Organic material-based ultraviolet photoelectric detector and preparation method thereof
Through the design of ultraviolet photodetectors based on organic materials and the combination of polymer donors and organic acceptors, the response ability to the visible blind ultraviolet region is improved, the problems of weak response and high cost in the existing technology are solved, and the Improved sensitivity and portability.
Patent Information
- Application Number
- CN202411180176.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-18
AI Technical Summary
Existing ultraviolet photodetectors have weak response when detecting the visible blind ultraviolet region, are easily affected by the external environment, and have high preparation costs and large volumes, which limits their application scenarios.
Using an ultraviolet photodetector based on organic materials, including a transparent rigid substrate, a bottom electrode, an electron transmission layer, a modification layer, a photoactive layer and a top electrode, the photoelectric conversion efficiency is improved through a reasonable combination of polymer donors and organic acceptors. , reduce the use of silicon, reduce equipment cost and volume.
It improves the response and sensitivity of the ultraviolet photodetector to the visible blind ultraviolet region, reduces the influence of the external environment, realizes a compact and portable structure, expands the use scenarios, simplifies the preparation process, and reduces the cost.
Smart Images

Figure CN118804609A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultraviolet light detectors, and in particular to an ultraviolet photoelectric detector based on organic materials and a preparation method thereof. Background Art
[0002] Ultraviolet sensing equipment plays a key role in multiple industries and is widely used in the medical field, semiconductor microchip manufacturing field, environmental monitoring field, etc. Ultraviolet sensing equipment can help people understand the intensity of ultraviolet rays by detecting and measuring the intensity of ultraviolet rays in sunlight, and then take protective measures or apply them.
[0003] UV sensors can be divided into photochromic sensors and photodetectors according to different detection principles, which are the main equipment for UV light detection and measurement. Among them, photochromic sensors have poor repeatability, low instantaneous response intensity, and are insensitive to weak light signal changes, which will affect the accuracy of the measurement results, which limits their application in situations requiring high-precision measurements.
[0004] Ultraviolet photodetectors are considered an important part of modern optoelectronic technology. They convert ultraviolet light signals into electrical signals to detect ultraviolet radiation levels. Ultraviolet photodetectors are not easily affected by long-wavelength electromagnetic interference and have good concealment. Therefore, ultraviolet photodetectors have unique advantages in space detection and military applications. In daily life, ultraviolet photodetectors can also accurately detect the intensity and dosage of ultraviolet radiation in technical processes such as sterilization, water purification, environmental monitoring, UV curing, etc., and provide data reference.
[0005] Current research on ultraviolet rays is mainly focused on invisible radiation areas other than blue light. There are three main invisible areas of ultraviolet radiation, namely: UVC (200-280nm) radiation spectrum area, UVB (280-320nm) radiation spectrum area and UVA (320-400nm) radiation spectrum area. Since this part of ultraviolet radiation cannot be observed with the naked eye, it is necessary to use ultraviolet photoelectric detectors to observe it, especially the monitoring of the UVA radiation spectrum area: The UVA radiation spectrum area (visible blind area) is also called long-wave dark spot effect ultraviolet rays. More than 98% of UVA in sunlight can penetrate the ozone layer and clouds to reach the earth's surface. UVA can directly affect the human skin layer, destroy the elastic fibers and collagen fibers in the skin, make the skin color darker and aged, and long-term exposure to the sun also has the risk of causing skin cancer.
[0006] Common ultraviolet photodetectors on the market mainly include photomultiplier ultraviolet photodetectors and silicon (Si)-based ultraviolet photodetectors. Although photomultiplier ultraviolet photodetectors have the advantages of large photosensitivity area and fast response speed, they are bulky, costly to prepare and sensitive to temperature, which limits their use in many application scenarios. Compared with photomultiplier ultraviolet photodetectors, silicon-based ultraviolet photodetectors have a mature preparation process, good adaptability and wider application. However, the band gap of silicon, the material used to prepare silicon-based ultraviolet photodetectors, is relatively small, which is more conducive to visible light response but not to ultraviolet light response. Therefore, additional filters and packaging technology are required to reduce the wide spectral absorption of silicon, which will increase the preparation cost of silicon-based ultraviolet photodetector equipment and increase the size of the equipment. Not only that, during use, researchers also found that the low resistance characteristics of raw material silicon under high temperature and high pressure will also cause the performance of silicon-based ultraviolet photodetectors to decrease.
