of Salen-Co catalyst and 1.5 eq. of PPNTFA were added into a 50 mL reactor in a glove box;
[0135] The reactor was placed in a 25°C water bath and filled with 4MPa of carbon dioxide. The reaction was stirred at 500rpm for 24h. After the reaction was completed, it was placed in an ice water bath for 15min. Part of the sample was tested for H NMR spectrum, and the remaining sample was dissolved in dichloromethane and precipitated in a 5wt% methanol solution of hydrochloric acid. The obtained polymer was filtered and dried for use. The polymer has a structure shown in formula (1) (wherein 5≤m≤5000, 5≤n≤5000).
[0136] GPC test showed that its molecular weight was 39.4 kg / mol and its molecular weight distribution was 1.34; NMR test showed that its conversion rate was 98%, carbonate unit content was 95%, and polymer selectivity was 99%. It was recorded as PPC8.
[0137] Preparation and testing of pressure-sensitive adhesive:
[0138] Example 1
[0139] PPC1 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 4 balls, the lasting adhesion is 0.5h, and the peel strength is 0.6N / cm.
[0140] Example 2
[0141] PPC1 was dissolved in acetone to prepare a 0.4 mg / mL polymer solution. 4 mL of the 0.4 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 10 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 4 balls, the lasting adhesion is 0.7h, and the peel strength is 1.5N / cm.
[0142] Example 3
[0143] PPC1 was dissolved in acetone to prepare a 0.6 mg / mL polymer solution. 4 mL of the 0.6 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. A 50 μm thick PET release film was then covered on it, and the thickness of the adhesive layer was measured to be 15 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 4 balls, the lasting adhesion is 0.8h, and the peel strength is 2.1N / cm.
[0144] Example 4
[0145] PPC2 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 3 balls, the lasting adhesion is 2h, and the peel strength is 2.5N / cm.
[0146] Example 5
[0147] PPC3 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 3 balls, the lasting adhesion is 8h, and the peel strength is 2.8N / cm.
[0148] Example 6
[0149] PPC4 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. A 50 μm thick PET release film was then covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 3 ball, the lasting adhesion is 5h, and the peel strength is 3.2N / cm.
[0150] Example 7
[0151] PPC5 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 2 ball, the lasting adhesion is 40h, and the peel strength is 5N / cm.
[0152] Figure 3 180° peeling test curve of the pressure-sensitive adhesive prepared by PPC5 of the present invention. Figure 3 It can be seen that the peel strength of the pressure-sensitive adhesive is 5N / cm.
[0153] Figure 4 The DSC diagram of the pressure-sensitive adhesive prepared by PPC5 of the present invention is shown in FIG. Figure 4 It can be seen that the glass transition temperature of the pressure-sensitive adhesive is -23°C.
[0154] Figure 5 Schematic diagram of thermal decomposition of the pressure-sensitive adhesive prepared by PPC5 of the present invention. Figure 5It can be seen that the thermal decomposition temperature of the pressure-sensitive adhesive is 220°C, and the maximum decomposition temperature is 236 / 295°C.
[0155] Figure 6 Schematic diagram of the rheology of the pressure-sensitive adhesive prepared by PPC5 of the present invention. Figure 6 It can be seen that within the application frequency range of 0.01Hz to 100Hz of the pressure-sensitive adhesive, the storage modulus and loss modulus of the polymer PPC5 are within 10 3 ~10 6 Pa, meeting the use requirements of pressure-sensitive adhesive for modulus 10 3 ~10 6 Pa.
[0156] Example 8
[0157] PPC6 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 1 ball, the lasting adhesion is 70h, and the peel strength is 8N / cm.
[0158] Example 9
[0159] PPC7 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. A 50 μm thick PET release film was then covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is 1 ball, the sustained adhesion is 150h, and the peel strength is 14N / cm.
[0160] Example 10
[0161] PPC8 was dissolved in acetone to prepare a 0.2 mg / mL polymer solution. 4 mL of the 0.2 mg / mL polymer solution was evenly coated on a 50 μm thick PET film of A4 size using a 50 μm wire rod coater, and the film was left standing in a fume hood at room temperature for 12 hours to evaporate and remove the solvent. Then a 50 μm thick PET release film was covered on it, and the thickness of the adhesive layer was measured to be 5 μm. A 25 mm fixed width knife was used to cut it into 25×300 mm strips, and the strips were placed on a 50×150 mm mirror stainless steel plate. A 2 kg steel roller was used to roll it evenly and slowly for 2 times. After standing for 6 hours, the initial adhesion (according to GB / T 4852-2002), the lasting adhesion (according to GB / T 4851-2014) and the 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that its initial adhesion is No. 1 ball, the lasting adhesion is 200h, and the peel strength is 18N / cm.
