Lithium-free negative electrode pole piece containing monatomic cobalt catalyst, lithium-free negative electrode battery and preparation method of lithium-free negative electrode pole piece
By using single-atom cobalt catalysts to regulate lithium ion deposition in lithium-free negative electrode batteries, the problems of low Coulombic efficiency and lithium dendrite formation caused by uneven lithium ion deposition are solved, and the energy density and safety of the battery are improved, making it suitable for industrial production. .
Patent Information
- Application Number
- CN202411143568.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium-free anode batteries have low Coulombic efficiency due to uneven lithium ion deposition, and are prone to the formation of lithium dendrites and dead lithium, resulting in insufficient battery safety and energy density.
Using a lithium-free negative electrode sheet containing a single-atom cobalt catalyst, the single-atom cobalt catalyst supported on the carbon matrix controls the lithium ion deposition process, reduces the nucleation overpotential and growth overpotential, achieves uniform deposition of lithium ions, and reduces lithium dendrites and Generation of dead lithium.
It significantly improves the Coulombic efficiency, cycle life and safety of the battery, increases the energy density of the battery, simplifies the preparation process, and is suitable for industrial production.
Smart Images

Figure CN118800876A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium-free negative electrode batteries, and in particular relates to a lithium-free negative electrode plate containing a single-atom cobalt catalyst, a lithium-free negative electrode battery and a preparation method thereof. Background Art
[0002] With the rapid development of electric vehicles and 3C electronic products, the requirements for battery energy density, cycle life and safety are constantly increasing. Traditional lithium-ion batteries mostly use active materials such as graphite in the negative electrode, but their energy density has reached its limit and it is difficult to meet the requirements. As a new type of battery technology, the core of lithium-free negative electrode batteries is that the negative electrode does not directly use pre-deposited lithium metal as an active material, but instead achieves the storage and release of electrical energy through the deposition and dissolution of lithium ions on the negative electrode current collector, thereby achieving higher energy density and better safety.
[0003] However, due to the uncontrollable process of lithium ion deposition and dissolution, a large amount of dead lithium and lithium dendrites will be generated at the negative electrode, causing serious battery safety problems such as thermal runaway. At the same time, the irreversible loss of active lithium in the battery causes the battery capacity to decrease rapidly, limiting the practical use of lithium-free negative electrode batteries.
[0004] At present, the main ways to improve lithium ion deposition include constructing a three-dimensional current collector and preparing a lithium-rich alloy coating. The invention patent with publication number CN113991054A, "A non-polar negative electrode sheet for lithium batteries and lithium batteries", uses cobalt or cobalt alloys to promote the uniform deposition of lithium on its surface. However, the alloy solution has the disadvantage of large mass itself. The formed alloy cannot exert the battery capacity and is an inert mass, which will greatly reduce the theoretical specific capacity of the battery and weaken the energy density advantage of the lithium-free negative electrode battery.
[0005] Therefore, how to suppress the formation of lithium dendrites and dead lithium in lithium-free negative electrode batteries and improve the coulombic efficiency of batteries while also improving the energy density of batteries remains an urgent problem to be solved in this field. Summary of the invention
[0006] In order to solve the problem of low coulombic efficiency of existing lithium-free negative electrode batteries due to uneven lithium ion deposition, the present invention provides a lithium-free negative electrode plate containing a single-atom cobalt catalyst, a lithium-free negative electrode battery and a preparation method thereof.
[0007] The technical solution of the present invention:
[0008] A lithium-free negative electrode plate containing a single-atom cobalt catalyst, wherein the lithium-free negative electrode plate comprises a single-atom cobalt catalyst, a metal current collector and a binder, wherein the single-atom cobalt catalyst is a single-atom cobalt supported on a carbon matrix.