[0007] In summary, it can be seen that the ultraviolet photodetectors currently on the market are relatively easily affected by the external environment to a certain extent. In addition, the limitations of the raw material properties affect the use of ultraviolet photodetectors. Therefore, there is an urgent need for an ultraviolet photodetector that can detect the visible-blind ultraviolet light region. It can not only reduce the impact of the external environment on the ultraviolet photodetector, improve the sensitivity and accuracy of detection in the visible-blind ultraviolet light region, but also has a small and portable structural characteristics, reducing the limitations of the external environment and expanding its usage scenarios. Summary of the invention
[0008] The object of the present invention is to provide an ultraviolet photodetector based on organic materials;
[0009] Another object of the present invention is to provide a method for preparing an ultraviolet photodetector based on organic materials.
[0010] The technical solution adopted to achieve the purpose of the present invention is:
[0011] An ultraviolet photodetector based on organic materials, which may also be referred to as an organic ultraviolet photodetector, includes a transparent rigid substrate, a bottom electrode, an electron transport layer, a modification layer, a photoactive layer, a hole transport layer and a top electrode arranged from bottom to top; or a transparent rigid substrate, a bottom electrode, a hole transport layer, a photoactive layer, an electron transport layer and a top electrode arranged from bottom to top.
[0012] Furthermore, the photoactive layer is a thin film formed by blending a polymer donor and an organic acceptor, wherein the polymer donor includes but is not limited to PBDB-T, PM6, and D18, and the organic acceptor is mainly a non-fullerene acceptor that absorbs ultraviolet light;
[0013] Further, the organic acceptor includes but is not limited to F-2F, CH-4F, CH-4Cl, CH17, Y6;
[0014] Further, the polymer donor is PM6, and the organic acceptor is CH-4F;
[0015] Furthermore, the mass ratio of the polymer donor to the organic acceptor is 1:1-1:100, so as to achieve absorption of light of different wavelengths by the photoactive layer, thereby improving the overall performance of the device;
[0016] Furthermore, the mass ratio of the polymer donor to the organic acceptor is 1:1;
[0017] Furthermore, the photoactive layer has a thickness of 10 nm-200 nm.
[0018] Furthermore, the transparent rigid substrate includes but is not limited to a quartz plate or other highly transparent rigid substrate with a transmittance of more than 90% to ultraviolet light;
[0019] Furthermore, the transparent rigid substrate is a quartz plate.
[0020] Furthermore, the bottom electrode includes but is not limited to indium tin oxide, metal nanowires, carbon nanotubes, conductive polymers, metal grids, graphene, and PH1000.
[0021] Furthermore, the top electrode includes, but is not limited to, silver, gold, lithium, calcium, strontium, barium, indium, magnesium, aluminum, and copper.
[0022] Furthermore, the electron transport layer is one or more of ZnO nanoparticles, ZnO nanocrystals, TiO2, SnO2, WO3, PDINO, and PNDIT-F3N.
[0023] Furthermore, the hole transport layer includes but is not limited to MoO3, PEDOT:PSS, CuO x 、WO3、NiO x , SAM-2PACz.
[0024] By using different types of electron transport layers and hole transport layers, the leakage current of the organic ultraviolet photodetector can be adjusted, thereby improving the dark current of the organic photodetector under the working bias and enhancing the detection capability of the organic photodetector.
[0025] Furthermore, the modification layer includes but is not limited to PFN-Br, PEIE, and PFN / PFBT.
