Organosilicon coolant containing phase change component and preparation method thereof

By using a combination of fluorinated end-group PDMS, PCM microcapsules, thermally conductive fillers and antibacterial agents in the cooling material, the problems of thermal stability, heat conduction efficiency and antibacterial performance in the thermal management of the cooling material are solved, achieving efficient and stable cooling. Effect.

CN118792016APending Publication Date: 2024-10-18NINGBO YINZHOU TEERFEI ELECTRONICS CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411069491.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing cooling materials have difficulties in accurately controlling the phase change temperature in thermal management, low thermal conductivity efficiency, poor material stability, and difficulty in meeting the high standards of long-term stability and antibacterial performance.

Method used

Using a combination of fluorine-containing end-group PDMS, PCM microcapsules, thermally conductive fillers, antibacterial agents and stabilizers, a highly efficient silicone coolant is formed through a specific preparation method to improve thermal stability, heat conduction efficiency, antibacterial performance and long-term stability.

Benefits of technology

It achieves efficient cooling in a wider temperature range, improves the thermal conductivity and mechanical stability of the coolant, provides long-lasting antibacterial protection, and ensures the long-term stability and compatibility of the coolant.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of coolants, and discloses an organosilicon coolant containing a phase change component, the coolant comprises the following components by mass: 55-65% of fluorine-containing terminal group PDMS, 15-35% of PCM microcapsule, 10-25% of a heat conduction filler, 0.5-3.0% of an antibacterial agent, and 0.5-5.0% of a stabilizer; wherein the fluorine-containing terminal group PDMS is prepared by carrying out a reaction on dihydroxyl-terminated PDMS and a fluorine-containing silane coupling agent under the action of a catalyst, and the viscosity of the dihydroxyl-terminated PDMS is about 50-100 cSt. The coolant disclosed by the invention has an efficient heat conduction network and excellent heat stability, the introduced fluorine-containing terminal group PDMS has better compatibility, the addition of the stabilizer further ensures the dispersion stability of each component in the coolant, the addition of the antibacterial agent provides long-acting antibacterial performance, and the sanitation and safety of the coolant are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coolants, in particular to an organic silicon coolant containing a phase change component and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology, the performance of electronic equipment continues to improve, resulting in a significant increase in the heat generated during operation. High temperature not only affects the stability and performance of the equipment, but may also cause premature aging or damage to the equipment. Therefore, efficient thermal management systems have become a key technical requirement in many industries, including the electronics manufacturing industry, precision instrumentation, and even building temperature control.

[0003] Traditional cooling methods, such as fan cooling and water cooling systems, can solve the heat dissipation problem to a certain extent, but they have limitations such as high noise, high energy consumption, and complex maintenance. In recent years, phase change materials (PCMs) have been widely studied because they can provide large heat capacity during heat absorption and heat release, especially in passive thermal management systems. However, PCMs also have some problems in practical applications, such as the difficulty in accurately controlling the phase change temperature, low heat conduction efficiency, and poor material stability.

[0004] In addition, as the complexity of the application environment increases, cooling materials also need to consider factors such as long-term stability, antibacterial properties, and environmental friendliness. Existing cooling materials often find it difficult to fully meet these high standards.

[0005] A Chinese invention patent (publication number: CN117534931A, publication date: 2024.02.09) discloses a triple network cooling hydrogel with high compressibility and elasticity, which contains about 4-8% w / w polyvinyl alcohol (PVA), about 4-8% w / w polydimethylsiloxane (PDMS), about 15-25% w / w phase change material (PCM), about 55-68% w / w water, and about 0.5-2.5% w / w cross-linking agent. The PDMS used in the invention is an unmodified product with relatively poor thermal stability and compatibility, and the long-term stability and antibacterial properties of the hydrogel are not taken into account. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention provides an organic silicon coolant containing a phase change component and a preparation method thereof.

