Layered graphite carbon-based ruthenium-cobalt electrocatalyst, preparation method thereof and battery
By using electrocatalysts with nitrogen-doped porous graphite carbon layers and ruthenium-cobalt alloy nanoclusters in the field of electrochemical energy storage, the problems of high overpotential and low energy conversion efficiency of noble metal-based electrocatalysts have been solved, achieving more efficient and stable electrochemical reaction, reducing production costs.
Patent Information
- Application Number
- CN202411281685.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing precious metal-based electrocatalysts have high overpotential and low energy conversion efficiency in the field of electrochemical energy storage, which limits the commercial application of batteries.
A nitrogen-doped porous flaky graphite carbon layer and a lamellar graphite carbon-based ruthenium-cobalt electrocatalyst loaded with ruthenium-cobalt alloy nanoclusters are used, and are prepared by electrochemical stripping to reduce costs and improve catalytic activity and stability.
A lower reversible oxygen overpotential is achieved, which improves energy conversion efficiency, reduces production costs, and enhances the broad application potential of electrocatalysts.
Smart Images

Figure CN118800922A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochemical energy storage, and in particular to a lamellar graphite carbon-based ruthenium-cobalt electrocatalyst and a preparation method and a battery thereof. Background Art
[0002] Bifunctional oxygen catalysts are catalysts that can catalyze two oxygen-related electrochemical reactions, which can undergo slow four-electron oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) at the air-electrode interface. The former reaction produces excellent power density output, and the latter reaction basically presents a stable charge-discharge voltage gap, which is a key indicator of bifunctional properties. To date, precious metal-based electrocatalysts such as Pt / C, IrO 2 and RuO 2 , which are considered the benchmark for ORR and OER. However, the high overpotentials and low overall energy conversion efficiencies of noble metal-based systems severely limit the commercial application of batteries. Therefore, the development of efficient and durable bifunctional oxygen catalysts with a maximum number of accessible active sites remains a challenge to achieve cheap batteries.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a lamellar graphite carbon-based ruthenium cobalt electrocatalyst and a preparation method and a battery thereof, so as to solve the problems of high overpotential, low energy conversion efficiency and limited commercial application of the noble metal-based system in the prior art.
[0005] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: In a first aspect, the present invention provides a lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, wherein the electrocatalyst comprises a nitrogen-doped porous flaky graphite carbon layer and ruthenium-cobalt alloy nanoclusters supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanoclusters is less than 8 nm.
[0006] As a further preferred technical solution, the content of ruthenium in the electrocatalyst is 3wt%-8wt%, the content of cobalt is 3wt%-10wt%, the content of nitrogen is 1wt%-5wt%, and the content of carbon is 77wt%-93wt%.
[0007] As a further preferred technical solution, the electrocatalyst has a specific surface area of 100-2000m 2 / g.
[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned lamellar graphite carbon-based ruthenium cobalt electrocatalyst, comprising the following steps: S1, continuously electrolyzing the graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a flaky carbon material; S2. Mixing the flaky carbon material with a ruthenium source, a cobalt source and a nitrogen source, stirring the mixture, drying the mixture and calcining the mixture in an inert atmosphere to obtain the electrocatalyst.
[0009] As a further preferred technical solution, in S1, the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 70-74 hours, and the scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 75-85° C. for 10-14 hours.
[0010] As a further preferred technical solution, the ruthenium source includes ruthenium chloride, the cobalt source includes cobalt nitrate, and the nitrogen source includes dopamine.
[0011] As a further preferred technical solution, the mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride, and the cobalt nitrate is (1-1.5): (0.5-1.0): (0.03-1.0): (0.01-1.0).
[0012] As a further preferred technical solution, in S2, the mixing and stirring comprises: mixing the lamellar carbon material, the dopamine and Tris-HCl, and stirring for 25-35 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 45-50 h.
[0013] As a further preferred technical solution, in S2, the calcination includes: first calcining at 150-250°C for 1.5-2.5h, and then calcining at 850-950°C for 1.5-2.5h.