[0026] The organic ultraviolet photodetector prepared from the above materials selects a transparent rigid substrate with high light transmittance, which can improve the responsiveness of the ultraviolet photodetector to the visible blind ultraviolet light region. The photoactive layer can improve the photoelectric conversion efficiency of the ultraviolet photodetector through the reasonable combination of polymer donors and organic acceptors. At the same time, it can also avoid the problem of detector performance degradation due to the influence of raw silicon in silicon-based ultraviolet photodetectors.
[0027] Furthermore, a method for preparing an ultraviolet photodetector based on organic materials is provided, which specifically comprises the following steps:
[0028] S1. Preparation of transparent rigid substrate:
[0029] The transparent rigid substrate is ultrasonically cleaned with glass cleaning liquid, deionized water, acetone, and isopropanol in sequence, and then the surface of the transparent rigid substrate is blown dry with a nitrogen gun, irradiated in a UV ozone treatment device, and placed in a glass culture dish for later use;
[0030] Furthermore, the transparent rigid substrate is a quartz sheet;
[0031] Further, irradiation was performed in a UV-ozone treatment device for 15 min;
[0032] S2. Preparation of bottom electrode:
[0033] The prepared bottom electrode solution is spin-coated onto a transparent rigid substrate, and an annealing treatment is performed to obtain a bottom electrode;
[0034] Further, the spin coating speed was 2000 rpm;
[0035] Further, the annealing conditions are: annealing at 130°C for 0.5 hours;
[0036] S3. Preparation of hole transport layer:
[0037] The hole transport layer material is mixed and diluted with deionized water, fully dispersed by ultrasound, filtered using a filter membrane, and spin-coated on the bottom electrode, and annealed to obtain the hole transport layer;
[0038] Further, the hole transport layer material is mixed and diluted with deionized water in a ratio of 1:1;
[0039] Further, the filter membrane is a PES 0.45 micron pore size filter membrane;
[0040] Further, the annealing conditions are: annealing at 150° C. for 0.5 hours;
[0041] S4. Preparation of photoactive layer:
[0042] The polymer donor and the organic acceptor are dissolved in a chloroform solvent at a mass ratio of 1:1-1:100, the prepared solution is spin-coated on the hole transport layer, and a photoactive layer is obtained after annealing;
[0043] Further, the polymer donor and the organic acceptor are dissolved in a chloroform solvent at a mass ratio of 1:1-1:100, dissolved at 45° C. for 5 hours and then spin-coated, with a spin-coating speed of 2000 rpm;
[0044] Further, the annealing condition is annealing at 100° C. for 10 minutes;
[0045] S5. Preparation of electron transport layer:
[0046] The electron transport layer is dissolved in methanol, and after stirring, the prepared solution is spin-coated on the active layer to obtain the electron transport layer;
[0047] Further, 2 g of the electron transport layer was dissolved in 2 mL of methanol, and after stirring for 6 hours, the prepared solution was spin-coated on the active layer at 3000 rpm to obtain the electron transport layer;
[0048] S6. Evaporation of top electrode:
[0049] Vapor depositing a top electrode on the electron transport layer to obtain the ultraviolet photodetector;
[0050] Furthermore, the thickness of the evaporated top electrode is 200 nm.
[0051] Based on the above preparation method, a modification layer can be added between the electron transport layer and the photoactive layer as needed.
[0052] Furthermore, due to the characteristics of organic ultraviolet photodetectors such as light weight, good flexibility and good biocompatibility, organic ultraviolet photodetectors can be used to prepare wearable products.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] 1. In order to increase the application scope of photoelectric detectors, the present application provides an ultraviolet photodetector based on organic materials. The ultraviolet photodetector based on organic materials can produce a photoelectric response to the visible blind ultraviolet region, thereby improving the universality of the ultraviolet photodetector in the visible blind ultraviolet region and reducing the impact of the external environment on the ultraviolet photodetector, so that it not only has good responsiveness but also has high sensitivity, and can be promoted in scientific research, military, medical and other fields; and the organic materials used in the ultraviolet photodetector based on organic materials have the advantages of simple production process, adjustable structure, strong solubility, good mechanical flexibility, light weight and low cost, which improves the complex preparation process and high energy consumption of existing inorganic ultraviolet photodetectors.
