Molded zeolite, adsorption device, method for producing purified gas, and method for producing molded zeolite
Patent Information
- Application Number
- CN202380024611.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-18
AI Technical Summary
[0074]根据本发明,能够提供针对二氧化碳吸附的耐脆化性优异的沸石成型体、包含该沸石成型体的吸附装置、使用该吸附装置的精制气体的制造方法、以及沸石成型体的制造方法。
Smart Images

Figure CN118804892A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a zeolite molded body, an adsorption device, a method for producing a purified gas, and a method for producing a zeolite molded body. Background Art
[0002] Zeolite can be used as an adsorbent, a desiccant, a separating agent, a catalyst, a catalyst carrier, a detergent builder, an ion exchanger, a wastewater treatment agent, a fertilizer, a food additive, a cosmetic additive, and the like, and is particularly useful for gas separation.
[0003] For example, among zeolites, a substance represented by a GIS structure in a code for defining zeolite structure established by IZA (International Zeolite Association) is called a GIS-type zeolite. GIS-type zeolite is a zeolite having fine pores composed of an 8-membered oxygen ring. Regarding this GIS-type zeolite, for example, in Patent Document 1, a GIS-type zeolite having an adsorption capacity for carbon dioxide is synthesized, and it is shown that when the GIS-type zeolite is used as an adsorbent material, it can be used for separation, recovery, and purification of carbon dioxide.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. WO2019 / 202933 Summary of the invention
[0007] Problems to be solved by the invention
[0008] When using an adsorbent material to separate, recover, and purify carbon dioxide, a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method is used. In these methods, zeolite is filled in a column or the like and used. In order to prevent the micro-powdered zeolite from accumulating in the flow path in the device and blocking the flow path, the zeolite is shaped and used in the form of a granular zeolite molded body. As the performance of the zeolite molded body, it is required to have sufficient durability for the use conditions.
[0009] The following problem has been found in zeolite molded bodies containing zeolite capable of adsorbing carbon dioxide: when a larger amount of carbon dioxide is adsorbed, the molded body becomes brittle, and if the zeolite molded body is in the form of pellets, it becomes powdery. This brittleness generates fine powder in the adsorption device, which makes it difficult to operate the device continuously due to pressure loss, etc.
[0010] An object of the present invention is to provide a zeolite molded body having excellent resistance to embrittlement with respect to carbon dioxide adsorption, an adsorption device including the zeolite molded body, a method for producing a purified gas using the adsorption device, and a method for producing a zeolite molded body.
[0011] Means for solving problems
[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found that the problems can be solved when the density of a zeolite molded body containing zeolite is within a predetermined range, thereby completing the present invention.
[0013] That is, the present invention includes the following embodiments.
[0014] <1>
[0015] A zeolite shaped body, comprising zeolite capable of adsorbing carbon dioxide, wherein:
[0016] The apparent density d of the zeolite molded body is a It is above 0.75.
[0017] <2>
[0018] like <1> The zeolite shaped body, wherein the zeolite has a diameter of 10 cm 3 / g or more carbon dioxide adsorption capacity.
[0019] <3>
[0020] like <1> or <2> The zeolite molded body, wherein the apparent density d a / True density d t The ratio is above 0.36.
[0021] <4>
[0022] like <1> ~ <3> The zeolite molded body according to any one of the preceding claims, wherein the bulk density d b / True density d t The ratio is greater than 0.25.
[0023] <5>
[0024] like <1> ~ <4> The zeolite molded body according to any one of the preceding claims, wherein the adsorption selectivity of the zeolite of carbon dioxide adsorption amount / second component gas adsorption amount is 10 or more.
[0025] <6>
[0026] like <1> ~ <5> The zeolite molded body according to any one of the preceding claims, wherein the zeolite is a GIS-type zeolite.
[0027] <7>
[0028] like <6> The zeolite molded body, wherein the silica-alumina ratio of the GIS type zeolite is 3.40 or more.
[0029] <8>
[0030] like <6> or <7> The zeolite shaped body contains potassium or lithium as the cationic species in the GIS type zeolite.