[0162] Comparative Example 1
[0163] The commercially available 3M Scotch tape uses polyacrylate polymers as adhesives, and adds various additives such as tackifiers and plasticizers, and is non-degradable.
[0164] The initial adhesion (according to GB / T 4852-2002), sustained adhesion (according to GB / T4851-2014) and 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that the initial adhesion is 6 ball, the sustained adhesion is 27h, and the peel strength is 3.5N / cm.
[0165] Figure 7180° peel strength curve of 3M Scotch tape in comparative example 1. According to the test curve results, the 180° peel strength of 3M Scotch tape is 3.5 N / cm, and the peel strength of the embodiment is better than that of the comparative example.
[0166] Comparative Example 2
[0167] The Japanese Nitto tape on the market has a peel strength of 3N / cm. It uses polyacrylate polymers as adhesives, and adds various additives such as tackifiers and plasticizers. It is non-degradable.
[0168] The initial adhesion (according to GB / T 4852-2002), sustained adhesion (according to GB / T4851-2014) and 180° peel strength (according to GB / T 2192-2014) were tested respectively. The test results show that the initial adhesion is 7 ball, the sustained adhesion is greater than 100h, and the peel strength is 3N / cm.
[0169] Figure 8 This is the 180° peel strength curve of the Japanese Nitto tape in Comparative Example 2. According to the test curve results, the 180° peel strength of the Nitto tape is 3.2 N / cm, and the peel strength of the embodiment is better than that of the comparative example.
[0170] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.
Claims
1. Application of a carbon dioxide-based terpolymer in the preparation of a pressure-sensitive adhesive; The carbon dioxide-based terpolymer has a structure shown in Formula I; In formula I, 5≤m≤5000, 5≤n≤5000; The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
2. The use according to claim 1, characterized in that: The R1 and R2 are independently selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, allyl or PEG groups.
3. The use according to claim 1, characterized in that: In the carbon dioxide-based terpolymer having the structure shown in formula I, the mass content of the carbonate unit is 85% to 99%, and the mass content of the ether segment is 1% to 15%.
4. The use according to claim 1, characterized in that: The carbon dioxide-based terpolymer having the structure shown in formula I is prepared by terpolymerization of carbon dioxide and epoxide; The epoxides include two of propylene oxide, 1,2-butylene oxide, 2,3-butylene oxide, cyclohexene oxide, 1,2-butylene oxide, 1,2-butylene oxide, 1,2-cyclopentene oxide, epichlorohydrin, glycidyl methacrylate (PEGMA), methyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, styrene oxide, 1,2-epoxy-4-vinylcyclohexane, 2-vinylethylene oxide and 2-[2-(2-methoxyethoxy)ethoxy]ethyl glycidyl ether.
5. The use according to claim 4, characterized in that: The main catalyst of the ternary copolymerization is a Salen-Co catalyst having a structure shown in Formula II; 6. The use according to claim 5, characterized in that: The co-catalyst for the ternary copolymerization is bis(triphenylphosphorane)ammonium trifluoroacetate (PPNTFA), having the structure shown in Formula III; 7. The use according to claim 6, characterized in that: The molar ratio of the co-catalyst to the main catalyst is 0 to 2:1; The molar ratio of the main catalyst to the epoxide is 1:1000-5000.
8. The use according to claim 4, characterized in that: The carbon dioxide pressure of the ternary copolymerization is 0 to 20 MPa, and is not zero.
9. The use according to claim 4, characterized in that: The temperature of the ternary copolymerization is 20-30° C., and the time is 6-72 hours.
10. A pressure-sensitive adhesive prepared from a carbon dioxide-based terpolymer; The carbon dioxide-based terpolymer has a structure shown in Formula I; In formula I, 5≤m≤5000, 5≤n≤5000; The R1 and R2 are independently selected from C1-C10 alkyl, C1-C10 alkoxy, C1-C10 substituted alkoxy; C1-C10 alkyl glycidyl ether, C1-C10 aryl glycidyl ether, C1-C10 cycloalkane or halogen.
Citation Information
Patent Citations
Method for preparing Wang resin supported chiral Salon-Co (III) catalyst
CN101905171A
Method for preparing polystyrene resin-immobilized Salon-Co (III) catalyst
CN101940947A
Preparation method of chiral Salen-Co(III) catalyst loaded by utilizing Merrifield resin
CN105618141A
Dual-function catalyst for preparing cyclic carbonates through cycloaddition of CO2 and epoxy compound and preparation method thereof
CN105665022A
Salen metal complex catalyst and preparation method thereof
CN114713287A