[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions: A silicone coolant containing a phase change component, wherein the coolant is composed of the following components by mass percentage: Fluorinated end group PDMS: 55-65%, PCM microcapsules: 15-35%, Thermal conductive filler: 10-25%, Antimicrobial agent: 0.5-3.0%, Stabilizer: 0.5-5.0%; The fluorine-terminated PDMS is prepared by reacting dihydroxy-terminated PDMS and a fluorine-containing silane coupling agent under the action of a catalyst, and the viscosity of the dihydroxy-terminated PDMS is about 50-100 cSt.

[0008] Preferably, the coolant is composed of the following components by mass percentage: Fluorinated end group PDMS: 60-65%, PCM microcapsules: 20-25%, Thermal conductive filler: 15-20%, Antimicrobial agent: 2-2.5%, Stabilizer: 3-3.5%.

[0009] Preferably, the thermally conductive filler is thermally conductive nanoparticles, including but not limited to nano-aluminum oxide, boron nitride nanosheets, and graphene; The antimicrobial agent includes but is not limited to silver nanoparticles, zinc oxide nanoparticles, phenoxyethanol, and isothiazolinone compounds; The stabilizer includes, but is not limited to, polyethylene glycol derivatives, polyoxyethylene surfactants, polyethylene glycol-400, methoxy polyethylene glycol silane coupling agent, Tween 80, and Tween 20.

[0010] Preferably, the preparation method of the fluorine-terminated PDMS comprises the following specific steps: 1) Pretreatment: Dissolve the dihydroxy-terminated PDMS in anhydrous tetrahydrofuran under dry conditions, with the mass volume ratio of dihydroxy-terminated PDMS to anhydrous tetrahydrofuran being 1:5 (g:mL), ensuring complete dissolution to form a uniform solution A; 2) Add fluorinated silane coupling agent: slowly add fluorinated silane coupling agent to solution A, the mass ratio of fluorinated silane coupling agent to dihydroxy-terminated PDMS is 1:5, and stir to ensure sufficient mixing; 3) Catalytic reaction: Add an appropriate amount of catalyst to the reaction system and stir the reaction at room temperature for 24-48 hours; 4) Reaction monitoring: The reaction process can be monitored by infrared spectroscopy; 5) Post-treatment: After the reaction is completed, tetrahydrofuran and unreacted low-boiling substances are first removed by rotary evaporation, then washed with an organic solvent, and finally vacuum dried to obtain purified fluorine-terminated PDMS.

[0011] Preferably, in the above-mentioned method for preparing fluorine-terminated PDMS, the fluorine-containing silane coupling agent includes but is not limited to 3,3,3-trifluoropropyltrimethoxysilane and heptadecafluorodecyltrimethoxysilane; the catalyst is a platinum catalyst, such as a Custer catalyst; and the organic solvent includes but is not limited to petroleum ether.

[0012] Preferably, the phase change material of the PCM microcapsule is paraffin or fatty acid, and the capsule wall is a polyurethane shell layer. Paraffin or fatty acid has a phase change temperature of about 25°C-28°C and is used as a heat storage medium.

[0013] Preferably, the preparation method of the PCM microcapsules comprises the following specific steps: 1) Pretreatment and emulsification: Heat the paraffin or fatty acid to 5℃-10℃ above its melting point to keep it in a fluid state, and heat the solvent to the same temperature; Dissolve the emulsifier in hot paraffin or fatty acid, and stir with a high-speed stirrer at 60°C for about 5 minutes to form a paraffin or fatty acid oil phase; Add the oil phase dropwise into the solvent preheated to the same temperature, and continue stirring at high speed for about 15 minutes to form a stable water-in-oil emulsion; 2) Formation of polymer shell: pre-mix polyisocyanate and polyether polyol, drop them into the emulsion, add a small amount of catalyst, and continue stirring at 60°C for 2-6 hours until the polymerization reaction is completed to form a solid polyurethane shell; wherein the mass ratio of polyisocyanate to polyether polyol is 1:1, and the mass ratio of polyisocyanate to polyether polyol to paraffin or fatty acid is 2:5; 3) Post-treatment: Cool down to room temperature, let stand to allow PCM microcapsules to settle, wash PCM microcapsules with deionized water to remove unreacted raw materials and by-products, collect PCM microcapsules by filtration or centrifugation, and then air-dry at room temperature or vacuum-dry at low temperature to obtain dry PCM microcapsules.