[0014] In a third aspect, the present invention provides a battery comprising an electrode, wherein the electrode comprises the above-mentioned lamellar graphite carbon-based ruthenium cobalt electrocatalyst or the lamellar graphite carbon-based ruthenium cobalt electrocatalyst obtained by the above-mentioned preparation method.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The lamellar graphite carbon-based ruthenium cobalt electrocatalyst provided by the present invention comprises a nitrogen-doped porous flaky graphite carbon layer and a ruthenium cobalt alloy nanocluster loaded on the graphite carbon layer, wherein the size of the ruthenium cobalt alloy nanocluster is less than 8nm, and no precious metal is used, thereby greatly reducing the cost and being widely used. In addition, the graphite carbon layer of the electrocatalyst is a porous flaky structure, which can effectively promote long-distance mass transfer and active site exposure, thereby improving the formation efficiency of the solid-liquid-gas reaction interface, and the energy conversion efficiency is higher. The ruthenium cobalt alloy nanocluster is used relative to the single-atom catalyst, and the catalytic activity is higher and more stable. The reversible oxygen overpotential of the electrocatalyst is 0.713 V or lower for OER / ORR.
[0016] For graphitized carbon-based materials, it is still difficult to manufacture a sheet-like open system with a large number of macropores and mesopores. The preparation method of the lamellar graphite carbon-based ruthenium cobalt electrocatalyst provided by the present invention prepares a sheet-like carbon material with abundant macropores and mesopores by electrochemical exfoliation. The preparation method is relatively simple, can reduce production costs, and improve the feasibility of large-scale production. In addition, the method can also ensure the integrity of the electrocatalyst structure and is easy to control the distribution and size of ruthenium cobalt alloy nanoclusters. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a SEM image of a graphite carbon layer during the preparation of a lamellar graphite carbon-based ruthenium-cobalt electrocatalyst in Example 8; Figure 2 is the high-resolution XPS spectrum of Co2p3 / 2 of the lamellar graphite carbon-based ruthenium cobalt electrocatalyst in Example 8; Figure 3 is the adsorption-desorption curve of the lamellar graphite carbon-based ruthenium-cobalt electrocatalyst under nitrogen in Example 8; Figure 4 This is the pore size distribution diagram of the lamellar graphite carbon-based ruthenium cobalt electrocatalyst under nitrogen in Example 8. DETAILED DESCRIPTION
[0018] The embodiments of the present invention will be described in detail below in conjunction with examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer.
[0019] As one aspect of the present invention, the present invention provides a lamellar graphite carbon-based ruthenium cobalt electrocatalyst, which includes a nitrogen-doped porous flaky graphite carbon layer and ruthenium cobalt alloy nanoclusters supported on the graphite carbon layer, and the size of the ruthenium cobalt alloy nanoclusters is less than 8nm.
[0020] Wherein, "porous flake graphite carbon layer" refers to a porous and flake-structured carbon layer formed by graphite. "Ruthenium-cobalt alloy nanoclusters" refers to nanoclusters of an alloy formed by ruthenium and cobalt, which are ultrafine particles of nanometer scale. It should be understood that the size of the above-mentioned ruthenium-cobalt alloy nanoclusters is less than 8nm, but does not include 0.
[0021] The above-mentioned lamellar graphite carbon-based ruthenium cobalt electrocatalyst includes a nitrogen-doped porous flaky graphite carbon layer and a ruthenium cobalt alloy nanocluster supported on the graphite carbon layer. The size of the ruthenium cobalt alloy nanocluster is less than 8nm, and no precious metal is used, thereby greatly reducing the cost and being widely used. In addition, the graphite carbon layer of the electrocatalyst is a porous flaky structure, which can effectively promote long-distance mass transfer and active site exposure, thereby improving the formation efficiency of the solid-liquid-gas reaction interface, and the energy conversion efficiency is higher. The use of ruthenium cobalt alloy nanocluster is higher and more stable than that of a single atom catalyst. The reversible oxygen overpotential of the electrocatalyst is 0.713 V or less for OER / ORR.