[0031] <9>
[0032] like <6> ~ <8> The zeolite molded body according to any one of the preceding claims, wherein a ratio (Z / T) of a total amount (Z) of potassium and lithium to a total amount (T) of alkali metals in the GIS-type zeolite is 0.05 or more.
[0033] <10>
[0034] like <6> ~ <9> The zeolite shaped body described in any one of the above, comprising GIS type zeolite, 29 When the peak area intensities attributed to Q4(3Al), Q4(2Al), Q4(1Al) and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c and d respectively, the GIS-type zeolite satisfies (a+d) / (b+c)≧0.192.
[0035] <11>
[0036] like <1> ~ <10> The zeolite shaped body described above comprises a carrier.
[0037] <12>
[0038] like <11> The zeolite shaped body, wherein the carrier comprises an inorganic binder and an organic binder.
[0039] <13>
[0040] like <11> or <12> The zeolite molded body described above has a total content of the carrier of 1 to 99% by mass relative to the total amount (100% by mass) of the zeolite molded body.
[0041] <14>
[0042] like <1> ~ <13> The zeolite molded body according to any one of the preceding claims, wherein the degree of weight loss per 1.2 g under the conditions of 300° C. and 2 hours is 1.0 or less.
[0043] <15>
[0044] like <1> ~ <14> The zeolite molded body according to any one of the preceding claims, wherein an aspect ratio is 1 to 10.
[0045] <16>
[0046] like <1> ~ <15> The zeolite molded body described in any one of the above aspects has a cylindrical shape.
[0047] <17>
[0048] like <16> The zeolite molded body has a length of 3 mm to 30 mm, and a diameter of 1 mm to 30 mm.
[0049] <18>
[0050] like <1> ~ <15> The zeolite molded body described in any one of the above aspects has a spherical shape.
[0051] <19>
[0052] like <18> The diameter of the zeolite molded body is not less than 3 mm and not more than 10 mm.
[0053] <20>
[0054] An adsorption device comprising <1> ~ <19> The zeolite shaped body described in any one of the above.
[0055] <21>
[0056] A method for producing a purified gas, comprising:
[0057] Separation process, using <20> The adsorption device separates one or more gases selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, Ar, CO and hydrocarbons.
[0058] <22>
[0059] like <21> The method for producing a purified gas as described above, wherein in the above-mentioned separation step, the above-mentioned gas is separated by a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method.
[0060] <23>
[0061] A method for producing a purified gas, wherein the carbon dioxide and the second component gas different from the carbon dioxide are separated from a mixed gas containing the carbon dioxide and the second component gas using an adsorption tower, wherein:
[0062] The manufacturing method comprises:
[0063] an adsorption step of introducing the mixed gas into the adsorption tower, allowing the carbon dioxide to be adsorbed on the adsorbent, and taking out the second component gas; and
[0064] The desorption step is to decompress and exhaust the carbon dioxide from the adsorption tower, thereby removing the carbon dioxide from the adsorbent.
[0065] The adsorption tower is filled with <1> ~ <22> An adsorbent of the zeolite shaped body as described above.
[0066] <24>
[0067] like <23> The method for producing a purified gas as described above, wherein the adsorption step and the desorption step are repeated a plurality of times or more.
[0068] <25>
[0069] A method for producing a zeolite shaped body, comprising:
[0070] a raw material mixing step (X) of mixing a zeolite capable of adsorbing carbon dioxide with a carrier comprising an inorganic binder and an organic binder;
[0071] a molding step (Y), subjecting the prepared raw material to a molding process to obtain a precursor; and
[0072] The calcining step (Z) is to calcine the above-mentioned precursor to obtain a zeolite molded body.
[0073] Effects of the Invention
[0074] According to the present invention, there can be provided a zeolite molded body having excellent embrittlement resistance to carbon dioxide adsorption, an adsorption device including the zeolite molded body, a method for producing a purified gas using the adsorption device, and a method for producing a zeolite molded body. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 This is a diagram illustrating an adsorption device according to this embodiment.
[0076] Figure 2 It is a diagram illustrating a schematic configuration of a purified gas production apparatus 100 according to the present embodiment.
[0077] Figure 3 It is a schematic diagram showing the temporal change of the pressure fluctuation of the carbon dioxide adsorption tower and the carbon dioxide adsorption tower due to the operation of the purified gas production device 100 .
