Conductive layer sheet structure and preparation method and application thereof

By using a parallelogram grid structure conductive network layer and a damping rubber layer composed of nanometal wires in the flexible conductor, the problem of conductivity decrease under large stretching of the flexible conductor is solved, and high conductivity and high stretch rate are achieved. Taking both into account and improving the reliability of the connection between the voice coil and the electrode.

CN118800501APending Publication Date: 2024-10-18SUZHOU ANTENG NANO TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027040.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The conductivity of existing flexible conductors decreases under large stretching, making it difficult to balance high stretch rate and high conductivity, and the conductive network is prone to disconnection under deformation.

Method used

A conductive network layer with a parallelogram grid structure composed of nanometal wires is used, and a nearly rectangular parallelogram network structure is formed by arranging a first conductor group and a second conductor group that intersect between two layers of flexible substrates, and the conductor spacing is The width is optimized, combined with a damping adhesive layer to improve bonding force and elasticity, and the nanometal wire orientation is consistent with the wire extension direction to reduce resistance.

Benefits of technology

It achieves high conductivity and high stretch rate of the conductive layer under large stretching, and has a low impedance change rate. It is suitable for scenarios requiring large deformation applications and improves the reliability of the connection between the voice coil and the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800501A_ABST
    Figure CN118800501A_ABST
Patent Text Reader

Abstract

The invention discloses a conductive layer sheet structure and a preparation method and application thereof. The conductive layer sheet structure comprises a first base material layer, a conductive net layer and a second base material layer which are sequentially arranged in a stacked mode. The conductive net layer comprises a first wire group and a second wire group which are arranged in a crossed manner at a preset angle, each of the first wire group and the second wire group comprises a plurality of wires which are arranged in parallel at intervals, and the wires comprise nano metal wires. The preparation method of the conductive layer sheet structure comprises the following steps: preparing a first wire group and a second wire group on the first substrate layer along a preset direction, or preparing the first wire group on the first substrate layer along a first preset direction, and preparing the second wire group on the second substrate layer along a second preset direction; then the first base material layer and the second base material layer are attached, the face where the wire set is located faces inwards, and the conducting layer sheet structure is obtained through compounding. The conductive layer sheet structure can give consideration to high conductivity and elasticity, can maintain high conductivity under the action of stress, and can be used as a vibrating diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of conductor materials, and in particular to a conductive layer structure and a preparation method and application thereof. Background Art

[0002] Flexible conductors are a type of conductor that can maintain conductivity under the action of bending, folding, stretching, etc., and are widely used in stretchable electronic products such as flexible sensors, wearable devices, and flexible displays. Although the current mainstream flexible conductive materials have good performance in flexibility and conductivity, they all have obvious defects in elastic strain limit. When the material is stretched and the stress reaches a certain value, the material will not return to its original state after the stress is removed. The strain corresponding to this stress value is called the elastic strain limit. The elastic strain limit of general metal materials is less than 0.5%. Although the conductive polymer PEDOT can obtain a better elastic strain limit by adding plasticizers and mixing with other polymers, it will cause its resistivity to increase further. Conductive metal slurry relies on its polymer matrix to disperse and fix metal particles. Once it is stretched, its resistivity will rise rapidly. According to experiments, although the bending fatigue performance of flexible metal slurry is excellent, its elastic strain limit is only less than 1%.

[0003] In order to improve the stretchability of flexible monomers, conductive materials are usually mixed with prepolymers of elastic polymers and molded to prepare stretchable conductors. The conductivity and elongation of the conductors are related to the amount of conductive materials added. When the amount is low, the elongation is high but the conductivity is poor. When the amount is high, the conductivity of the conductor is improved, but the elongation is greatly reduced. Therefore, it is difficult to take into account the stretchability and conductivity of the conductor. The conductivity of the conductor will significantly decrease with the increase of the stretching length, which greatly limits the application field of this type of flexible conductor. Although the flexible conductor prepared by preparing a nanometal wire network layer on the surface of the elastic matrix can improve the conductivity of the flexible conductor to a certain extent, the arrangement of the nanometal wires in the nanometal wire network layer is currently mostly disordered, and some overlap points will be disconnected as the flexible conductor is stretched, which cannot effectively improve the conductivity of the flexible conductor under large deformation.