[0055] 2. In the present application, the polymer donor and the organic acceptor are rationally matched to prepare a photoactive layer with good properties, thereby improving the response capability of the photodetector to the visible-blind ultraviolet region, overcoming the shortcoming of the weak response of the traditional silicon detector in the visible-blind ultraviolet region, and developing an ultraviolet photodetector that meets the needs through simple preparation technology.
[0056] 3. Ultraviolet photodetectors based on organic materials have smaller mass and better plasticity, making them more suitable for making large-scale devices and can also be used in wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 This is a schematic diagram of the vertical structure of the organic ultraviolet photodetector prepared in Example 1 of the present invention;
[0058] Figure 2 The external quantum efficiency diagram of the organic ultraviolet photodetector of the present invention and the commercial Si-based ultraviolet photodetector;
[0059] Figure 3 Spectral responsivity diagram of the organic ultraviolet photodetector of the present invention and the commercial Si-based ultraviolet photodetector;
[0060] Figure 4 JV curves of the organic ultraviolet photodetector prepared in Example 1 of the present invention and the commercial Si-based ultraviolet photodetector in the dark state;
[0061] Figure 5 This is a diagram of the external quantum efficiency of the organic ultraviolet photodetector and the organic photodetector prepared in Example 1 of the present invention;
[0062] Figure 6 Spectral responsivity diagram of the organic ultraviolet photodetector and the organic photodetector prepared in Example 1 of the present invention;
[0063] Figure 7 The response current curves of the organic ultraviolet photodetector prepared in Example 1 of the present invention and the commercial Si-based ultraviolet photodetector to 365nm ultraviolet light. DETAILED DESCRIPTION
[0064] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0066] The ultraviolet photodetector based on organic materials involved in the embodiments of the present application is referred to as an organic ultraviolet photodetector for short.
[0067] Example 1 Preparation of organic ultraviolet photodetector PM6:CH-4F
[0068] S1. Preparation of transparent rigid substrate:
[0069] The quartz plate was ultrasonically cleaned with glass cleaning liquid, deionized water, acetone, and isopropanol in sequence, the surface of the quartz plate was blown dry with a nitrogen gun, irradiated in a UV ozone treatment device for 15 minutes, and placed in a glass culture dish for later use;
[0070] S2. Preparation of bottom electrode:
[0071] The prepared bottom electrode solution PH1000 solution (5% DMSO + 0.5% FS-30) was spin-coated onto a transparent rigid substrate at 2000 rpm, and annealed at 130° C. for 0.5 hours to obtain a bottom electrode after annealing.
[0072] S3. Preparation of hole transport layer:
[0073] The hole transport layer material PEDOT:PSS was mixed and diluted with deionized water in a ratio of 1:1, and after being fully dispersed by ultrasound, it was filtered using a PES 0.45 μm pore size filter membrane, and then spin-coated on the bottom electrode PH1000, and annealed at 150°C for 0.5 hours to obtain a hole transport layer after annealing.
[0074] S4. Preparation of photoactive layer:
[0075] PM6:CH-4F was dissolved in chloroform solvent at a mass ratio of 1:1 to obtain a solution concentration of 6 mg / mL, and dissolved at 45°C for 5 hours; the prepared solution was spin-coated on the hole transport layer at 2000 rpm and annealed at 100°C for 10 minutes to obtain a PM6:CH-4F photoactive layer;
[0076] S5. Preparation of electron transport layer:
[0077] 2 g of PNDIT-F3N was dissolved in 2 mL of methanol, and after stirring for 6 h, the prepared solution was spin-coated onto the active layer at 3000 rpm to obtain an electron transport layer;
[0078] S6. Evaporation of top electrode:
[0079] A 200nm top electrode Ag layer was evaporated on the electron transport layer to obtain an organic ultraviolet photodetector PM6:CH-4F, whose structure is as follows: Figure 1 shown.