[0078] Figure 4 It is a diagram illustrating the gas separation performance evaluation device of the present invention. DETAILED DESCRIPTION
[0079] The specific implementation mode of the present invention (hereinafter referred to as "the present implementation mode") is described in detail below. The present invention is not limited to the following description, and can be implemented in various ways within the scope of its main points. It should be noted that in this specification, the expression of a numerical range such as "1 to 100" includes both its lower limit "1" and upper limit "100". In addition, the expression of other numerical ranges is the same.
[0080] [Zeolite Molded Body]
[0081] The zeolite molded body of the present embodiment includes zeolite capable of adsorbing carbon dioxide, and the apparent density d of the zeolite molded body is a is 0.75 or more. The zeolite molded body of the present embodiment has excellent resistance to embrittlement against carbon dioxide adsorption. According to the present embodiment, it is considered that by making the zeolite molded body high-densified, controlling the amount of voids present in the zeolite molded body and densifying it, the maximum stress generated by the expansion and contraction of the zeolite itself can be reduced, and a zeolite molded body having durability against degradation caused by expansion and contraction, an adsorption device including the zeolite molded body, a method for producing a purified gas using the adsorption device, and a method for producing a zeolite molded body can be provided.
[0082] From the viewpoint of improving the embrittlement resistance against carbon dioxide adsorption, the apparent density d a (g / cm 3 ) is 0.75 or more, preferably 0.78 or more, more preferably 0.80 or more. a The upper limit of is not particularly limited, and may be, for example, 3.20 or less, 2.80 or less, or 2.50 or less. a The predetermined range may be adjusted by selecting the vector species described later.
[0083] From the viewpoint of enabling gas separation using a smaller device, the bulk density d of the zeolite molded body is b (g / cm 3 ) is preferably 0.20 or more, more preferably 0.40 or more, and even more preferably 0.50 or more. Bulk density d b The upper limit of is not particularly limited, and may be, for example, 3.00 or less, 2.50 or less, or 1.50 or less. b The predetermined range may be achieved by adjusting the size of the molded product described later.
[0084] True density of zeolite shaped body d t (g / cm 3) can be, for example, 1.00 to 4.00, 1.50 to 3.50, or 2.00 to 3.00. t The predetermined range may be achieved by adjusting the type of carrier, the amount of carrier added, etc., as described later.
[0085] From the viewpoint of improving the recovery purity of carbon dioxide and the recovery rate of the second component gas, the apparent density d a / True density d t It is preferably 0.36 or more, more preferably 0.42 or more, and even more preferably 0.50 or more. a / True density d t Less than 1.0, preferably less than 0.90, more preferably less than 0.80, and further preferably less than 0.70. In the case of separating carbon dioxide through a zeolite molded body, for example, there is a method of desorbing carbon dioxide by reducing pressure after circulating carbon dioxide so that carbon dioxide is adsorbed on the zeolite molded body. At this time, it was found that in this separation method, the recovery purity of carbon dioxide and the recovery rate of the second component gas could not exceed a certain level, and their values decreased. If the recovery purity of carbon dioxide and the recovery rate of the second component gas are low, the gas needs to be repeatedly treated to improve the recovery purity of carbon dioxide and the recovery rate of the second component gas, and the cost of gas purification increases. In response to this issue, it was found that if there are voids in the zeolite molded body through which carbon dioxide is adsorbed and desorbed, the second component gas will remain in an unadsorbed state and remain in the adsorption tower, so the recovery purity of carbon dioxide cannot be improved. It was further found that the second component gas remaining in the voids cannot be recovered in the form of purified gas, so the recovery rate of the second component gas cannot be improved. It is therefore believed that by making the apparent density d of the zeolite molded body a / True density d t In the above range, the proportion of voids in the zeolite molded body can be reduced, resulting in a reduction in the amount of residual gas, so that the recovery purity of carbon dioxide and the recovery rate of the second component gas can be improved. a / True density d t The predetermined range may be achieved by adjusting the content by selecting a carrier, a granulation method, etc. as described below.