[0009] Furthermore, the preparation method of the single-atom cobalt catalyst is as follows: 2-methylimidazole is dissolved in methanol to obtain solution A, zinc nitrate hexahydrate and cobalt nitrate hexahydrate are dissolved in methanol solution to obtain solution B, the solution B is added to the solution A, and the mixture is fully mixed to obtain solution C, the solution C is reacted under stirring to obtain a suspension, the suspension is centrifuged to obtain crystals, the obtained crystals are washed and dried to obtain dry powder, and the dry powder is heat-treated in an Ar environment to obtain a single-atom cobalt catalyst.
[0010] Furthermore, the molar ratio of the 2-methylimidazole, zinc nitrate hexahydrate and cobalt nitrate hexahydrate is 20-40:5-8:0.5-1.0.
[0011] Furthermore, the reaction time of the solution C under stirring is 6 to 18 hours; the rotation speed of the suspension centrifuge is 10,000 rpm; the centrifugation time is 15 to 30 minutes; the crystal drying temperature is 50 to 90°C, and the drying time is 2 to 6 hours; the heating rate of the dry powder during heating treatment in an Ar environment is 5°C / min, the heating temperature is 900°C, and the heating time is 0.5 to 2.0 hours.
[0012] Furthermore, the metal current collector is a foil or mesh made of copper, nickel, titanium or stainless steel; and the binder is a combination of carboxymethyl cellulose and styrene-butadiene latex.
[0013] A method for preparing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst provided by the present invention comprises the following steps:
[0014] Step 1, adding deionized water to the first binder and stirring evenly to obtain slurry I;
[0015] Step 2: adding the single-atom cobalt catalyst powder provided by the present invention to the slurry I obtained in step 1, and stirring evenly to obtain slurry II;
[0016] Step 3, adding a second binder to the slurry II obtained in step 2, and stirring evenly to obtain slurry III;
[0017] Step 4: Apply the slurry III obtained in step 3 on the surface of the metal current collector, and obtain a lithium-free negative electrode sheet containing a single-atom cobalt catalyst after vacuum drying and roller pressing.
[0018] Furthermore, in the step one, the first binder is carboxymethyl cellulose, in the step three, the second binder is styrene-butadiene latex, and the mass ratio of the first binder, the second binder, and the single-atom cobalt catalyst powder in the slurry III is 1 to 2:1 to 2:16.
[0019] Furthermore, the stirring speed in step 1, step 2 and step 3 is 600-1000 rpm, the stirring time is 1-4 h, the stirring temperature is 20-30° C., and the vacuum condition of stirring is -0.01-0.1 MPa.
[0020] Furthermore, the coating thickness in step 4 is 10-30 μm, the vacuum drying temperature is 60-100° C., the drying time is 24-48 hours, the vacuum degree is 0.01-0.2 MPa; and the roller pressing pressure is 20±5 t.
[0021] A lithium-free negative electrode battery comprises the lithium-free negative electrode plate containing a single-atom cobalt catalyst provided by the invention.
[0022] Beneficial effects of the present invention:
[0023] The lithium-free negative electrode plate containing a single-atom cobalt catalyst provided by the present invention uses a single-atom cobalt catalyst as an active layer, utilizes the characteristics of the 2P electrons of the N atom in the cobalt single atom and the material work function, and reduces the nucleation overpotential and the growth overpotential by regulating the reaction speed of two key steps in the lithium ion deposition process, thereby achieving uniform deposition of lithium ions, avoiding excessive local concentration, and reducing the generation of lithium dendrites; at the same time, uniform lithium deposition enables the negative electrode to utilize space more effectively, reduces the generation of dead lithium, and further reduces the loss of active lithium, effectively reducing the irreversible decay of the battery capacity.