[0080] Example 2 Preparation of organic ultraviolet photodetector PM6:F-2F
[0081] The same preparation method as in Example 1 was used, except that the photoactive layer was replaced with PM6:F-2F to prepare an organic ultraviolet photodetector PM6:F-2F.
[0082] Example 3 Preparation of organic ultraviolet photodetector PM6:CH-4Cl
[0083] The same preparation method as in Example 1 was used, except that the photoactive layer was replaced with PM6:CH-4Cl to prepare an organic ultraviolet photodetector PM6:CH-4Cl.
[0084] Example 4 Preparation of organic ultraviolet photodetector D18:CH-4F
[0085] The preparation method is the same as that in Example 1, except that the photoactive layer is replaced with D18:CH-4F to prepare an organic ultraviolet photodetector D18:CH-4F.
[0086] Example 5 Preparation of organic ultraviolet photodetector PBDB-T:CH-4F
[0087] The preparation method is the same as that in Example 1, except that the photoactive layer is replaced with PBDB-T:CH-4F to prepare an organic ultraviolet photodetector PBDB-T:CH-4F.
[0088] Example 6 Preparation of organic ultraviolet photodetector PCE-10:CH-4F
[0089] The same preparation method as in Example 1 was used, except that the photoactive layer was replaced with PCE-10:CH-4F to prepare an organic ultraviolet photodetector PCE-10:CH-4F.
[0090] Example 7 Preparation of Organic Photodetector PM6:CH-4F
[0091] The organic photodetector PM6:CH-4F was prepared in the same manner as in Example 1, except that the transparent rigid substrate was replaced with a glass substrate.
[0092] Example 8 Performance Test of Organic Ultraviolet Photodetector
[0093] The performance of the organic ultraviolet photodetector prepared by Examples 1-6 and the commercial silicon-based ultraviolet photodetector model OA3011-T purchased from OAROS Photonics Research Institute were tested.
[0094] The test results are as follows Figure 2 , 3 , 4 are respectively the EQE (external quantum efficiency) test, dark current test, and response calculation results of the organic ultraviolet photodetector and the purchased commercial silicon-based ultraviolet photodetector. The dark current test results of the commercial Si-based ultraviolet photodetector and the organic ultraviolet photodetector under different reverse bias voltages are shown in Table 1 below. The response / recovery time of the commercial Si-based ultraviolet photodetector and the organic ultraviolet photodetector to 365nm ultraviolet light is shown in Table 2 below:
[0095] Table 1 Dark current of commercial Si-based UV photodetectors and organic UV photodetectors at different reverse bias voltages
[0096]
[0097] Table 2 Response / recovery time of commercial Si-based UV photodetectors and organic UV photodetectors to 365 nm UV light
[0098]
[0099]
[0100] First, from Figure 2 and 3 It can be seen that the EQE of organic UV photodetectors PM6:CH-4F, PM6:CH-4Cl, D18:CH-4F and PBDB-T:CH-4F in the visible-blind UV region are all greater than 50%, and their responsivity is greater than 0.2A / W, which is significantly better than the commercial Si-based UV photodetectors currently on the market; the EQE of organic UV photodetectors PM6:F-2F and PCE-10:CH-4F in the visible-blind UV region are both greater than 40%, and the responsivity is greater than 0.1A / W, which is comparable to the performance of commercial Si-based UV photodetectors.
[0101] Figure 4 The JV curve of the organic UV photodetector in the dark state is shown. Combined with the data in Table 1 and Table 2, it can be seen that:
[0102] The test results of the organic UV photodetector PM6:F-2F are as follows: under -1V reverse bias, the dark current of OPD is -160nA; under -0.1V reverse bias, the dark current of OPD is -23nA; under no bias, the dark current of OPD is 50pA; the rise time t rise and the fall time t fall It is 116.7 / 206.6ns.