[0086] The "second component gas" refers to a substance other than carbon dioxide that is a gas at a temperature of 25°C and a pressure of 0.10 MPa. Examples of the second component gas include H2, N2, O2, Ar, CO, and hydrocarbons. The hydrocarbons are not particularly limited, and examples thereof include methane, ethane, ethylene, propane, propylene, 1-butene, 2-butene, 2-methylpropylene, dimethyl ether, and acetylene.
[0087] From the viewpoint of improving the recovery purity of carbon dioxide and the recovery rate of the second component gas, the bulk density d in the zeolite molded body is b / True density d t It is preferably 0.25 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. Bulk density d b / True density d t The upper limit of is not particularly limited, but is less than 1.0, preferably less than 0.90, more preferably less than 0.70, and further preferably less than 0.60. It has been found that even in the gaps between the zeolite molded bodies through which carbon dioxide is adsorbed and desorbed, the unadsorbed gas remains in the adsorption tower, and therefore the recovery purity of carbon dioxide cannot be improved. It has also been found that since the second component gas remaining in the gaps between the molded bodies cannot be recovered as a purified gas, the recovery rate of the second component gas cannot be improved. It is therefore believed that by increasing the bulk density d of the zeolite molded body to 1.5, the recovery rate of the second component gas cannot be increased. b / True density d t When the bulk density d is within the above range, the ratio of voids between the zeolite molded bodies can be reduced, resulting in a reduction in the amount of residual gas. As a result, the recovery purity of carbon dioxide and the recovery rate of the second component gas can be improved. b / True density d t The predetermined range may be achieved by adjusting the size of the carrier, the size of the molded product, the granulation method, etc., which will be described later.
[0088] The above apparent density d a , bulk density d b and the true density d t The measurement method is based on the method described in the Examples.
[0089] (Zeolite)
[0090] The zeolite preferably has a diameter of 10 cm 3 / g or more of carbon dioxide adsorption. The carbon dioxide adsorption of zeolite is preferably 20cm 3 / g or more, more preferably 40cm 3 / g or more, more preferably 50cm 3 The upper limit of the carbon dioxide adsorption amount of zeolite is not particularly limited, but is, for example, 100 cm 3 / g or less.
[0091] In zeolite, from the perspective of further improving the recovery purity of carbon dioxide, the adsorption selectivity of carbon dioxide adsorption / second component gas adsorption is preferably 10 or more, more preferably 13 or more, and even more preferably 15 or more. The upper limit of the adsorption selectivity of carbon dioxide adsorption / second component gas adsorption in zeolite is not particularly limited, and is, for example, 100 or less. The gas adsorption of carbon dioxide and second component gas is the carbon dioxide adsorption capacity (cm2) per 1g of zeolite at 25°C. 3 ). More specifically, the measurement was performed by the method described in the Examples.
[0092] In zeolite, from the perspective of further improving the recovery purity of carbon dioxide, the adsorption selectivity of carbon dioxide adsorption / methane adsorption is preferably 10 or more, more preferably 13 or more, and even more preferably 15 or more. The upper limit of the adsorption selectivity of carbon dioxide adsorption / methane adsorption of zeolite is not particularly limited, and is, for example, 100 or less.
[0093] In zeolite, from the perspective of further improving the recovery purity of carbon dioxide, the adsorption selectivity of carbon dioxide adsorption / nitrogen adsorption is preferably 10 or more, more preferably 13 or more, and even more preferably 15 or more. The upper limit of the adsorption selectivity of carbon dioxide adsorption / nitrogen adsorption of zeolite is not particularly limited, and is, for example, 100 or less.
[0094] Examples of zeolite capable of adsorbing carbon dioxide include GIS zeolite, FAU zeolite, MWF zeolite, etc. Among these, GIS zeolite is preferred.