[0004] Based on this, there is an urgent need for a flexible conductor that can maintain high conductivity under large stretching to meet applications that require large deformation. Summary of the invention

[0005] To solve the above problems, the present invention provides a conductive layer sheet structure and a preparation method and application thereof, wherein a conductive mesh layer composed of nanometal wires and having a parallelogram grid structure is arranged between two flexible substrates. The conductive mesh layer having such a structure is highly deformable and is conducive to stress dispersion. Under the synergistic effect of the upper and lower flexible substrates, it not only has a high stretch rate, but also a low rate of change of impedance with increasing stretch rate.

[0006] Specifically, the following technical solutions are provided:

[0007] A first aspect of the present invention provides a conductive layer structure, comprising a first substrate layer, a conductive mesh layer and a second substrate layer stacked in sequence;

[0008] The conductive mesh layer includes a first conductive line group and a second conductive line group that are cross-arranged. The first conductive line group and the second conductive line group both include a plurality of conductive lines that are parallel and spaced apart. The conductive lines include nano metal wires.

[0009] Furthermore, the materials of the first substrate layer and the second substrate layer are the same or different, and can be selected from one or more of polyethylene terephthalate, polyethylene naphthalate, polymethyl methacrylate, polyimide, polyamide, polyurethane, polyarylate, polyphenylene sulfide, polysulfone, polyether sulfone, polyphenylene sulfide sulfone, rubber, silicone resin, polyether ether ketone, polycarbonate, polypropylene, and polydimethylsiloxane, respectively. The above-mentioned rubber includes but is not limited to natural rubber, silicone rubber, etc.; the thickness of the first substrate layer and the second substrate layer is preferably 1-30μm, for example, 10μm, 15μm, 20μm, 25μm, 30μm, etc., including but not limited to the thickness values ​​listed above.

[0010] Further, the angle between the first wire group and the second wire group is preferably 80°-100°, such as 80°, 85°, 90°, 95°, 100°, etc., including but not limited to the angles listed above, and the first wire group and the second wire group form a conductive mesh layer with a nearly rectangular parallelogram network structure. More preferably, the angle between the first wire group or the second wire group and the predetermined stretching direction of the conductive layer structure is preferably 40°-50°, such as 45°. When the conductive layer is stretched, in the predetermined stretching direction, the angle between the first wire group and the second wire group varies widely. Within this wider range, the conductive network will be in a new equilibrium state, so that the formed conductive mesh layer has a high stretch rate along the predetermined stretching direction while maintaining high conductivity. The predetermined stretching direction is defined as the direction in which the conductive layer structure is subjected to the maximum external force / the maximum deformation.

[0011] Further, in the first wire group and / or the second wire group, the spacing between adjacent parallel wires is preferably 1-500μm, for example, 1-10μm, 10-50μm, 50-100μm, 100-200μm, 200-500μm or any value within the above range; more preferably, the wires in the first wire group and the second wire group are equally spaced and parallel, and the spacing between adjacent parallel wires in the first wire group is equal to the spacing between adjacent parallel wires in the second wire group, and the conductive mesh layer formed by the first wire group and the second wire group has a diamond grid structure, so that the prepared conductive layer has excellent stretchability in the above-mentioned predetermined stretching direction and in a direction perpendicular to the predetermined stretching direction.

[0012] Furthermore, the width of the wire is 1-500μm, for example, 1-50μm, 50-100μm, 100-200μm, 200-500μm or any value within the above range. The wire width will affect the elasticity and resistivity of the conductive layer structure. The wider the width, the lower the resistivity but the elasticity will decrease. Conversely, the resistivity increases. In order to make the conductive layer structure have both low resistance and good elasticity, preferably, the width of the wire is controlled in the range of 1-500μm.

[0013] Furthermore, the orientation of the nanometal wires in the conductor is consistent with the direction in which the conductor extends, thereby increasing the effective overlap between the first conductor group and the second conductor group during the stretching process and reducing the stretching resistance.