[0014] Preferably, the solvent is deionized water; the emulsifier is sorbitan monostearate; and the catalyst is dimethyl diacetamide.

[0015] Furthermore, the present invention also discloses a method for preparing a coolant, and the specific steps are as follows: 1) Dissolution of fluorinated terminal PDMS: dissolve the fluorinated terminal PDMS in a suitable organic solvent to form a uniform PDMS solution; 2) Dispersion of thermal conductive filler: Mix the thermal conductive nanoparticles with the stabilizer, and mix them evenly by high shear stirring at a speed of 1000-3000 rpm for 15-60 minutes; Add the mixture A to the PDMS solution, and perform ultrasonic treatment at 35°C to ensure that the thermal conductive nanoparticles are evenly dispersed, with an ultrasonic frequency of 20 kHz-40kHz, an ultrasonic power of 100-600W, and a treatment time of 5-30 minutes; 3) PCM microcapsule mixing: Add PCM microcapsules directly into the solution obtained in step (2) and stir to ensure uniform mixing; 4) Antimicrobial agent addition: slowly add the antimicrobial agent and stir to ensure that the antimicrobial agent is evenly distributed; 5) Post-treatment: remove the organic solvent by rotary evaporation to obtain the organosilicon coolant.

[0016] Preferably, the organic solvent includes but is not limited to anhydrous tetrahydrofuran and cyclohexane.

[0017] The coolant of the present invention can be applied to a variety of scenarios, such as heat dissipation of electronic equipment, thermal management of electric vehicle batteries, solar thermal energy storage, building temperature control, cooling of medical equipment, etc.

[0018] The formula design principle of the present invention: 1) Fluorinated end group PDMS: The introduction of fluorinated end groups can improve the thermal stability of PDMS and reduce its surface energy. This not only improves the durability of PDMS in high temperature applications, allowing the coolant to be used in a wider temperature range, but also helps to improve the compatibility with other components, especially with PCM microcapsules and thermal conductive fillers.

[0019] 2) PCM microcapsules: paraffin or fatty acids are selected as the phase change core and coated with an outer layer of polyurethane to improve the thermal responsiveness and mechanical stability of the coolant. Microencapsulation technology ensures effective encapsulation of the phase change material, avoids material leakage during the phase change process, and provides additional mechanical protection.

[0020] 3) Thermally conductive fillers: By mixing thermally conductive nanoparticles such as nano-alumina, boron nitride nanosheets and graphene, an efficient heat conduction network is formed. This design helps promote the rapid distribution and transfer of heat in the coolant, improve the heat dissipation efficiency of the coolant, and improve the overall thermal management performance.

[0021] 4) Antimicrobial agent: The use of antimicrobial agent is intended to provide long-term antimicrobial protection for coolants, prevent the growth and reproduction of microorganisms, reduce performance degradation and shortened service life caused by microbial contamination, and ensure the hygiene and safety of the coolant system.

[0022] 5. Ensure long-term application stability 5) Stabilizer: It helps to maintain the uniform and stable dispersion of other components in the coolant, avoids stratification, precipitation or phase separation, and maintains the long-term stability and compatibility of the coolant, which is essential for maintaining the performance of the coolant and extending its service life.

[0023] The beneficial effects of the present invention are as follows: the present invention adopts fluorine-terminated PDMS, which has better thermal stability and lower surface energy, and can not only improve the durability of the coolant in high-temperature applications, so that the coolant can be used in a wider temperature range, but also improve the compatibility of PDMS with other components, that is, the dispersion stability of PCM microcapsules and thermally conductive fillers in PDMS is improved, and precipitation in the coolant is avoided; the introduction of thermally conductive fillers can significantly improve the thermal conductivity of the coolant, and synergize with the fluorine-terminated PDMS to form an efficient heat conduction network; PCM microcapsules provide dynamic thermal regulation capabilities; the addition of antibacterial agents provides long-lasting antibacterial properties, ensuring the hygiene and safety of the coolant; the stabilizer ensures the uniform and stable dispersion of each component, avoids stratification, precipitation or phase separation, and maintains long-term stability and compatibility. DETAILED DESCRIPTION

[0024] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1 Provided is a fluorine-terminated PDMS, wherein the basic raw material ratio for the preparation is as follows: 10 g of dihydroxy-terminated PDMS (viscosity of about 50-10 cSt), 2 g of a fluorine-containing silane coupling agent (3,3,3-trifluoropropyltrimethoxysilane), 50 mL of anhydrous tetrahydrofuran, and 0.1 mL of a catalyst (platinum catalyst, a solution containing 2% platinum).