[0103] The test results of the organic UV photodetector PM6:CH-4Cl are as follows: under -1V reverse bias, the dark current of OPD is -260nA; under -0.1V reverse bias, the dark current of OPD is -46.6nA; under no bias, the dark current of OPD is 15pA; the rise time t rise and the fall time t fall It is 58.1 / 69.2ns.
[0104] The test results of the organic UV photodetector PM6:CH-4F are as follows: under -1V reverse bias, the dark current of OPD is -140nA; under -0.1V reverse bias, the dark current of OPD is -14nA; under no bias, the dark current of OPD is 25pA; the rise time t rise and the fall time t fall It is 30.5 / 80.5ns.
[0105] The test results of the organic UV photodetector D18:CH-4F are as follows: under -1V reverse bias, the dark current of OPD is -15μA; under -0.1V reverse bias, the dark current of OPD is -210nA; under no bias, the dark current of OPD is 35pA; the rise time t rise and the fall time t fall It is 46.5 / 60.5ns.
[0106] The test results of the organic ultraviolet photodetector PBDB-T:CH-4F are as follows: under -1V reverse bias, the dark current of OPD is -2.8μA; under -0.1V reverse bias, the dark current of OPD is -40nA; under no bias, the dark current of OPD is 20pA; the rise time t rise and the fall time t fall It is 34.2 / 56.6ns.
[0107] The test results of the organic UV photodetector PCE-10:CH-4F are as follows: under -1V reverse bias, the dark current of OPD is -4.4μA; under -0.1V reverse bias, the dark current of OPD is -205nA; under no bias, the dark current of OPD is 400pA. The rise time t rise and the fall time t fall It is 304.5 / 433.8ns.
[0108] For the combination selection between different donors and acceptors, it is necessary to follow the energy level offset between the donor and the acceptor, and ΔEHOME and ΔELUME must be 0.3~0.5eV. Through performance test analysis, it can be seen that the prepared organic ultraviolet photodetectors PM6:CH-4Cl, PM6:CH-4F, D18:CH-4F and PBDB-T:CH-4F all meet the requirements, while the organic ultraviolet photodetectors PM6:F-2F and PCE-10:CH-4F cannot meet the requirements. The large energy level offset between the donor and the acceptor leads to low responsiveness and long response time.
[0109] Organic ultraviolet photodetectors PM6:CH-4Cl, PM6:CH-4F, D18:CH-4F and PBDB-T:CH-4F performed well in performance tests, overcoming the shortcomings of weak response of traditional silicon detectors in the visible-blind ultraviolet region. They have high ultraviolet photoelectric response and meet the needs of ultraviolet photoelectric detection devices in many fields such as ultraviolet communication, detection and early warning.
[0110] Example 9 Performance test comparison between organic ultraviolet photodetector PM6:CH-4F and organic photodetector PM6:CH-4F
[0111] The organic ultraviolet photodetector PM6:CH-4F and the organic photodetector PM6:CH-4F differ only in the selection of the transparent rigid substrate in the preparation method. The transparent rigid substrate selected by the organic ultraviolet photodetector PM6:CH-4F is a quartz sheet, and the transparent rigid substrate selected by the organic photodetector PM6:CH-4F is glass. The EQE and responsivity of the organic ultraviolet photodetector PM6:CH-4F and the organic photodetector PM6:CH-4F are tested, and the test results are as follows: Figure 5 , 6 shown.