[0014] Furthermore, the nanometal wire comprises one or more of nanosilver wire, nanogold wire, nanocopper wire, and nanosilver-clad copper wire; preferably, the nanometal wire has a length of 20-80 μm and a diameter of 20-100 nm, and more preferably has a length of 45-65 μm and a diameter of 55-65 nm; in order to reduce the resistance change rate of the conductive mesh layer during stretching, a nanometal wire with a length-to-diameter ratio is used to prepare the conductive mesh layer, but the length of the nanometal wire cannot be too long. Too long nanometal wires are prone to agglomeration and are difficult to effectively orient and arrange, which in turn affects the resistance stability of the conductive layer structure under stretching.

[0015] Furthermore, the thickness of the conductive mesh layer is 100nm-10μm, more preferably 500nm-1μm; the thickness of the conductive mesh layer will affect its rigidity and conductivity. If the thickness is too thick, the rigidity of the conductive mesh layer will increase and the elongation at break will decrease, which is not conducive to the tensile performance and the cost will increase; but the thickness of the conductive mesh layer cannot be too thin. If the conductive mesh layer is too thin, its impedance will be difficult to meet the requirements; therefore, the thickness of the conductive mesh layer in the conductive layer sheet structure needs to be controlled within a suitable range, such as any value between 100nm-10μm.

[0016] Furthermore, the conductive layer structure also includes a damping rubber layer; the damping rubber layer is arranged in the grid of the conductive mesh layer to improve the bonding force between the substrate layer and the conductive mesh layer or the bonding force between the two substrate layers; the damping rubber is a low-stress rubber, which is more flexible after molding. This type of low-stress rubber can be selected from one or more of saw blade damping rubber, instantaneous damping rubber, two-component epoxy damping elastic potting rubber, epoxy damping potting rubber, and flame retardant damping insulating rubber; preferably, the thickness of the damping rubber layer is 100nm-10μm.

[0017] The second aspect of the present invention provides a method for preparing the conductive layer structure according to the first aspect, comprising the following method:

[0018] Method 1:

[0019] Forming a plurality of conductive lines in parallel and at intervals along a first preset direction and a second preset direction on the first substrate layer to form a conductive mesh layer;

[0020] The prepolymer of the second substrate layer is coated on the conductive mesh layer of the first substrate layer, and cured to obtain the conductive layer sheet structure; or, the first substrate layer including the conductive mesh layer is laminated with the second substrate layer, wherein the conductive mesh layer of the first substrate layer faces inward, and the conductive layer sheet structure is obtained by laminating;

[0021] Method 2:

[0022] Forming a plurality of conductive wires in parallel and at intervals along a first preset direction on the first substrate layer to form a first conductive wire group; and forming a plurality of conductive wires in parallel and at intervals along a second preset direction on the second substrate layer to form a second conductive wire group;

[0023] The first substrate layer including the first conductive wire group and the second substrate layer including the second conductive wire group are laminated together, wherein the surfaces where the first conductive wire group and the second conductive wire group are located face inwards, to obtain the conductive layer structure.

[0024] Furthermore, in method one and method two, before forming the wire, the surface of the first substrate layer and / or the second substrate layer is subjected to surface treatment, and the surface includes one or more of corona treatment, polylysine modification, flame treatment, and plasma treatment to improve the interface bonding strength between the substrate layer and the wire.

[0025] Furthermore, in method 1: the molding step includes: coating the nanometal wire dispersion on the first substrate layer by one or more combinations of a pulling method, a wire rod coating method, a capillary assisted jet method, and a screen printing method, and curing to obtain the conductive mesh layer;

[0026] In method 2: the forming step includes: coating the nanometal wire dispersion on the first substrate layer and the second substrate layer by one or more combinations of the pulling method, the wire rod coating method, the capillary assisted jet method, and the screen printing method, and curing to obtain the first wire group and the second wire group. Preferably, the nanometal wire dispersion is coated by one or more combinations of the pulling method, the wire rod coating method, and the capillary assisted jet method.