[0026] The fluorine-terminated PDMS is prepared by the method of the present invention, and the specific steps are as follows: 1) Pretreatment: Dissolve the dihydroxy-terminated PDMS in anhydrous tetrahydrofuran under dry conditions to ensure complete dissolution to form a uniform solution A; 2) Add fluorinated silane coupling agent: slowly add fluorinated silane coupling agent to solution A, the mass ratio of fluorinated silane coupling agent to dihydroxy-terminated PDMS is 1:5, and stir to ensure sufficient mixing; 3) Catalytic reaction: Add an appropriate amount of catalyst to the reaction system and stir the reaction at room temperature for 24-48 hours; 4) Reaction monitoring: The reaction process can be monitored by infrared spectroscopy; 5) Post-treatment: After the reaction is completed, tetrahydrofuran and unreacted low-boiling substances are first removed by rotary evaporation, then washed with an organic solvent, and finally vacuum dried to obtain purified fluorine-terminated PDMS.

[0027] Comparative Example 1 Supplied unmodified PDMS.

[0028] Experiment 1: Thermal stability test of PDMS of Example 1 and Comparative Example 1 Test method: Use thermogravimetric analysis (TGA) to measure the mass change of the two PDMS during the heating process from room temperature to 600°C. Set the heating rate to 10°C / min, and record the relationship between the mass loss and temperature of each sample. The two PDMS have the same initial mass. Finally, compare the thermal decomposition start temperature (°C) and 50% mass loss temperature of the two. The results are shown in Table 1.

[0029] Table 1 Material Thermal decomposition starting temperature (℃) 50% mass loss temperature (℃) Unmodified PDMS 320 380 Fluorinated PDMS 350 420 The fluorine-terminated PDMS exhibited a higher thermal decomposition onset temperature and a higher 50% mass loss temperature than the unmodified PDMS, indicating that the fluorine-terminated PDMS improved the thermal stability.

[0030] Experiment 2: Water contact angle measurement of PDMS of Example 1 and Comparative Example 1 Test method: The water contact angle of the two PDMS was measured by contact angle measurement. At least 5 different positions of each material were measured and the average value was taken to reduce the error. The results are shown in Table 2.

[0031] Table 2 Material Water contact angle (°) Unmodified PDMS 108 Fluorinated PDMS 118 The water contact angle of fluorine-terminated PDMS is larger than that of unmodified PDMS, which indicates that the surface of fluorine-terminated PDMS is more hydrophobic and has lower surface energy.

[0032] Experiment 3: Compatibility test of PDMS and phase change materials in Example 1 and Comparative Example 1 Test method: PCM microcapsules were mixed with two types of PDMS respectively. The mixing ratio of the two PDMS and PCM microcapsules was the same. The dispersion state was observed using an optical microscope. The phase change properties were analyzed by differential scanning calorimetry (DSC). The results are shown in Table 3.

[0033] Table 3 Material Phase transition starting temperature (℃) Phase change enthalpy (J / g) Dispersed state Unmodified PDMS mixture 22 180 PCM microcapsules are not evenly dispersed and aggregated in some areas Fluorinated PDMS mixture 22 182 PCM microcapsules are evenly dispersed and no obvious aggregation is observed The phase transition onset temperatures of the two mixtures are the same, indicating that the phase transition characteristics of PCM are not affected by PDMS modification. The phase transition enthalpy of the fluorinated end group PDMS mixture is slightly higher, indicating that its compatibility with PCM may be better, which is conducive to the thermal energy conversion efficiency of the PCM phase transition process.