[0095] The lower the silica-alumina ratio (expressed as the molar ratio of silica to alumina expressed as SiO2 / Al2O3, hereinafter also referred to as "SAR") of the GIS type zeolite of the present embodiment, the more hydrophilic it is, and the stronger the adsorption force of polar molecules such as carbon dioxide. If the SAR is low, the adsorption force is too strong, so the energy required for desorption by heating or vacuuming increases, and thus a high SAR is preferred. The SAR of the GIS type zeolite is preferably 3.40 or more, more preferably 4.40 or more, more preferably 4.50 or more, further preferably 4.69 or more, further preferably 4.90 or more, further preferably 5.40 or more, and further preferably 6.01 or more. There is no particular limit to the upper limit of the SAR, but if the SAR is too high, the interaction with the adsorbate is reduced, and thus the SAR of the GIS type zeolite is preferably 3000 or less, more preferably 500 or less, and further preferably 100 or less. The SAR of the zeolite in the zeolite molded body is determined by performing 29 SAR can be determined by Si-MAS-NMR measurement. SAR can be measured in more detail by the method described in the examples below. SAR can be determined by mixing water and OH in the gel. -Adjust the amount ratio, etc.
[0096] From the perspective of the energy required for desorption, a high SAR is preferred. On the other hand, when the SAR in the GIS type zeolite increases, it is confirmed that the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide becomes dominant. In the GIS type zeolite of the present embodiment, the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide can be eliminated by controlling the bonding mode of Si and Al in the zeolite framework. Specifically, 29 The peak area intensities attributable to Q4(3Al), Q4(2Al), Q4(1Al), and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c, and d, respectively, preferably satisfying (a+d) / (b+c)≧0.192, more preferably 0.913≧(a+d) / (b+c)≧0.195, and further preferably 0.519≧(a+d) / (b+c)≧0.199. 29 Peaks such as Q4(3Al), Q4(2Al), Q4(1Al), and Q4(0Al) observed in the Si-MAS-NMR spectrum represent the bonding mode of Si and Al in the zeolite framework, and (a+d) and (b+c), which are the sum of the area intensities, represent the sum of the amounts of these bonding modes, and (a+d) / (b+c) represents the existence ratio. The existence ratio of the bonding modes of Si and Al affects the structural changes of the zeolite framework itself during adsorption and desorption. Therefore, by making the existence ratio of the bonding modes of Si and Al in the zeolite framework, i.e., (a+d) / (b+c), within an appropriate range, the adsorption-desorption hysteresis in the adsorption-desorption isotherm can be eliminated. (a+d) / (b+c) can be measured by the method described in the examples described later. In order to make (a+d) / (b+c) within a specified range, a salt compound containing an alkali metal and / or an alkaline earth metal can be added, and the adjustment can be made by the amount ratio of the cation and the aluminum source brought about by the addition of the salt compound.
[0097] From the perspective of improving the selective adsorption capacity of carbon dioxide, as the cationic species in the GIS type zeolite, it is preferred to contain potassium or lithium, and more preferably potassium. In addition, the total content of potassium and lithium in the zeolite is calculated as the ratio (Z / T) of the total value of the amount of substance of potassium and lithium in the GIS type zeolite (Z) relative to the total value of the amount of substance of alkali metals (T). Z / T is preferably greater than 0.05, more preferably greater than 0.10, and further preferably greater than 0.15. There is no particular limit to the upper limit of Z / T, and Z / T can be less than 1.00. Regarding Z / T, it can be measured by ICP-emission spectrometry using a liquid that is appropriately diluted after the zeolite is thermally dissolved using an aqueous sodium hydroxide solution or aqua regia. In more detail, Z / T can be measured by the method described in the examples described later. Z / T can be adjusted by changing the ratio of potassium and lithium in the cationic species of the GIS type zeolite.
[0098] The ratio (K / T) of the total amount of potassium (K) in the GIS zeolite to the total amount of each alkali metal (T) is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more. The upper limit of K / T is not particularly limited, and K / T may be 1.00 or less.
[0099] In GIS type zeolite, the weight loss per 1.2 g is 1.0 or less under the conditions of 300°C and 2 hours. By making the weight loss 1.0 or less, high temperature durability is improved. The weight loss is preferably 0.5 or less, more preferably 0.2 or less, and further preferably 0.1 or less.
[0100] The weight reduction is based on the measurement method described in the Examples. The weight reduction can be adjusted to the above range by reducing the organic binder or sintering the zeolite molded body at a temperature exceeding 300°C.
[0101] The preferred content of zeolite may be 50% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more relative to the total amount 100% by mass of the zeolite molded body. In addition, the content of zeolite may be 98% by mass or less, or 95% by mass or less relative to the total amount 100% by mass of the zeolite molded body.