[0027] By coating the nanometal wire dispersion by the pulling method, the wire rod coating method, and the capillary assisted jet method, the nanometal wires can be oriented in the same direction as the extension direction of the wires, thereby reducing the lap resistance between the first wire group and the second wire group, and improving the stability of the conductivity of the conductive mesh layer under the action of stretching. For example, the capillary assisted jet method can be used to prepare a wire with regularly arranged nanometal wires. When the nanometal wire dispersion flows through the capillary, the nanometal wires are self-assembled in the capillary along the capillary direction.

[0028] Furthermore, the mass proportion of the nanometal wires in the nanometal wire dispersion is preferably 0.5%-2%, more preferably 1%-1.5%. If the mass proportion of the nanometal wires in the nanometal wire dispersion is too high, agglomeration will occur easily, while if it is too low, the nanometal wires in the prepared wire will be sparse, affecting the electrical conductivity. Therefore, the mass proportion of the nanometal wires in the nanometal wire dispersion is preferably controlled at 0.5%-2%.

[0029] Furthermore, the nanometal wire dispersion may also contain other nanometal materials, including nanometal sheets and / or nanometal particles. Preferably, the ratio of the other nanometal materials to the nanometal wires is less than 1. Under the premise of not affecting the tensile properties, the impedance of the conductive layer structure is further reduced by introducing two-dimensional or zero-dimensional nanometal materials.

[0030] Furthermore, method one also includes the step of coating damping glue on the conductive mesh layer of the first substrate layer, by introducing low-stress damping glue on the surface of the conductive mesh layer in contact with the second substrate layer to improve the bonding force between the conductive mesh layer and the second substrate layer; preferably, the damping glue is coated after the conductive mesh layer is cured.

[0031] A third aspect of the present invention provides a diaphragm of a sound-emitting device, the diaphragm comprising the conductive layer structure described in the first aspect or the conductive layer structure prepared by the preparation method described in the second aspect, the conductive layer structure being used to connect the voice coil and the electrode of the sound-emitting device, thereby converting the contact resistance between the voice coil and the electrode from line resistance to surface resistance.

[0032] The arrangement of the conductive layer is such that the predetermined stretching direction is configured to match the direction in which the elastic deformation amplitude of the diaphragm is the largest.

[0033] Furthermore, a through hole from the second substrate layer to the conductive mesh layer is provided on each side of the second substrate layer, and the through hole is used to connect the electrode; the voice coil can be electrically connected to the conductive mesh layer through a lead wire, or directly penetrate the second substrate layer / first substrate to form an electrical connection with the conductive mesh layer.

[0034] In existing speakers, the voice coil and the electrode are conductively connected through copper wire (lead), and there is line resistance between them. During the operation of the speaker, the lead between the voice coil and the electrode will be stretched due to vibration, which may easily lead to the risk of lead breakage. The above-mentioned conductive layer structure prepared by the present invention has a higher elastic tensile polarity than copper wire, etc. The voice coil lead is now connected to the electrode through a conductive mesh layer that is conductive on the entire surface, and the stress generated during the vibration process can be effectively released through the elastic deformation of the conductive layer, reducing the risk of lead breakage; or the voice coil is directly penetrated through the top surface and electrically connected to the conductive mesh layer, and the voice coil and the electrode are transformed into a surface resistance, thereby improving the reliability of the connection between the voice coil and the electrode.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The present invention provides a conductive layer sheet structure having a sandwich structure, which is composed of upper and lower flexible substrate layers and an inner conductive mesh layer having a parallelogram grid shape. The conductive mesh layer having this structure has low impedance, strong shape deformability and is conducive to stress dispersion, which is beneficial to improving the conductivity and elongation of the conductive layer sheet. Moreover, under the protective effect of the upper and lower flexible substrates on the conductive mesh layer, the conductive layer sheet not only has a high elongation rate, but also has a low impedance change rate with increasing elongation rate.

[0037] 2. The present invention also provides a method for preparing a conductive layer structure, which can directly use a nanometal wire dispersion to prepare a specific pattern of wires on the surface of a substrate, and without adding specific additives such as surfactants, a specific coating method can be used to make the orientation of the nanometal wires in the prepared wire consistent with the extension direction of the wire, so that a micro-grid structure is formed in the overlap area, thereby realizing the preparation of a highly conductive conductive mesh layer, and at the same time effectively reducing the resistance growth rate of the conductive layer structure under tension. The above method is simple to operate, and the performance of the prepared conductive layer structure is controllable, which is suitable for large-scale preparation.