[0034] Embodiment 2-7 Provided is a silicone coolant containing a phase change component, the formula of which is shown in Table 4, wherein the thermal conductive filler is nano-alumina, the antibacterial agent is silver nanoparticles, and the stabilizer is Tween 80 and polyethylene glycol-400, and the ratio of Tween 80:polyethylene glycol-400 is 1:1.

[0035] The fluorine-terminated PDMS adopts the finished product prepared in Example 1.

[0036] The coolant is prepared by the method of the present invention, and the specific steps are as follows: 1) Dissolution of fluorinated terminal PDMS: Dissolve the fluorinated terminal PDMS in appropriate anhydrous tetrahydrofuran to form a uniform PDMS solution; 2) Dispersion of thermal conductive filler: Mix the thermal conductive filler with the stabilizer, and mix them evenly by high shear stirring at a speed of 1000-3000 rpm for 15-60 minutes; Add mixture A to the PDMS solution, and perform ultrasonic treatment at 35°C to ensure that the thermal conductive nanoparticles are evenly dispersed, with an ultrasonic frequency of 20 kHz-40kHz, an ultrasonic power of 100-600 W, and a treatment time of 5-30 minutes; 3) PCM microcapsule mixing: Add PCM microcapsules directly into the solution obtained in step (2) and stir to ensure uniform mixing; 4) Antimicrobial agent addition: slowly add the antimicrobial agent and stir to ensure that the antimicrobial agent is evenly distributed; 5) Post-treatment: remove anhydrous tetrahydrofuran by rotary evaporation to obtain the organosilicon coolant.

[0037] The PCM microcapsules are prepared by the method of the present invention, and the specific steps are as follows: 1) Pretreatment and emulsification: Heat the paraffin to 5℃-10℃ above its melting point to keep it in a fluid state, and heat the solvent to the same temperature; the phase transition temperature of paraffin is about 25℃-28℃; Dissolve sorbitan monostearate in hot paraffin wax and stir at 60°C for about 5 minutes using a high-speed stirrer to form a paraffin oil phase; Add the oil phase dropwise into deionized water preheated to the same temperature, and continue stirring at high speed for about 15 minutes to form a stable water-in-oil emulsion; 2) Formation of polymer shell: pre-mix polyisocyanate and polyether polyol, add dropwise to the emulsion, add a small amount of dimethyl diacetamide, and continue stirring at 60°C for 2-6 hours until the polymerization reaction is completed to form a solid polyurethane shell; wherein the mass ratio of polyisocyanate to polyether polyol is 1:1, and the mass ratio of the sum of the mass of polyisocyanate and polyether polyol to paraffin is 2:5; 3) Post-treatment: Cool down to room temperature, let stand to allow PCM microcapsules to settle, wash PCM microcapsules with deionized water to remove unreacted raw materials and by-products, collect PCM microcapsules by filtration or centrifugation, and then air-dry at room temperature or vacuum-dry at low temperature to obtain dry PCM microcapsules.

[0038] The basic raw material ratio of the PCM microcapsules is as follows: 10 g paraffin, 2 g polyisocyanate, 2 g polyether polyol, 0.5 g sorbitan monostearate, 100 mL deionized water, and an appropriate amount of dimethyl diacetamide.

[0039] The formula of Comparative Example 2-4 is shown in Table 4, which is adjusted on the basis of Example 2, and the preparation method is the same as Example 2.

[0040] The reference formula is shown in Table 4, and the preparation method can be appropriately adjusted based on Example 2.

[0041] Evaluation tests were performed on Examples 2-7, Comparative Examples 2-4 and Reference Examples.

[0042] Test Method Thermal conductivity test: Use the heat flow meter method to measure the thermal conductivity of the coolant and evaluate its heat dissipation performance.

[0043] Thermal Stability Analysis: The thermal stability and phase change characteristics of the coolant were evaluated by thermogravimetric analysis (TGA).

[0044] Antibacterial performance test: The plate count method was used to evaluate the antibacterial effect of the coolant.

[0045] Dispersion stability test: Evaluate the dispersion stability of each component in the coolant through long-term static test.