[0024] Since the lithium-free negative electrode sheet containing a single-atom cobalt catalyst prepared by the present invention can reduce the generation of lithium dendrites and dead lithium, using it to prepare a lithium-free negative electrode battery can significantly improve the coulombic efficiency, cycle life, safety and energy density of the battery. The preparation process of the single-atom cobalt catalyst and the lithium-free negative electrode sheet of the present invention is simple and suitable for the industrial production of lithium metal secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a spherical aberration-corrected electron microscope characterization spectrum of the single-atom cobalt catalyst obtained in Example 1;
[0026] Figure 2 Capacity-cycle number diagram of the batteries prepared in Example 7 and Comparative Example 1;
[0027] Figure 3 Capacity-cycle number diagram of the batteries prepared in Example 8 and Comparative Example 1;
[0028] Figure 4 The discharge voltage-capacity curve of the lithium-free negative electrode battery prepared in Example 8;
[0029] Figure 5 The discharge capacitance-capacity curve of the battery prepared in Comparative Example 1;
[0030] Figure 6 The following are pictures showing the evolution of the morphology during lithium deposition on the surface of the negative electrode in the batteries of Example 9 and Comparative Example 2;
[0031] Figure 7 This is a comparison chart of the Aurbach coulomb efficiency test results of the batteries prepared in Example 7, Comparative Example 3 and Comparative Example 4, in which a is a lithium-free negative electrode sheet containing a single-atom cobalt catalyst, b is a nitrogen-doped graphene lithium-free negative electrode, and c is a copper foil;
[0032] Figure 8 These are scanning electron micrographs of the negative electrode sheets in the batteries after cycles of Example 7 and Comparative Example 4, where a, b, and c are copper foils, and d, e, and f are lithium-free negative electrode sheets containing single-atom cobalt catalysts. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0034] Example 1
[0035] This embodiment provides a single-atom cobalt catalyst and a preparation method thereof.
[0036] The preparation method of the single-atom cobalt catalyst in this embodiment is as follows:
[0037] 28.0mmol of 2-methylimidazole was dissolved in 60ml of methanol to obtain solution A, 6.3mmol of zinc nitrate hexahydrate and 0.7mmol of cobalt nitrate hexahydrate were dissolved in 60ml of methanol solution to obtain solution B, the solution B was added into the solution A, and the mixture was fully mixed to obtain solution C, the solution C was reacted for 12h under stirring to obtain a suspension, the obtained suspension was centrifuged at 10000rpm for 20min to obtain crystals, the crystals were collected and washed three times with methanol, the washed crystals were placed in a vacuum oven at 70°C and dried for 4h to obtain dry powder, the obtained dry powder was heated to 900°C in an Ar environment at a heating rate of 5°C / min and maintained for 1h to obtain a single atom cobalt catalyst.
[0038] Figure 1 This is a spherical aberration-corrected electron microscope characterization spectrum of the single-atom cobalt catalyst obtained in this example. The picture proves that the single cobalt atom was successfully synthesized.
[0039] Example 2
[0040] This embodiment provides a single-atom cobalt catalyst and a preparation method thereof.
[0041] The preparation method of the single-atom cobalt catalyst in this embodiment is as follows:
[0042] 20.0mmol of 2-methylimidazole was dissolved in 60ml of methanol to obtain solution A, 5.0mmol of zinc nitrate hexahydrate and 0.5mmol of cobalt nitrate hexahydrate were dissolved in 60ml of methanol solution to obtain solution B, the solution B was added into the solution A, and the mixture was fully mixed to obtain solution C, the solution C was reacted for 6h under stirring to obtain a suspension, the obtained suspension was centrifuged at 10000rpm for 20min to obtain crystals, the crystals were collected and washed three times with methanol, the washed crystals were placed in a 50°C vacuum oven and dried for 6h to obtain dry powder, the obtained dry powder was heated to 900°C in an Ar environment at a heating rate of 5°C / min and maintained for 0.5h to obtain a single atom cobalt catalyst.
[0043] Example 3
[0044] This embodiment provides a single-atom cobalt catalyst and a preparation method thereof.