[0038] 3. The present invention uses a macroscopic design on the conductive mesh layer structure and a microscopic design on the orientation of nano-metal wires in the conductive wire, combined with the protective effect of the upper and lower flexible substrate layers, to make the conductive layer structure have both high conductivity and high elongation, a low resistance change rate under stretching, and good resilience, and can be used as a diaphragm in a sound-generating device. It can continuously stretch and rebound during the vibration process, effectively improving the reliability of the electrical connection between the voice coil and the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Schematic diagram of the structure of preparing a conductive grid on a first substrate layer, 01 is a first preset direction, 02 is a second preset direction, 03 is a predetermined stretching direction, and 04 is the first substrate layer;

[0040] Figure 2 Schematic diagram of the diaphragm structure prepared in Example 1, 11 is a first substrate layer, 12 is a conductive mesh layer, 13 is a second substrate layer, and 14 is a through hole;

[0041] Figure 3 Schematic diagram of the conductive layer structure prepared in Example 2, 21 is a first substrate layer, 22 is a conductive mesh layer, 23 is a damping rubber layer, and 24 is a second substrate layer;

[0042] Figure 4 31 is a schematic diagram of a conductive layer structure, 32 is a first substrate layer, 33 is a damping adhesive layer, 34 is a second conductor group, and 35 is a second substrate layer. DETAILED DESCRIPTION

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0044] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0045] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0046] Example 1

[0047] This embodiment relates to the preparation of a conductive layer structure and a diaphragm, and the specific operations are as follows:

[0048] Preparation of conductive layer structure:

[0049] (1) Plasma treatment was performed on the surface of the first substrate layer (rubber substrate) having a thickness of 15 μm;

[0050] (2) applying a nano silver wire dispersion along a first preset direction and a second preset direction by a wire bar onto one side of the surface treated first substrate layer to prepare a first wire group and a second wire group, and curing the dispersion at 150° C. for 5 min to form a conductive mesh layer having a diamond grid shape; wherein the nano silver wire dispersion is composed of surface modified nano silver wires, a dispersant, a thickener, and a coupling agent, the mass proportion of the nano silver wires in the nano silver wire dispersion is 1%, the length of the nano silver wires is about 55 μm, the diameter is about 60 nm, the thickness of the conductive mesh layer is 500 nm, the angle between the first wire group and the second wire group is 90°, the angle between the first wire group and the predetermined stretching direction is 45°, the spacing between adjacent parallel wires in the first wire group and the second wire group is the same, both are 4 μm, and the wire width is 2 μm;

[0051] (3) PDMS prepolymer was coated on the conductive mesh layer of the first substrate layer, and after curing at 180° C. for 10 min, a second substrate layer with a thickness of 15 μm was obtained to obtain a conductive layer structure.

[0052] Preparation of the diaphragm:

[0053] In one embodiment, a voice coil is installed on the conductive layer structure (e.g., embedded in the middle of the conductive layer, etc.), and the leads at both ends of the voice coil are electrically connected to the conductive mesh layer, and the positive and negative electrodes of the voice coil are respectively connected to the independent conductive mesh layers on the left and right sides (the conductive mesh layers on both sides are not conductive, which can be achieved by only setting a wire group on both sides of the conductive layer structure and not setting a wire group in the middle part, for example, by covering the middle part with a mask, and peeling off the wire group in the middle part after the wire group is formed, so that the conductive mesh on both sides of the mask is not conductive), and through holes 14 are opened on both sides of the PDMS (second substrate layer) on the upper layer of the conductive layer structure for connecting electrodes, such as Figure 2 As shown, the voice coil is electrically connected to the electrode through the conductive layer that is conductive on the entire surface. The resistance between the voice coil and the electrode is the surface resistance, which improves the reliability of the connection between the voice coil and the electrode. The stress generated during the vibration process can be effectively released through the elastic deformation of the conductive layer, reducing the risk of lead breakage.