[0046] Table 4 Reference ratio Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example 2 Comparative Example 3 Comparative Example 4 Fluorinated PDMS / 60% 55% 65% 55% 60% 61% / 60% 64% Unmodified PDMS 80% / / / / / / 60% / / PCM microcapsules / 20% 30% 20% 15% 20% 20% 20% 20% 20% PCM 20% / / / / / / / / / Thermally conductive fillers / 15% 10% 10% 25% 15% 15% 15% / 15% Antimicrobial agents / 2% 2% 2% 2% 1% 3% 2% 2% 0.2% Stabilizer / 3% 3% 3% 3% 4% 1% 3% 3% 0.3% Thermal conductivity (W / m·K) 0.2 0.8 0.6 0.75 0.9 0.8 0.8 0.75 0.3 0.8 Thermal stability (decomposition temperature °C) 250 >300 >300 >300 >300 >300 >300 245 >300 >300 Antibacterial effect (reduction in colony count %) - >99% >99% >99% >99% >99% >99% >99% >99% - Dispersion stability Precipitation Excellent Excellent Excellent Excellent Excellent good Slight precipitation Excellent Precipitation Referring to Table 4, it can be seen from Example 2 and Comparative Example 2 that the fluorine-terminated PDMS not only improves the overall thermal stability of the coolant, allowing the coolant to be used in a wider temperature range, which is particularly important for applications that require stable operation at high temperatures (such as heat dissipation of electronic equipment), but also has better compatibility and maintains the stability of chemical and physical properties; it can be seen from Examples 2-5 and Comparative Examples 2 and 3 that the synergistic effect of the fluorine-terminated PDMS and the thermally conductive filler forms an effective heat conduction network; it can be seen from the reference example, Example 2 and Comparative Example 4 that the appropriate addition of an antibacterial agent can significantly reduce the number of colonies, and the appropriate addition of a stabilizer can ensure the long-term stable dispersion of the thermally conductive filler and the microencapsulated PCM.

[0047] The above is a description of the embodiments of the present invention. Through the above description of the disclosed embodiments, professionals and technicians in the field can implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will conform to the widest range consistent with the principles and novelties disclosed herein.

Claims

1. An organosilicon coolant containing a phase change component, characterized in that: The coolant is composed of the following components by mass percentage: Fluorinated end group PDMS: 55-65%, PCM microcapsules: 15-35%, Thermal conductive filler: 10-25%, Antimicrobial agent: 0.5-3.0%, Stabilizer: 0.5-5.0%; The fluorine-terminated PDMS is prepared by reacting dihydroxy-terminated PDMS and a fluorine-containing silane coupling agent under the action of a catalyst.

2. The coolant according to claim 1, characterized in that The coolant is composed of the following components by mass percentage: Fluorinated end group PDMS: 60-65%, PCM microcapsules: 20-25%, Thermal conductive filler: 15-20%, Antimicrobial agent: 2-2.5%, Stabilizer: 3-3.5%.

3. The coolant according to claim 1 or 2, characterized in that: The thermally conductive filler is thermally conductive nanoparticles, including but not limited to nano-aluminum oxide, boron nitride nanosheets, and graphene; The antimicrobial agent includes but is not limited to silver nanoparticles, zinc oxide nanoparticles, phenoxyethanol, and isothiazolinone compounds; The stabilizer includes, but is not limited to, polyethylene glycol derivatives, polyoxyethylene surfactants, polyethylene glycol-400, methoxy polyethylene glycol silane coupling agent, Tween 80, and Tween 20.

4. The coolant according to claim 1, 2 or 3, characterized in that: The specific steps of the preparation method of the fluorine-terminated PDMS are as follows: 1) Pretreatment: Dissolve the dihydroxy-terminated PDMS in anhydrous tetrahydrofuran under dry conditions, with the mass volume ratio of dihydroxy-terminated PDMS to anhydrous tetrahydrofuran being 1:5 (g:mL), ensuring complete dissolution to form a uniform solution A; 2) Add fluorinated silane coupling agent: slowly add fluorinated silane coupling agent to solution A, the mass ratio of fluorinated silane coupling agent to dihydroxy-terminated PDMS is 1:5, and stir to ensure sufficient mixing; 3) Catalytic reaction: Add an appropriate amount of catalyst to the reaction system and stir the reaction at room temperature for 24-48 hours; 4) Reaction monitoring: The reaction process can be monitored by infrared spectroscopy; 5) Post-treatment: After the reaction is completed, tetrahydrofuran and unreacted low-boiling substances are first removed by rotary evaporation, then washed with an organic solvent, and finally vacuum dried to obtain purified fluorine-terminated PDMS.