[0045] The preparation method of the single-atom cobalt catalyst in this embodiment is as follows:
[0046] 40.0mmol of 2-methylimidazole was dissolved in 60ml of methanol to obtain solution A, 8.0mmol of zinc nitrate hexahydrate and 1.0mmol of cobalt nitrate hexahydrate were dissolved in 60ml of methanol solution to obtain solution B, the solution B was added into the solution A, and the mixture was fully mixed to obtain solution C, the solution C was reacted for 18h under stirring to obtain a suspension, the obtained suspension was centrifuged at 10000rpm for 20min to obtain crystals, the crystals were collected and washed three times with methanol, the washed crystals were placed in a vacuum oven at 90°C and dried for 2h to obtain dry powder, the obtained dry powder was heated to 900°C in an Ar environment at a heating rate of 5°C / min and maintained for 2.0h to obtain a single atom cobalt catalyst.
[0047] Example 4
[0048] This embodiment provides a single-atom cobalt catalyst and a preparation method thereof.
[0049] The preparation method of the single-atom cobalt catalyst in this embodiment is as follows:
[0050] 25.0mmol of 2-methylimidazole was dissolved in 60ml of methanol to obtain solution A, 7.0mmol of zinc nitrate hexahydrate and 0.8mmol of cobalt nitrate hexahydrate were dissolved in 60ml of methanol solution to obtain solution B, the solution B was added into the solution A, and the mixture was fully mixed to obtain solution C, the solution C was reacted for 15h under stirring to obtain a suspension, the obtained suspension was centrifuged at 10000rpm for 20min to obtain crystals, the crystals were collected and washed three times with methanol, the washed crystals were placed in a vacuum oven at 80°C and dried for 3h to obtain dry powder, the obtained dry powder was heated to 900°C in an Ar environment at a heating rate of 5°C / min and maintained for 1.5h to obtain a single atom cobalt catalyst.
[0051] Example 5
[0052] In this example, a lithium-free negative electrode plate was prepared using the single-atom cobalt catalyst prepared in Example 1 as the active layer.
[0053] The preparation method of the lithium-free negative electrode plate of this embodiment is as follows:
[0054] Step 1: add an appropriate amount of deionized water to 10 mg of carboxymethyl cellulose, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of -0.05 MPa, and stir evenly to obtain slurry I;
[0055] Step 2: Add 160 mg of the single-atom cobalt catalyst powder prepared in Example 1 to the slurry I obtained in Step 1, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of −0.05 MPa, and stir to obtain slurry II;
[0056] Step 3: Add 10 mg of styrene-butadiene latex to the slurry II obtained in step 2, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of -0.05 MPa, and stir evenly to obtain a slurry III with a viscosity of 4000 mPa·s;
[0057] Step 4: Cut the copper foil into appropriate size, clean and dry it with anhydrous ethanol, stick insulating tape to determine the coating area before coating, and apply slurry III obtained in step 3 on the surface of the copper foil with a coating thickness of 20μm. After single-sided coating is completed, vacuum dry the electrode to a certain degree, and then coat the other side with a coating thickness of 20μm.
[0058] The double-sided coated negative electrode sheet was dried in a vacuum oven at a temperature of 80°C, a vacuum degree of 0.1 MPa and a drying time of 36 h. The dried negative electrode sheet was roll-pressed in a roller press at a pressure of 20 t to obtain a lithium-free negative electrode sheet containing a single-atom cobalt catalyst.
[0059] The obtained lithium-free negative electrode sheet was cut using a steel knife paper cutter. Except for the active material area, a 3 mm wide area of the metal current collector was reserved for welding.
[0060] Example 6
[0061] In this example, a lithium-free negative electrode plate was prepared using the single-atom cobalt catalyst prepared in Example 1 as the active layer.