[0054] In other implementations, the voice coil body may also be directly electrically connected to the conductive mesh layer through the first substrate layer or the second substrate layer of the conductive layer structure without providing a lead wire.

[0055] The arrangement of the conductive layer is such that the predetermined stretching direction is configured to match the direction in which the elastic deformation amplitude of the diaphragm is the largest.

[0056] Example 2

[0057] This embodiment relates to the preparation of a conductive layer structure, which is different from the preparation of the conductive layer structure in Example 1 in that: before preparing the second substrate layer (PDMS), a layer of UV-curable damping glue (nitrile rubber) with a thickness of 500 nm is first coated on the conductive mesh layer, and then the second substrate layer is prepared on the damping glue layer. The rest of the operations are the same to obtain Figure 3 The conductive layer structure shown.

[0058] Example 3

[0059] This embodiment relates to the preparation of a conductive layer structure, and the specific operations are as follows:

[0060] (1) Plasma treatment was performed on the surfaces of a first substrate layer (rubber substrate) having a thickness of 30 μm and a second substrate layer (PDMS layer) having a thickness of 30 μm;

[0061] (2) The nano silver wire dispersion is applied along a first preset direction by a wire bar onto one side of the first substrate layer after surface treatment to prepare a first wire group, and the wire group is cured at 150°C for 5 minutes; the nano silver wire dispersion is applied along a second direction by a wire bar onto one side of the second substrate layer after surface treatment to prepare a second wire group, and the wire group is cured at 150°C for 5 minutes. The nano silver wire dispersion is composed of surface-modified nano silver wires, a dispersant, a thickener, and a coupling agent. The mass proportion of the nano silver wires in the nano silver wire dispersion is 1%. The nano silver wires are about 55 μm long and about 60 nm in diameter. The thickness of the first wire group and the second wire group is 250 nm. The spacing between adjacent parallel wires in the first wire group and the second wire group is the same, both 4 μm, and the wire width is 2 μm. In this embodiment, when the surfaces of the substrate where the first wire group and the second wire group are located are both facing upward, the first direction is the same as the second direction, and the angle with the predetermined stretching direction is 45°. When the surfaces of the substrate where the first wire group and the second wire group are located are in contact with each other, the angle between the first wire group and the second wire group is 90°.

[0062] (3) The surface of the first substrate layer where the first conductive wire group is located is laminated with the surface of the second substrate layer where the second conductive wire group is located, and hot pressing is performed (0.6 MPa, 180° C.) to obtain a conductive layer sheet structure.

[0063] Example 4

[0064] This embodiment relates to the preparation of a conductive layer sheet structure, and the only difference from Embodiment 1 is that the thickness of the conductive mesh layer is 1000 nm, and the other operations are the same to obtain a conductive layer sheet structure.

[0065] Example 5

[0066] This embodiment relates to the preparation of a conductive layer sheet structure, and the only difference from Embodiment 1 is that the thickness of the conductive mesh layer is 5 μm, and the other operations are the same to obtain a conductive layer sheet structure.

[0067] Example 6

[0068] This embodiment relates to the preparation of a conductive layer structure, and the only difference from Embodiment 1 is that a conductive mesh layer having a diamond grid shape is prepared by screen printing, and the other operations are the same to obtain a conductive layer structure with non-oriented nano silver wires.

[0069] Example 7

[0070] This embodiment relates to the preparation of a conductive layer structure, which is different from Embodiment 1 only in that the spacing between adjacent parallel wires in the first wire group and the second wire group is 8 μm, and the other operations are the same to obtain a conductive layer structure.

[0071] Example 8

[0072] This embodiment relates to the preparation of a conductive layer structure, which is different from the embodiment 1 only in that the length of the nano silver wire is about 80 μm, and the other operations are the same to obtain a conductive layer structure.

[0073] Example 9

[0074] This embodiment relates to the preparation of a conductive layer structure, which is different from Embodiment 1 only in that the angle between the first conductive wire group and the predetermined stretching direction is 60°, and the other operations are the same to obtain a conductive layer structure.