[0102] (Synthesis method of GIS type zeolite)
[0103] The method for producing the GIS type zeolite of the present embodiment may include, for example, a step of preparing a mixed gel, the mixed gel containing a silicon oxide source containing silicon, an aluminum source containing aluminum, an alkali source containing at least one selected from an alkali metal (M1) and an alkaline earth metal (M2), a salt compound containing at least one selected from an alkali metal (M1) and an alkaline earth metal (M2), a phosphorus source containing phosphorus, an organic structure directing agent, and water. The mixed gel and the components contained therein are described below.
[0104] [Mixed gel]
[0105] The hybrid gel in the present embodiment is a mixture containing a silicon oxide source, an aluminum source, a salt compound, and water as components, and optionally containing a phosphorus source, an alkali source, and an organic structure-directing agent.
[0106] The silicon oxide source refers to a component in the mixed gel that is a raw material of silicon contained in the zeolite manufactured from the mixed gel, the aluminum source refers to a component in the mixed gel that is a raw material of aluminum contained in the zeolite manufactured from the mixed gel, the salt compound refers to a component in the mixed gel that is a raw material of alkali metal and / or alkaline earth metal contained in the zeolite manufactured from the mixed gel, the alkali source refers to a component for adjusting the alkalinity of the mixed gel, and the phosphorus source refers to a component in the mixed gel that is a raw material of phosphorus contained in the zeolite manufactured from the mixed gel.
[0107] [Silicon oxide source]
[0108] As a silicon oxide source, there is no particular limitation as long as it is a commonly used silicon oxide source, and examples thereof include crystalline silicon oxide, amorphous silicon oxide, silicic acid, silicates, and organic silicic acid compounds. More specific examples include sodium silicate, potassium silicate, calcium silicate, magnesium silicate, fumed silica, precipitated silica, silica gel, colloidal silica, aluminum silicate, tetraethoxysilane (TEOS), trimethylethoxysilane, and the like. These compounds can be used alone or in combination. Here, aluminum silicate is both a silicon oxide source and an aluminum source.
[0109] Among these, fumed silica, colloidal silica, or precipitated silica is preferred because zeolite with high crystallinity tends to be obtained.
[0110] [Aluminum source]
[0111] The aluminum source is not particularly limited as long as it is a commonly used aluminum source, and specific examples thereof include sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum acetate, aluminum hydroxide, aluminum oxide, aluminum chloride, aluminum alkoxide, metallic aluminum, amorphous aluminum silicate gel, etc. These compounds may be used alone or in combination of a plurality of them.
[0112] Among these, sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum acetate, aluminum hydroxide, aluminum chloride, and aluminum alkoxide are preferred because they tend to produce zeolites with high crystallinity. From the same perspective, sodium aluminate and aluminum hydroxide are more preferred, and sodium aluminate is further preferred.
[0113] [Salt compounds]
[0114] The salt compound is a compound containing alkali metals such as Li, Na, K, Rb, and Cs, and alkaline earth metals such as Ca, Mg, Sr, and Ba, which promote crystallization into a zeolite structure when manufacturing zeolite. As the alkali metal and alkaline earth metal contained in the added salt compound, Na and K are preferably used, and Na is more preferably used, from the aspect that the crystallization of the GIS type skeleton is easier. In addition, the salt compound can be used alone or in combination of multiple types.