[0112] By comparison Figure 5 and Figure 6 The results show that in the visible blind ultraviolet region, the EQE value of the organic ultraviolet photodetector PM6:CH-4F is significantly higher than that of the organic photodetector PM6:CH-4F, and the responsivity of the organic ultraviolet photodetector PM6:CH-4F in the visible blind ultraviolet region is also significantly better than that of the organic photodetector PM6:CH-4F. Through analysis, it can be seen that compared with the organic photodetector PM6:CH-4F, although the organic photodetector has shown good performance in the photoelectric detection process, it cannot meet the detection requirements for the visible blind ultraviolet region. Compared with them, the organic ultraviolet photodetector can meet more detection requirements and has greater research and development space in the fields of materials science and optoelectronic technology.
[0113] Example 10 Performance test comparison of organic ultraviolet photodetector PM6:CH-4F and commercial Si-based ultraviolet photodetector
[0114] pass Figure 2-4 , as well as Table 1 and Table 2 in Example 8, it can be seen that the test results of the silicon-based ultraviolet photodetector are -910pA under -1V reverse bias; -630pA under -0.1V reverse bias; -2pA under no bias; good light absorption efficiency is exhibited in the wavelength range of 320-400nm in the visible blind ultraviolet region, and the responsivity is greater than 0.1A / W; the rise time t rise and the fall time t fall It is 30.3 / 33.3ns.
[0115] However, organic UV photodetectors are superior to silicon-based UV photodetectors in performance, especially at the same wavelength, organic UV photodetectors have higher responsivity. On this basis, we further take the organic UV photodetector PM6:CH-4F as an example, and draw the response current curve based on the photoelectron conversion data obtained by testing it under 365nm UV light with commercial silicon-based UV photodetectors, as shown in the figure. Figure 7 shown.
[0116] from Figure 7 It can be seen that the photocurrent generated by the organic ultraviolet photodetector PM6:CH-4F under ultraviolet light of 365nm is significantly higher than that of the commercial Si-based ultraviolet photodetector, and the responsivities of PM6:CH-4F and commercial Si-based ultraviolet photodetectors at 365nm are 0.23A / W and 0.15A / W respectively, which are proportional to the size of the generated photocurrent. This shows that the organic ultraviolet photodetector PM6:CH-4F is significantly better than the commercial Si-based ultraviolet photodetector in absorbing ultraviolet light. Under the same conditions, the organic ultraviolet photodetector has a greater responsiveness, a faster response speed, and a higher sensitivity.
[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An ultraviolet photodetector based on organic materials, characterized in that: It includes a transparent rigid substrate, a bottom electrode, an electron transport layer, a modification layer, a photoactive layer, a hole transport layer and a top electrode arranged from bottom to top; or a transparent rigid substrate, a bottom electrode, a hole transport layer, a photoactive layer, an electron transport layer and a top electrode arranged from bottom to top; the photoactive layer is a thin film formed by blending a polymer donor and an organic acceptor, the polymer donor includes but is not limited to PBDB-T, PM6, D18, and the organic acceptor includes but is not limited to F-2F, CH-4F, CH-4Cl, CH17, Y6.
2. The ultraviolet photodetector based on organic materials as claimed in claim 1, characterized in that: The polymer donor is at least one of PBDB-T, PM6, and D18, and the organic acceptor is at least one of CH-4F and CH-4Cl.
3. An organic material-based ultraviolet photodetector as claimed in claim 2, characterized in that: The polymer donor is PM6, and the organic acceptor is CH-4F.
4. The ultraviolet photodetector based on organic materials as claimed in claim 1, characterized in that: The mass ratio of the polymer donor to the organic acceptor is 1:1-1:
100.
5. The ultraviolet photodetector based on organic materials as claimed in claim 4, characterized in that: The mass ratio of the polymer donor to the organic acceptor is 1:
1.
6. The ultraviolet photodetector based on organic materials as claimed in claim 1, characterized in that: The photoactive layer has a thickness of 10 nm to 200 nm.