[0075] Comparative Example

[0076] This comparative example involves the preparation of a conductive layer structure, and the only difference from Example 1 is that an equal amount of nanosilver wire dispersion is used to prepare a 200 nm thick conductive layer on a first substrate layer by conventional coating, and the rest of the operations are the same to obtain a conductive layer structure.

[0077] Performance Testing

[0078] The conductive layer structures prepared in the above-mentioned embodiments and comparative examples were subjected to resistance tests under tension, and the test method was as follows:

[0079] The conductive layer structures prepared in Example 1 and Comparative Example 1 were cut to obtain similar strips, each strip was stretched in the length direction, and the resistance change of the strip was tested.

[0080] The test results are shown in Table 1 below:

[0081] Table 1

[0082]

[0083]

[0084] The “ / ” in the table indicates that no measurement was performed. When the conductive layer structure is destroyed under the action of stretching, it indicates that the material can no longer be used normally. Usually, the resistance in this case exceeds 20 times the initial impedance and increases rapidly with stretching.

[0085] It can be seen from Table 1 that, compared with the conductive layer structure prepared by the conventional coating method in the comparative example, the conductive layer having a conductive mesh layer structure prepared in Examples 1-9 has a high elongation rate and a low impedance change rate with increasing elongation rate. When stretched by 50%, the resistance of each spline does not exceed 20 times the initial resistance, while the resistance of the splines prepared in the comparative example exceeds 30 times the initial resistance under the same stretching degree.

[0086] It can be seen from Examples 1 and 2 that the introduction of the damping rubber layer will increase the initial impedance of the conductive layer structure, but the elasticity will not change significantly.

[0087] It can be seen from Examples 1, 4 and 5 that the initial impedance of the conductive layer structure will decrease with the increase of the thickness of the conductive mesh layer, but under the same stretching degree, the change rate of the conductive layer resistance will increase with the increase of the thickness of the conductive mesh layer. Preferably, the thickness of the conductive mesh layer is controlled within 500nm-1μm, so that the prepared conductive layer structure has high conductivity, high stretch rate and small change rate of stretching resistance.

[0088] It can be seen from Examples 1 and 6 that the orientation of the silver nanowires will affect the resistance change rate of the conductive layer structure under stretching. Example 6 uses screen printing to prepare the conductive mesh layer of the conductive layer, and the silver nanowires in the prepared conductive mesh layer are randomly oriented. Its initial impedance is similar to that of the conductive mesh layer prepared in Example 1, but the change rate increases significantly under stretching.

[0089] It can be seen from Examples 1 and 7 that as the wire spacing increases, the silver nanowire content in the conductive mesh layer is lower under the same surface area, so the resistance of the prepared conductive layer is higher.

[0090] It can be seen from Examples 1 and 8 that excessively long nano-silver wires will reduce the resistance stability of the conductive layer structure under tension. This is because excessively long nano-metal wires are prone to agglomeration and it is difficult to effectively arrange them uniformly.

[0091] It can be seen from Examples 1 and 9 that the angle between the wire group in the conductive mesh layer and the predetermined stretching direction will affect the resistance stability of the conductive layer under stretching. For example, compared with Example 1, Example 9 changes the angle between the first / second wire group and the predetermined stretching direction from 45° / 45° to 60° / 30°. When the conductive layer structure is stretched by 50%, the resistance is more than 16 times the initial resistance. This is because the greater the deviation of the angle from 45°, when the conductive layer is stretched, the variable angle range between the first wire group and the second wire group in the predetermined stretching direction is limited to the smaller one of the angles. If the variable angle range is exceeded, the conductive network cannot be in a balanced state, resulting in a significant increase in resistance under a larger stretching state.

[0092] The above-mentioned embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by technicians in the technical field on the basis of the present invention are all within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A conductive layer structure, characterized in that: It includes a first substrate layer, a conductive mesh layer and a second substrate layer which are stacked in sequence; The conductive mesh layer includes a first conductive line group and a second conductive line group that are cross-arranged. The first conductive line group and the second conductive line group both include a plurality of conductive lines that are parallel and spaced apart. The conductive lines include nano metal wires.