[0022] In an optional embodiment, the content of ruthenium in the electrocatalyst is 3wt%-8wt%, the content of cobalt is 3wt%-10wt%, the content of nitrogen is 1wt%-5wt%, and the content of carbon is 77wt%-93wt%. The content of ruthenium is typically but not limited to 3wt%, 4wt%, 5wt%, 6wt%, 7wt% or 8wt%. The content of cobalt is typically but not limited to 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%. The content of nitrogen is typically but not limited to 1wt%, 2wt%, 3wt%, 4wt% or 5wt%. The content of carbon is typically but not limited to 77wt%, 78wt%, 79wt%, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt% or 93wt%. When the content of each element in the electrocatalyst is within the above range, the catalytic activity of the catalyst is higher.
[0023] In an optional embodiment, the electrocatalyst has a specific surface area of 100-2000 m 2 The above specific surface area is typically, but not limited to, 100, 200, 400, 600, 800, 1000, 1200, 1400, 1600, 1800 or 2000 m 2 When the specific surface area of the electrocatalyst is within the above range, the reaction activity is higher and the reaction rate is higher.
[0024] As another aspect of the present invention, the present invention provides a method for preparing a lamellar graphite carbon-based ruthenium cobalt electrocatalyst, comprising the following steps: S1, continuously electrolyzing the graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a flaky carbon material; S2. Mixing the flaky carbon material with a ruthenium source, a cobalt source and a nitrogen source, stirring the mixture, drying the mixture and calcining the mixture in an inert atmosphere to obtain the electrocatalyst.
[0025] For graphitized carbon-based materials, it is still difficult to manufacture a sheet-like open system with a large number of macropores and mesopores. The above-mentioned preparation method of lamellar graphite carbon-based ruthenium cobalt electrocatalyst prepares a sheet-like carbon material with abundant macropores and mesopores by electrochemical exfoliation. The preparation method is relatively simple, which can reduce production costs and improve the feasibility of large-scale production. In addition, the method can also ensure the integrity of the electrocatalyst structure and easily control the distribution and size of ruthenium cobalt alloy nanoclusters.
[0026] In an optional embodiment, in S1, the electrolyte is 0.5 M H 2 SO 4 Aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode, the continuous electrolysis includes: cyclic voltammetry measurement is continuously performed for 70-74 hours, and the scanning potential is 1.0 V~2.5 V; the electrolyte stirring includes: stirring at 75-85°C for 10-14 hours. The above cyclic voltammetry duration is typically but not limited to 70, 70.5, 71, 71.5, 72, 72.5, 73, 73.5 or 74 hours. The scanning potential is typically but not limited to 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5 V. The electrolyte stirring temperature is typically, but not limited to, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, or 85° C. The electrolyte stirring time is typically, but not limited to, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, or 14 h.
[0027] In an optional embodiment, the ruthenium source includes ruthenium chloride, the cobalt source includes cobalt nitrate, and the nitrogen source includes dopamine.
[0028] In an optional embodiment, the mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride, and the cobalt nitrate is (1-1.5): (0.5-1.0): (0.03-1.0): (0.01-1.0). The above mass ratio is typically but not limited to 1:0.5:0.03:0.01, 1:0.8:0.5:0.5, 1:1:1:1, 0.5:0.5:0.03:0.01, 0.5:1:1:1, 1.5:0.5:1.03:0.01, 1.5:0.8:0.5:0.5, 1.5:1:1:1, etc.
[0029] In an optional embodiment, in S2, the mixing and stirring includes: mixing the layered carbon material, the dopamine and Tris-HCl, stirring for 25-35 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 45-50 h. The stirring time after the layered carbon material, dopamine and Tris-HCl are mixed is typically but not limited to 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35 min. The stirring time after adding ruthenium chloride and cobalt nitrate is typically but not limited to 45, 45.5, 46, 46.5, 47, 47.5, 48, 48.5, 49, 49.5 or 50 h. Wherein, Tris-HCl is a buffer solution.