[0062] The preparation method of the lithium-free negative electrode plate of this embodiment is as follows:
[0063] Step 1, add an appropriate amount of deionized water to 20 mg of carboxymethyl cellulose, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of -0.05 MPa, and stir evenly to obtain slurry I;
[0064] Step 2: Add 160 mg of the single-atom cobalt catalyst powder prepared in Example 1 to the slurry I obtained in Step 1, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of −0.05 MPa, and stir to obtain slurry II;
[0065] Step 3: Add 20 mg of styrene-butadiene latex to the slurry II obtained in step 2, stir at 800 rpm for 2 h at a temperature of 25° C. and a vacuum degree of -0.05 MPa, and stir evenly to obtain a slurry III with a viscosity of 4000 mPa·s;
[0066] Step 4: Cut the copper foil into appropriate size, clean and dry it with anhydrous ethanol, stick insulating tape to determine the coating area before coating, and apply slurry III obtained in step 3 on the surface of the copper foil with a coating thickness of 20μm. After single-sided coating is completed, vacuum dry the electrode to a certain degree, and then coat the other side with a coating thickness of 20μm.
[0067] The double-sided coated negative electrode sheet was dried in a vacuum oven at a temperature of 80°C, a vacuum degree of 0.1 MPa and a drying time of 36 h. The dried negative electrode sheet was roll-pressed in a roller press at a pressure of 30 t to obtain a lithium-free negative electrode sheet containing a single-atom cobalt catalyst.
[0068] The obtained lithium-free negative electrode sheet was cut using a steel knife paper cutter. Except for the active material area, a 3 mm wide area of the metal current collector was reserved for welding.
[0069] Example 7
[0070] In this example, a lithium-free negative electrode battery is prepared using the lithium-free negative electrode sheet prepared in Example 5.
[0071] The preparation method of the lithium-free negative electrode battery in this embodiment is:
[0072] The experiment was carried out in a glove box, where the argon content was 99.999%, the oxygen content was <0.1ppm, and the moisture content was <0.1ppm. The lithium-free negative electrode plate and NCM811 positive electrode prepared in Example 5 were used to form a lithium-free negative electrode battery. The electrolyte used was 1MLiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator was Celgard2320.
[0073] Example 8
[0074] In this example, the lithium-free negative electrode sheet prepared in Example 5 was used to prepare a pre-lithiated lithium-free negative electrode battery.
[0075] The preparation method of the lithium-free negative electrode battery in this embodiment is:
[0076] Step 1. The lithium-free negative electrode sheet prepared in Example 5 is pre-lithiated: the argon content in the glove box is 99.999%, the oxygen content is less than 0.1ppm, and the moisture content is less than 0.1ppm; the lithium-free negative electrode sheet prepared in Example 5 and the lithium sheet are used to form a battery, and the electrolyte is 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator is Celgard2320. At 0.1mA / cm 2 The battery was discharged at a current density of , and the cut-off capacity was calculated based on the surface capacity of the NCM811 positive electrode. The battery was disassembled to obtain a pre-lithiated lithium-free negative electrode sheet (N / P=1).
[0077] Step 2. The process is carried out in a glove box with an argon content of 99.999%, an oxygen content of <0.1ppm, and a moisture content of <0.1ppm. A lithium-free negative electrode battery is formed with a pre-lithiated lithium-free negative electrode sheet and an NCM811 positive electrode. The electrolyte is 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator is Celgard2320.
[0078] Example 9
[0079] In this example, a lithium-free negative electrode half-cell was prepared using the lithium-free negative electrode sheet prepared in Example 5.
[0080] The preparation method of the lithium-free negative electrode battery in this embodiment is:
[0081] The test was carried out in a glove box, where the argon content was 99.999%, the oxygen content was <0.1ppm, and the moisture content was <0.1ppm. The lithium-free negative electrode plate and Li plate prepared in Example 5 were used as the positive electrode to form a lithium-free negative electrode battery. The electrolyte used was 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator was Celgard2320.
[0082] Comparative Example 1
[0083] In this comparative example, a lithium-free negative electrode battery was prepared using copper foil as a metal current collector. The specific preparation method is as follows:
[0084] The experiment was carried out in a glove box with an argon content of 99.999%, an oxygen content of <0.1ppm, and a moisture content of <0.1ppm. A lithium-free negative electrode battery was composed of copper foil as the negative electrode and NCM811 as the positive electrode. The electrolyte used 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator used Celgard2320.