2. The conductive layer structure according to claim 1, characterized in that: The materials of the first substrate layer and the second substrate layer are respectively selected from one or more of polyethylene terephthalate, polyethylene naphthalate, polymethyl methacrylate, polyimide, polyamide, polyurethane, polyarylate, polyphenylene sulfide, polysulfone, polyether sulfone, polyphenylene sulfide sulfone, rubber, silicone resin, polyether ether ketone, polycarbonate, polypropylene, and polydimethylsiloxane; The thickness of the first substrate layer is 1-30 μm; The thickness of the second substrate layer is 1-30 μm.

3. The conductive layer structure according to claim 1, characterized in that: The angle between the first wire group and the second wire group is 80°-100°; The angle between the first wire group or the second wire group and the predetermined stretching direction of the conductive layer structure is 40°-50°; In the first conductive line group and / or the second conductive line group, a spacing between adjacent parallel conductive lines is 1-500 μm; The wire has a width of 1-500 μm.

4. The conductive layer structure according to claim 1, characterized in that: The orientation of the nanometal wires in the wire is consistent with the direction in which the wire extends; The length of the nanometal wire is 20-80 μm, and the diameter is 20-100 nm; The nano metal wires include one or more of nano silver wires, nano gold wires, nano copper wires, and nano silver-coated copper wires.

5. The conductive layer structure according to claim 1, characterized in that: The thickness of the conductive mesh layer is 100nm-10μm; preferably 500nm-1μm; The conductive layer structure further comprises a damping rubber layer; the damping rubber layer is arranged in the grid of the conductive mesh layer; The damping glue in the damping glue layer is selected from one or more of saw blade damping glue, instantaneous damping glue, two-component epoxy damping elastic potting glue, epoxy damping potting glue, flame retardant damping insulating glue, and UV curing damping glue; The thickness of the damping adhesive layer is 100nm-10μm.

6. A method for preparing a conductive layer structure according to any one of claims 1 to 5, characterized in that: Includes the following methods: Method 1: Forming a plurality of conductive lines in parallel and at intervals along a first preset direction and a second preset direction on the first substrate layer to form a conductive mesh layer; The conductive layer structure is obtained by coating the prepolymer of the second substrate layer on the conductive mesh layer of the first substrate layer and curing the prepolymer to obtain the conductive layer structure; or, the first substrate layer including the conductive mesh layer is laminated with the second substrate layer, wherein the conductive mesh layer of the first substrate layer faces inwards, and the conductive layer structure is obtained by laminating the first substrate layer with the second substrate layer; Method 2: Forming a plurality of conductive wires in parallel and at intervals along a first preset direction on the first substrate layer to form a first conductive wire group; and forming a plurality of conductive wires in parallel and at intervals along a second preset direction on the second substrate layer to form a second conductive wire group; The first substrate layer including the first conductive wire group and the second substrate layer including the second conductive wire group are laminated together, wherein the surfaces where the first conductive wire group and the second conductive wire group are located face inwards, to obtain the conductive layer structure.

7. The preparation method according to claim 6, characterized in that: In the method 1: The forming step comprises: coating the nano-metal wire dispersion on the first substrate layer by one or more combinations of a pulling method, a wire rod coating method, a capillary assisted jet method, and a screen printing method, and curing to obtain the conductive mesh layer; In the second method: The forming step includes: coating the nanometal wire dispersion on the first substrate layer and the second substrate layer by one or more combinations of the pulling method, wire rod coating method, capillary assisted jet method, and screen printing method, and curing to obtain the first wire group and the second wire group.

8. The preparation method according to claim 7, characterized in that: The mass proportion of the nano-metal wires in the nano-metal wire dispersion is 0.5%-2%.

9. The preparation method according to claim 6, characterized in that: The method 1 further comprises the step of coating damping glue on the conductive mesh layer of the first substrate layer; The second method also includes the step of coating damping glue on the surface where the first wire group is located or the surface where the second wire group is located.

10. A diaphragm of a sound-generating device, characterized in that: The diaphragm comprises the conductive layer structure described in any one of claims 1 to 5 or the conductive layer structure prepared by the preparation method described in any one of claims 6 to 9.