[0030] In an optional embodiment, in S2, the calcination includes: first calcining at 150-250°C for 1.5-2.5h, and then calcining at 850-950°C for 1.5-2.5h. The temperature of the first calcination is typically but not limited to 150, 160, 170, 180, 190, 200, 210, 220, 230, 240 or 250°C, and the time of the first calcination is typically but not limited to 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4 or 2.5 h. The temperature of the second calcination is typically but not limited to 850, 860, 870, 880, 890, 900, 910, 920, 930, 940 or 950°C and the time of the second calcination is typically but not limited to 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4 or 2.5 h.
[0031] Optionally, the inert atmosphere comprises nitrogen or argon.
[0032] As another aspect of the present invention, the present invention provides a battery, comprising an electrode, wherein the electrode comprises the above-mentioned lamellar graphite carbon-based ruthenium cobalt electrocatalyst or the lamellar graphite carbon-based ruthenium cobalt electrocatalyst obtained by the above-mentioned preparation method.
[0033] It should be noted that the focus of the above-mentioned battery of the present invention is the use of the above-mentioned lamellar graphite carbon-based ruthenium cobalt electrocatalyst. As for the specific configuration relationship between the electrodes and other components, the present invention does not make any special restrictions, and any one that can be implemented in the field can be used.
[0034] The present invention is further described in detail below with reference to Examples and Comparative Examples.
[0035] Example 1 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, the electrocatalyst comprising a nitrogen-doped porous lamellar graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 5nm. The content of ruthenium in the electrocatalyst is 7wt%, the content of cobalt is 9wt%, the content of nitrogen is 5wt%, and the content of carbon is 78wt%. The specific surface area of the electrocatalyst is 2000m 2 / g.
[0036] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyzing a graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a lamellar carbon material; wherein the electrolyte is perchloric acid; in the three-electrode system, the graphite rod, carbon paper, and Ag / AgCl electrode are respectively used as a working electrode, a counter electrode, and a reference electrode; the continuous electrolysis includes: cyclic voltammetry measurement is continuously performed for 65 h, and the scanning potential is 1.0 V~2.5 V; the electrolyte stirring includes: stirring at 90°C for 8 h.
[0037] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1.5:1.0:1.0:1.0. The mixing and stirring comprises: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 25 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 45 h. The calcination comprises: first calcining at 150°C for 2 h, and then calcining at 850°C for 2.5 h.
[0038] Example 2 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, which is different from Example 1 in that the content of ruthenium, the content of cobalt, the content of nitrogen, and the content of carbon in the electrocatalyst of this embodiment are 3wt%, 3wt%, 1wt%, and 93wt%. In the preparation process of the electrocatalyst, the mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride, and the cobalt nitrate is 1.2:0.9:0.8:1.0, and the rest is the same as Example 1.
[0039] The content of each element in this embodiment is within the preferred range of the present invention.
[0040] Example 3 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, which is different from Example 1 in that the content of ruthenium in the electrocatalyst of this embodiment is 8wt%, the content of cobalt is 10wt%, the content of nitrogen is 5wt%, and the content of carbon is 77wt%. During the preparation of the electrocatalyst, the mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride, and the cobalt nitrate is 1.3:1.0:0.9:1.0, and the rest is the same as Example 1.
[0041] The content of each element in this embodiment is within the preferred range of the present invention.
[0042] Example 4 A lamellar graphite carbon-based ruthenium cobalt electrocatalyst, which is different from Example 3 in that the specific surface area of the electrocatalyst in this embodiment is 1000m 2 / g.
[0043] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyzing a graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a lamellar carbon material; wherein the electrolyte is perchloric acid; in the three-electrode system, the graphite rod, carbon paper, and Ag / AgCl electrode are respectively used as a working electrode, a counter electrode, and a reference electrode; the continuous electrolysis includes: cyclic voltammetry measurement is continuously performed for 65 h, and the scanning potential is 1.0 V~2.5 V; the electrolyte stirring includes: stirring at 90°C for 8 h.