[0085] Figure 2 The capacity-cycle number diagram of the batteries prepared in Example 7 and Comparative Example 1; Figure 2 As shown, the lithium-free negative electrode battery containing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst still maintains a capacity retention rate of 78.55% after 150 cycles, while the capacity retention rate of the battery composed of copper foil is less than 10% after 54 cycles.
[0086] Figure 3 Capacity-cycle number diagram of the batteries prepared in Example 8 and Comparative Example 1; Figure 4 and Figure 5 The discharge voltage-capacity curves of the lithium-free negative electrode battery prepared in Example 8 and the battery prepared in Comparative Example 1 are as follows; Figure 3 , Figure 4 , Figure 5 As shown, the lithium-free negative electrode battery composed of the lithium-free negative electrode sheet containing single-atom cobalt catalyst still maintains a capacity retention rate of 98.82% after 150 cycles, while that composed of copper foil is only 34.98%.
[0087] Comparative Example 2
[0088] In this comparative example, a lithium-free negative electrode half-cell was prepared using copper foil as the positive electrode and Li sheet as the anode. The specific preparation method is as follows:
[0089] The experiment was carried out in a glove box with an argon content of 99.999%, an oxygen content of <0.1ppm, and a moisture content of <0.1ppm. A lithium-free negative electrode battery was composed of a copper foil as the negative electrode and a Li sheet as the positive electrode. The electrolyte used 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator used Celgard2320.
[0090] The evolution of the morphology of the negative electrode surface during lithium deposition in the batteries of Example 7 and Comparative Example 2 was observed by optical microscopy. The results are as follows: Figure 6 As shown, it can be found that on the lithium-free negative electrode sheet containing single-atom cobalt catalyst, lithium deposition is more uniform and stable; while lithium dendrites and dead lithium quickly appear on the copper foil.
[0091] Comparative Example 3
[0092] In this comparative example, a lithium-free negative electrode battery was prepared using nitrogen-doped graphene as the negative electrode. The specific preparation method is as follows:
[0093] The experiment was carried out in a glove box with an argon content of 99.999%, an oxygen content of <0.1ppm, and a moisture content of <0.1ppm. A lithium-free negative electrode battery was composed of a nitrogen-doped graphene lithium-free negative electrode as the negative electrode and NCM811 as the positive electrode. The electrolyte used 1M LiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator used Celgard2320.
[0094] Comparative Example 4
[0095] In this comparative example, a lithium-free negative electrode battery is prepared using pre-lithiated copper foil as the negative electrode. The specific preparation method is as follows:
[0096] The experiment was carried out in a glove box with an argon content of 99.999%, an oxygen content of <0.1ppm, and a moisture content of <0.1ppm. The pre-lithiation copper foil was used as the negative electrode and NCM811 was used as the positive electrode to form a lithium-free negative electrode battery. The electrolyte used was 1MLiPF6, ethylene carbonate, diethyl carbonate, and dimethyl carbonate (1 / 1 / 1, v / v / v), and the battery separator was Celgard2320.
[0097] The Aurbach coulomb efficiency test was performed on the batteries prepared in Example 7, Comparative Example 3 and Comparative Example 4. The results are as follows: Figure 7 As shown, the lithium-free negative electrode sheet containing single-atom cobalt catalyst can stably deposit / strip lithium for up to 657 hours, and the average CE of the whole cycle reaches 99.19%, which is much higher than the average CE of 95.05% in 213 hours on copper foil and the average CE of 96.98.8% in 213 hours on nitrogen-doped graphene lithium-free negative electrode.
[0098] The cycled battery was disassembled in a glove box, and the lithium deposition morphology on the surface of the lithium-free negative electrode sheet and copper foil containing single-atom cobalt catalyst was further verified using scanning electron microscopy (SEM). The results are as follows: Figure 8 As shown, the lithium particles deposited on the lithium-free negative electrode sheet containing single-atom cobalt catalyst are smaller in size compared to copper foil.