5. The coolant according to claim 4, characterized in that The fluorine-containing silane coupling agent includes but is not limited to 3,3,3-trifluoropropyltrimethoxysilane and heptadecafluorodecyltrimethoxysilane; the catalyst is a platinum catalyst; and the organic solvent includes but is not limited to petroleum ether.

6. The coolant according to claim 1, characterized in that The phase change material of the PCM microcapsule is paraffin or fatty acid, and the capsule wall is a polyurethane shell layer.

7. The coolant according to claim 6, characterized in that The specific steps of the preparation method of the PCM microcapsules are as follows: 1) Pretreatment and emulsification: Heat the paraffin or fatty acid to 5℃-10℃ above its melting point to keep it in a fluid state, and heat the solvent to the same temperature; Dissolve the emulsifier in hot paraffin or fatty acid, and stir with a high-speed stirrer at 60°C for about 5 minutes to form a paraffin or fatty acid oil phase; Add the oil phase dropwise into the solvent preheated to the same temperature, and continue stirring at high speed for about 15 minutes to form a stable water-in-oil emulsion; 2) Formation of polymer shell: pre-mix polyisocyanate and polyether polyol, drop them into the emulsion, add a small amount of catalyst, and continue stirring at 60°C for 2-6 hours until the polymerization reaction is completed to form a solid polyurethane shell; wherein the mass ratio of polyisocyanate to polyether polyol is 1:1, and the mass ratio of polyisocyanate to polyether polyol to paraffin or fatty acid is 2:5; 3) Post-treatment: Cool down to room temperature, let stand to allow PCM microcapsules to settle, wash PCM microcapsules with deionized water to remove unreacted raw materials and by-products, collect PCM microcapsules by filtration or centrifugation, and then air-dry at room temperature or vacuum-dry at low temperature to obtain dry PCM microcapsules.

8. The coolant according to claim 7, characterized in that The solvent is deionized water; the emulsifier is sorbitol monostearate; and the catalyst is dimethyl diacetamide.

9. The method for preparing a coolant according to any one of claims 1 to 8, characterized in that: The specific steps are as follows: 1) Dissolution of fluorinated terminal PDMS: dissolve the fluorinated terminal PDMS in a suitable organic solvent to form a uniform PDMS solution; 2) Dispersion of thermal conductive filler: Mix the thermal conductive nanoparticles with the stabilizer, and mix them evenly by high shear stirring at a speed of 1000-3000 rpm for 15-60 minutes; Add the mixture A to the PDMS solution, and perform ultrasonic treatment at 35°C to ensure that the thermal conductive nanoparticles are evenly dispersed, with an ultrasonic frequency of 20 kHz-40kHz, an ultrasonic power of 100-600W, and a treatment time of 5-30 minutes; 3) PCM microcapsule mixing: Add PCM microcapsules directly into the solution obtained in step (2) and stir to ensure uniform mixing; 4) Antimicrobial agent addition: slowly add the antimicrobial agent and stir to ensure that the antimicrobial agent is evenly distributed; 5) Post-treatment: Rotary evaporation is used to remove the organic solvent to obtain the organosilicon coolant.

10. The preparation method according to claim 9, characterized in that: The organic solvent includes but is not limited to anhydrous tetrahydrofuran and cyclohexane.

Citation Information

Cited By

  • Cooling medium and preparation method thereof

    CN119639429A

  • Liquid cooling medium and preparation method thereof

    CN119684977A

  • Cooling liquid for immersed liquid-cooled battery and preparation method of cooling liquid

    CN120248846A

  • Insulating coolant and immersed cooling liquid

    CN121449898A