[0044] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium nitrate, the cobalt source is cobalt chloride, and the nitrogen source is ammonium chloride. The mass ratio of the lamellar carbon material, the ammonium chloride, the ruthenium nitrate and the cobalt chloride is 1.4:1.0:0.7:0.8. The mixing and stirring includes: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 30 minutes; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 48 hours. The calcination includes: first calcining at 150°C for 2 hours, and then calcining at 850°C for 2.5 hours.
[0045] The specific surface area in this embodiment is within the preferred range of the present invention.
[0046] Example 5 A lamellar graphite carbon-based ruthenium cobalt electrocatalyst, which is different from Example 3 in that the specific surface area of the electrocatalyst in this embodiment is 2000m 2 / g.
[0047] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyzing a graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a lamellar carbon material; wherein the electrolyte is phosphoric acid; in the three-electrode system, the graphite rod, carbon paper, and Ag / AgCl electrode are respectively used as a working electrode, a counter electrode, and a reference electrode; the continuous electrolysis includes: cyclic voltammetry measurement is continuously performed for 65 hours, and the scanning potential is 1.0 V to 2.5 V; the electrolyte stirring includes: stirring at 90°C for 8 hours.
[0048] S2, mixing and stirring the sheet carbon material with a ruthenium source, a cobalt source and a nitrogen source, drying, and calcining in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium acetate, the cobalt source is cobalt sulfate, and the nitrogen source is dicyandiamide. The mass ratio of the sheet carbon material, dicyandiamide, ruthenium acetate, and cobalt sulfate is 2:1:2:2. The mixing and stirring includes: mixing the sheet carbon material, dicyandiamide and Tris-HCl, stirring for 4 min; then adding the ruthenium acetate and the cobalt sulfate, and stirring for 45h. The calcining includes: first calcining at 180°C for 2h, and then calcining at 900°C for 1.5h.
[0049] The specific surface area in this embodiment is within the preferred range of the present invention.
[0050] Example 6 A lamellar graphite carbon-based ruthenium cobalt electrocatalyst, which is different from Example 3 in that the specific surface area of the electrocatalyst in this embodiment is 1000m 2 / g.
[0051] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyzing a graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a lamellar carbon material; wherein the electrolyte is acetic acid; in the three-electrode system, the graphite rod, carbon paper, and Ag / AgCl electrode are respectively used as a working electrode, a counter electrode, and a reference electrode; the continuous electrolysis includes: cyclic voltammetry measurement is continuously performed for 65 hours, and the scanning potential is 1.0 V~2.5 V; the electrolyte stirring includes: stirring at 90°C for 8 hours.
[0052] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium nitrate, the cobalt source is cobalt sulfate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium nitrate and the cobalt sulfate is 1.3:1:0.7:0.6. The mixing and stirring includes: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 30 minutes; then adding the ruthenium nitrate and the cobalt sulfate, and stirring for 50 hours. The calcination includes: first calcining at 250°C for 2 hours, and then calcining at 850°C for 2 hours.
[0053] The specific surface area in this embodiment is within the preferred range of the present invention.
[0054] Example 7 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, wherein the size of the ruthenium-cobalt alloy nanoclusters in the electrocatalyst is 3 nm. Different from Example 6, the electrocatalyst of this embodiment is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 12 hours.
[0055] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1.4:0.5:0.8:0.8. The mixing and stirring includes: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 30 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 18 h. The calcination includes: first calcining at 200°C for 2 h, and then calcining at 900°C for 2 h.
[0056] The catalyst parameters and preparation process parameters of this embodiment are all within the preferred range of the present invention.
[0057] Example 8 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, the electrocatalyst comprising a nitrogen-doped porous flaky graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 5nm. The content of ruthenium in the electrocatalyst is 8wt%, the content of cobalt is 5wt%, the content of nitrogen is 2wt%, and the content of carbon is 85wt%. The specific surface area of the electrocatalyst is 130m 2 / g.
[0058] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 12 hours.
[0059] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry them, and calcine them in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1:0.6:0.8:0.7. The mixing and stirring comprises: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 30 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 48 h. The calcination comprises: first calcining at 200°C for 2h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2h.