7. An organic material-based ultraviolet photodetector according to any one of claims 1 to 6, characterized in that: The transparent rigid substrate includes but is not limited to a quartz plate or other highly transparent rigid substrate with a transmittance of more than 90% to ultraviolet light; The bottom electrode includes but is not limited to indium tin oxide, metal nanowires, carbon nanotubes, conductive polymers, metal grids, graphene, and PH1000; The top electrode includes, but is not limited to, silver, gold, lithium, calcium, strontium, barium, indium, magnesium, aluminum, and copper; The electron transport layer is one or more of ZnO nanoparticles, ZnO nanocrystals, TiO2, SnO2, WO3, PDINO, and PNDIT-F3N; The hole transport layer includes but is not limited to MoO3, PEDOT:PSS, CuO x 、WO3、NiO x , SAM-2PACz; The modification layer includes but is not limited to PFN-Br, PEIE, and PFN / PFBT.
8. The organic material-based ultraviolet photodetector according to claim 7, characterized in that: The transparent rigid substrate is a quartz plate.
9. A method for preparing an ultraviolet photodetector based on organic materials according to any one of claims 1 to 6, characterized in that: Specifically, the steps include: S1. Preparation of transparent rigid substrate: The transparent rigid substrate is ultrasonically cleaned with glass cleaning liquid, deionized water, acetone, and isopropanol in sequence, and then the surface of the transparent rigid substrate is blown dry with a nitrogen gun, irradiated in a UV ozone treatment device, and placed in a glass culture dish for later use; S2. Preparation of bottom electrode: The prepared bottom electrode solution is spin-coated onto a transparent rigid substrate, and an annealing treatment is performed to obtain a bottom electrode; S3. Preparation of hole transport layer: The hole transport layer material is mixed and diluted with deionized water, fully dispersed by ultrasound, filtered using a filter membrane, and spin-coated on the bottom electrode, and annealed to obtain the hole transport layer; S4. Preparation of photoactive layer: The polymer donor and the organic acceptor are dissolved in a chloroform solvent at a mass ratio of 1:1-1:100, and the prepared solution is spin-coated on the hole transport layer and annealed to obtain a photoactive layer; S5. Preparation of electron transport layer: The electron transport layer is dissolved in methanol, and after stirring, the prepared solution is spin-coated on the photoactive layer to obtain the electron transport layer; S6. Evaporation of top electrode: A top electrode is evaporated on the electron transport layer to obtain the ultraviolet photodetector.
10. A method for preparing an ultraviolet photodetector based on organic materials as claimed in claim 9, characterized in that: Specifically, the following steps are included: S1. Preparation of transparent rigid substrate: The transparent rigid substrate was ultrasonically cleaned with glass cleaning liquid, deionized water, acetone, and isopropanol in sequence, the surface of the transparent rigid substrate was blown dry with a nitrogen gun, irradiated in a UV ozone treatment device for 15 minutes, and placed in a glass culture dish for later use; S2. Preparation of bottom electrode: The prepared bottom electrode solution was spin-coated onto a transparent rigid substrate at 2000 rpm, and annealed at 130° C. for 0.5 hours to obtain a bottom electrode after annealing. S3. Preparation of hole transport layer: The hole transport layer material was mixed and diluted with deionized water in a ratio of 1:1, and after being fully dispersed by ultrasound, it was filtered using a PES 0.45 μm pore size filter membrane, and then spin-coated on the bottom electrode, and annealed at 150° C. for 0.5 hour to obtain a hole transport layer after annealing; S4. Preparation of photoactive layer: The polymer donor and the organic acceptor are dissolved in a chloroform solvent at a mass ratio of 1:1-1:100 at 45°C for 5 hours; the prepared solution is spin-coated on the hole transport layer at 2000 rpm and annealed at 100°C for 10 minutes to obtain a photoactive layer; S5. Preparation of electron transport layer: 2 g of the electron transport layer was dissolved in 2 mL of methanol, and after stirring for 6 hours, the prepared solution was spin-coated on the photoactive layer at 3000 rpm to obtain the electron transport layer; S6. Evaporation of top electrode: A 200nm top electrode is evaporated on the electron transport layer to obtain the ultraviolet photodetector.