Claims
1. A lithium-free negative electrode sheet containing a single-atom cobalt catalyst, It is characterized in that The lithium-free negative electrode plate comprises a single-atom cobalt catalyst, a metal current collector and a binder, and the single-atom cobalt catalyst is a single-atom cobalt supported on a carbon matrix.
2. A lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 1, It is characterized in that The preparation method of the single-atom cobalt catalyst is as follows: 2-methylimidazole is dissolved in methanol to obtain solution A, zinc nitrate hexahydrate and cobalt nitrate hexahydrate are dissolved in methanol solution to obtain solution B, the solution B is added to the solution A, and the mixture is fully mixed to obtain solution C, the solution C is reacted under stirring to obtain a suspension, the suspension is centrifuged to obtain crystals, the obtained crystals are washed and dried to obtain dry powder, and the dry powder is heated in an Ar environment to obtain a single-atom cobalt catalyst.
3. A lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 2, It is characterized in that The molar ratio of the 2-methylimidazole, zinc nitrate hexahydrate and cobalt nitrate hexahydrate is 20-40:5-8:0.5-1.
0.
4. A lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 2 or 3, It is characterized in that The reaction time of the solution C under stirring is 6 to 18 hours; the rotation speed of the suspension centrifuge is 10,000 rpm; the centrifugation time is 15 to 30 minutes; the crystal drying temperature is 50 to 90°C, and the drying time is 2 to 6 hours; the heating rate of the dry powder in the Ar environment is 5°C / min, the heating temperature is 900°C, and the heating time is 0.5 to 2.0 hours.
5. A lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 4, It is characterized in that The metal current collector is a foil or mesh made of copper, nickel, titanium or stainless steel; the binder is a combination of carboxymethyl cellulose and styrene-butadiene latex.
6. A method for preparing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst as claimed in any one of claims 1 to 5, It is characterized in that Here are the steps: Step 1, adding deionized water to the first binder and stirring evenly to obtain slurry I; Step 2, adding the single-atom cobalt catalyst powder according to any one of claims 1 to 5 to the slurry I obtained in step 1, and stirring to obtain slurry II; Step 3, adding a second binder to the slurry II obtained in step 2, and stirring evenly to obtain slurry III; Step 4: Apply the slurry III obtained in step 3 on the surface of the metal current collector, and obtain a lithium-free negative electrode sheet containing a single-atom cobalt catalyst after vacuum drying and roller pressing.
7. A method for preparing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 6, It is characterized in that In the step one, the first binder is carboxymethyl cellulose, in the step three, the second binder is styrene-butadiene latex, and the mass ratio of the first binder, the second binder, and the single-atom cobalt catalyst powder in the slurry III is 1-2:1-2:
16.
8. A method for preparing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 6 or 7, It is characterized in that The stirring speeds in step 1, step 2 and step 3 are all 600 to 1000 rpm, the stirring time is all 1 to 4 h, the stirring temperature is all 20 to 30° C., and the vacuum conditions for stirring are all -0.01 to -0.1 MPa.
9. A method for preparing a lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to claim 6 or 7, It is characterized in that The coating thickness of step 4 is 20 μm, the vacuum drying temperature is 60-100° C., the drying time is 24-48 hours, the vacuum degree is 0.01-0.2 MPa; and the roller pressing pressure is 30 t.
10. A lithium-free negative electrode battery, It is characterized in that A lithium-free negative electrode sheet containing a single-atom cobalt catalyst according to any one of claims 1 to 5.
Citation Information
Patent Citations
Monoatomic dispersed PtCo-N-C catalyst as well as preparation method and application thereof
CN116230972A
Preparation method and application of honeycomb nitrogen-doped carbon material loaded with lithium-loving nanoparticles
CN116332153A