[0060] Example 9 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, the electrocatalyst comprising a nitrogen-doped porous lamellar graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 8nm. The content of ruthenium in the electrocatalyst is 5wt%, the content of cobalt is 7wt%, the content of nitrogen is 4wt%, and the content of carbon is 84wt%. The specific surface area of the electrocatalyst is 114m 2 / g.
[0061] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 12 hours.
[0062] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry them, and calcine them in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1:0.5:0.1:0.2. The mixing and stirring includes: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 35 minutes; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 48 hours. The calcination includes: first calcining at 200°C for 2 hours, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2 hours.
[0063] Example 10 A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, the electrocatalyst comprising a nitrogen-doped porous flaky graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 4 nm. The content of ruthenium in the electrocatalyst is 1 wt%, the content of cobalt is 7 wt%, the content of nitrogen is 8 wt%, and the content of carbon is 84 wt%. The specific surface area of the electrocatalyst is 140 m 2 / g.
[0064] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 18 hours.
[0065] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry them, and calcine them in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1:0.6:0.08:0.1. The mixing and stirring comprises: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 35 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 48 h. The calcination comprises: first calcining at 200°C for 2h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2h.
[0066] Comparative Example 1 A catalyst comprising a nitrogen-doped porous flaky graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 10 nm. The catalyst contains 10 wt% ruthenium, 15 wt% cobalt, 7 wt% nitrogen and 68 wt% carbon. The catalyst has a specific surface area of 2500 m 2 / g.
[0067] The size of the ruthenium-cobalt alloy nanoclusters in this comparative example is not within the scope of the present invention.
[0068] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 18 hours.
[0069] S2. Mix and stir the lamellar carbon material with a ruthenium source, a cobalt source and a nitrogen source, dry them, and calcine them in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, the cobalt source is cobalt nitrate, and the nitrogen source is dopamine. The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is 1:0.3:0.02:0.1. The mixing and stirring comprises: mixing the lamellar carbon material, the dopamine and Tris-HCl, stirring for 50 minutes; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 10 hours. The calcination comprises: first calcining at 500°C for 2 hours, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2 hours.
[0070] Comparative Example 2 A catalyst comprises a porous flaky graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 5 nm. The content of ruthenium in the catalyst is 10 wt %, the content of cobalt is 15 wt %, and the content of carbon is 75 wt %. The specific surface area of the catalyst is 500 m 2 / g.
[0071] The graphite carbon layer in this comparative example was not doped with nitrogen.
[0072] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 18 hours.
[0073] S2. Mix and stir the lamellar carbon material with a ruthenium source and a cobalt source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, and the cobalt source is cobalt nitrate. The mass ratio of the lamellar carbon material, the ruthenium chloride, and the cobalt nitrate is 1:1:0.5. The mixing and stirring comprises: mixing the lamellar carbon material and Tris-HCl, stirring for 60 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 10 h. The calcination comprises: first calcining at 500°C for 2 h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2 h.
[0074] Comparative Example 3 A catalyst comprising a ruthenium-cobalt alloy nanocluster supported on a nitrogen-doped porous non-graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is 5 nm. The catalyst contains 10 wt% ruthenium, 15 wt% cobalt, 7 wt% nitrogen and 68 wt% carbon. The catalyst has a specific surface area of 400 m 2 / g.
[0075] The carbon layer in this comparative example is not a graphite carbon layer.
[0076] The electrocatalyst is prepared by the following method, comprising the following steps: The sheet carbon material is mixed with a nitrogen source, a ruthenium source, and a cobalt source, and then dried and calcined in a nitrogen atmosphere to obtain the electrocatalyst. The carbon material is activated carbon, the nitrogen source is dopamine, the ruthenium source is ruthenium chloride, and the cobalt source is cobalt nitrate. The mass ratio of the carbon material, the dopamine, the ruthenium chloride, and the cobalt nitrate is 1:1.5:0.5:0.7. The mixing and stirring includes: mixing the carbon material, the dopamine, and Tris-HCl, stirring for 60 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 10 h. The calcination includes: first calcining at 300°C for 2h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2h.
[0077] Comparative Example 4 A catalyst comprising a nitrogen-doped porous flaky graphite carbon layer and metal ruthenium and metal cobalt supported on the graphite carbon layer. The catalyst has a ruthenium content of 10wt%, a cobalt content of 15wt%, a nitrogen content of 7wt%, and a carbon content of 68wt%. The catalyst has a specific surface area of 2500m 2 / g.
[0078] In this comparative example, metal ruthenium and metal cobalt are supported on the graphite carbon layer.
[0079] The electrocatalyst is prepared by the following method, comprising the following steps: S1. Continuously electrolyze the graphite rod in a three-electrode electrolytic cell, stir the electrolyte, centrifuge, wash, and dry to obtain a flaky carbon material; wherein the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 72 hours, and a scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 80° C. for 18 hours.
[0080] S2. Mix and stir the lamellar carbon material with a ruthenium source and a cobalt source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, and the cobalt source is cobalt nitrate. The mass ratio of the lamellar carbon material, the ruthenium chloride, and the cobalt nitrate is 1:1:0.5. The mixing and stirring comprises: mixing the lamellar carbon material and Tris-HCl, stirring for 60 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 10 h. The calcination comprises: first calcining at 500°C for 2 h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 2 h.
[0081] Comparative Example 5 A catalyst comprising nitrogen-doped porous graphite carbon and ruthenium-cobalt alloy nanoclusters supported on the graphite carbon, wherein the size of the ruthenium-cobalt alloy nanoclusters is 5 nm. The content of ruthenium in the catalyst is 10 wt %, the content of cobalt is 15 wt %, the content of nitrogen is 7 wt %, and the content of carbon is 68 wt %. The specific surface area of the catalyst is 2500 m 2 / g.
[0082] The graphite carbon in this comparative example does not have a flaky structure.
[0083] The electrocatalyst is prepared by the following method, comprising the following steps: S1. PVP, ammonium chloride and melamine were mixed and ground, and calcined in a muffle furnace at 500°C for 2h, and then heated to 900°C at a heating rate of 5°C / min, and calcined at 900°C for 2h to obtain a carbon material. S2. Mix and stir the carbon material with a ruthenium source and a cobalt source, dry, and calcine in a nitrogen atmosphere to obtain the electrocatalyst. Wherein, the ruthenium source is ruthenium chloride, and the cobalt source is cobalt nitrate. The mass ratio of the carbon material, the ruthenium chloride, and the cobalt nitrate is 1:1:0.5. The mixing and stirring includes: mixing the lamellar carbon material and Tris-HCl, stirring for 60 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 10 h. The calcination includes: first calcining at 200°C for 2h, then heating to 900°C at a heating rate of 5°C / min, and calcining at 900°C for 4h.
[0084] Performance test method: 5 mg catalyst, 5 ml ethanol, and 30 ul (5.0 wt%) nafion were mixed, and the mixture was ultrasonically treated for 30 min to obtain the corresponding uniform catalyst ink. Then, the prepared ink was dropped onto a rotating disk electrode (RDE, 0.19625 / cm 2 ) with a loading of 0.6 mg / cm 2 . OER / ORR tests were performed on a typical three-electrode system. 2 / N 2 In saturated KOH solution, the linear sweep voltammetry (LSV) method was used, with the RDE electrode, graphite rod electrode and Hg / HgO electrode as the working electrode, counter electrode and reference electrode, respectively. 2 The potential (E j10 , OER) and ORR half-wave potential (E 1 / 2 ,ORR) to obtain the reversible oxygen overpotential.
[0085] In addition, from Figure 1-Figure 4It can be seen that the lamellar graphite carbon-based ruthenium cobalt electrocatalyst described in Example 8 has the desired microstructure.
[0086] Figure 1 The SEM image of the carbon material shows that its morphology is a porous sheet array morphology.
[0087] Figure 2 The XPS diagram of the catalyst shows two peaks in the high-resolution XPS spectrum of Co 2p3 / 2, corresponding to Co02p3 / 2 and Co2 + 2p3 / 2 state.
[0088] Figure 3 The nitrogen adsorption and desorption curve of the catalyst is shown in Figure 2. The specific surface area of the catalyst is calculated to be 130 m 2 / g.
[0089] Figure 4 The pore size distribution diagram of the catalyst shows that the catalyst contains mesopores and macropores.
[0090] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.
Claims
1. A lamellar graphite carbon-based ruthenium-cobalt electrocatalyst, It is characterized in that The electrocatalyst comprises a nitrogen-doped porous flaky graphite carbon layer and a ruthenium-cobalt alloy nanocluster supported on the graphite carbon layer, wherein the size of the ruthenium-cobalt alloy nanocluster is less than 8 nm.
2. The lamellar graphite carbon-based ruthenium-cobalt electrocatalyst according to claim 1, It is characterized in that The electrocatalyst has a ruthenium content of 3wt%-8wt%, a cobalt content of 3wt%-10wt%, a nitrogen content of 1wt%-5wt%, and a carbon content of 77wt%-93wt%.
3. The lamellar graphite carbon-based ruthenium-cobalt electrocatalyst according to claim 1 or 2, It is characterized in that The specific surface area of the electrocatalyst is 100-2000m 2 / g.
4. A method for preparing the lamellar graphite carbon-based ruthenium-cobalt electrocatalyst according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1, continuously electrolyzing the graphite rod through a three-electrode electrolytic cell, stirring the electrolyte, centrifuging, washing, and drying to obtain a flaky carbon material; S2. Mixing the flaky carbon material with a ruthenium source, a cobalt source and a nitrogen source, stirring the mixture, drying the mixture and calcining the mixture in an inert atmosphere to obtain the electrocatalyst.
5. The preparation method according to claim 4, It is characterized in that In S1, the electrolyte is 0.5 M H 2 SO 4 aqueous solution; in a three-electrode system, a graphite rod, a carbon paper and an Ag / AgCl electrode are respectively used as a working electrode, a counter electrode and a reference electrode; the continuous electrolysis comprises: cyclic voltammetry measurement is continuously performed for 70-74 hours, and the scanning potential is 1.0 V to 2.5 V; the electrolyte stirring comprises: stirring at 75-85° C. for 10-14 hours.
6. The preparation method according to claim 4, It is characterized in that The ruthenium source includes ruthenium chloride, the cobalt source includes cobalt nitrate, and the nitrogen source includes dopamine.
7. The preparation method according to claim 6, It is characterized in that The mass ratio of the lamellar carbon material, the dopamine, the ruthenium chloride and the cobalt nitrate is (1-1.5): (0.5-1.0): (0.03-1.0): (0.01-1.0).
8. The preparation method according to claim 6, It is characterized in that In S2, the mixing and stirring comprises: mixing the layered carbon material, the dopamine and Tris-HCl, and stirring for 25-35 min; then adding the ruthenium chloride and the cobalt nitrate, and stirring for 45-50 h.
9. The preparation method according to any one of claims 4 to 8, It is characterized in that In S2, the calcination includes: first calcining at 150-250°C for 1.5-2.5h, and then calcining at 850-950°C for 1.5-2.5h.
10. A battery, It is characterized in that It comprises an electrode, wherein the electrode comprises the lamellar graphite carbon-based ruthenium-cobalt electrocatalyst described in any one of claims 1-3 or the lamellar graphite carbon-based ruthenium-cobalt electrocatalyst obtained by the preparation method described in any one of claims 4-9.
Citation Information
Patent Citations
Pt-Ru alloy nano electro-catalyst having doped graphene carrier and preparation method thereof
CN103816894A
Composite material of nitrogen doped three-dimensional graphene supported nano silver and preparation method thereof
CN107248581A
Oxygen and nitrogen doped carbon coated ruthenium-M alloy nanoparticle catalyst and preparation method and application method thereof
CN116121770A
Supported nano ruthenium-based catalyst as well as preparation method and application thereof
CN118594582A
A method in order to generate graphene based electrode
WO2017171682A2