[0115] Specifically, examples of salt compounds include, but are not limited to, sodium sulfate, sodium sulfite, sodium thiosulfate, sodium nitrite, sodium nitrate, sodium carbonate, sodium bicarbonate, sodium phosphate, sodium acetate, sodium formate, sodium citrate, sodium oxalate, sodium fluoride, sodium chloride, sodium bromide, sodium iodide, sodium sulfide, sodium silicate, sodium metasilicate, sodium tetraborate, sodium chlorate, sodium perchlorate, sodium cyanide, sodium metastannate, sodium hexahydroxytin (IV) acid, sodium hexacyanoferrous (II) acid, sodium permanganate, sodium chromate, sodium dichromate,
[0116] Potassium sulfate, potassium sulfite, potassium thiosulfate, potassium nitrite, potassium nitrate, potassium carbonate, potassium bicarbonate, potassium phosphate, potassium acetate, potassium formate, potassium citrate, potassium oxalate, potassium fluoride, potassium chloride, potassium bromide, potassium iodide, potassium sulfide, potassium silicate, potassium metasilicate, potassium tetraborate, potassium chlorate, potassium perchlorate, potassium cyanide, potassium metastannate, potassium hexahydroxytin (IV) acid, potassium hexacyanoferrous (II) acid, potassium permanganate, potassium chromate, potassium dichromate,
[0117] Lithium sulfate, lithium sulfite, lithium thiosulfate, lithium nitrite, lithium nitrate, lithium carbonate, lithium bicarbonate, lithium phosphate, lithium acetate, lithium formate, lithium citrate, lithium oxalate, lithium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium sulfide, lithium silicate, lithium metasilicate, lithium tetraborate, lithium chlorate, lithium perchlorate, lithium cyanide, lithium metastannate, lithium hexahydroxytin (IV) acid, lithium hexacyanoferrous (II) acid, lithium permanganate, lithium chromate, lithium dichromate,
[0118] Rubidium sulfate, rubidium sulfite, rubidium thiosulfate, rubidium nitrite, rubidium nitrate, rubidium carbonate, rubidium bicarbonate, rubidium phosphate, rubidium acetate, rubidium formate, rubidium citrate, rubidium oxalate, rubidium fluoride, rubidium chloride, rubidium bromide, rubidium iodide, rubidium sulfide, rubidium silicate, rubidium metasilicate, rubidium tetraborate, rubidium chlorate, rubidium perchlorate, rubidium cyanide, rubidium metastannate, rubidium hexahydroxytin (IV) acid, rubidium hexacyanoferrous (II) acid, rubidium permanganate, rubidium chromate, rubidium dichromate,
[0119] Cesium sulfate, cesium sulfite, cesium thiosulfate, cesium nitrite, cesium nitrate, cesium carbonate, cesium bicarbonate, cesium phosphate, cesium acetate, cesium formate, cesium citrate, cesium oxalate, cesium fluoride, cesium chloride, cesium bromide, cesium iodide, cesium sulfide, cesium silicate, cesium metasilicate, cesium tetraborate, cesium chlorate, cesium perchlorate, cesium cyanide, cesium metastannate, cesium hexahydroxytin (IV) acid, cesium hexacyanoferrous (II) acid, cesium permanganate, cesium chromate, cesium dichromate,
[0120] Magnesium sulfate, magnesium sulfite, magnesium thiosulfate, magnesium nitrite, magnesium nitrate, magnesium carbonate, magnesium bicarbonate, magnesium phosphate, magnesium acetate, magnesium formate, magnesium citrate, magnesium oxalate, magnesium fluoride, magnesium chloride, magnesium bromide, magnesium iodide, magnesium sulfide, magnesium silicate, magnesium metasilicate, magnesium tetraborate, magnesium chlorate, magnesium perchlorate, magnesium cyanide, magnesium metastannate, magnesium hexahydroxystannate (IV), magnesium hexacyanoferrous (II), magnesium permanganate, magnesium chromate, magnesium dichromate,
[0121] Calcium sulfate, calcium sulfite, calcium thiosulfate, calcium nitrite, calcium nitrate, calcium carbonate, calcium bicarbonate, calcium phosphate, calcium acetate, calcium formate, calcium citrate, calcium oxalate, calcium fluoride, calcium chloride, calcium bromide, calcium iodide, calcium sulfide, calcium silicate, calcium metasilicate, calcium tetraborate, calcium chlorate, calcium perchlorate, calcium cyanide, calcium metastannate, calcium hexahydroxystannate (IV), calcium hexacyanoferrous (II), calcium permanganate, calcium chromate, calcium dichromate,
[0122] Strontium sulfate, strontium sulfite, strontium thiosulfate, strontium nitrite, strontium nitrate, strontium carbonate, strontium bicarbonate, strontium phosphate, strontium acetate, strontium formate, strontium citrate, strontium oxalate, strontium fluoride, strontium chloride, strontium bromide, strontium iodide, strontium sulfide, strontium silicate, strontium metasilicate, strontium tetraborate, strontium chlorate, strontium perchlorate, strontium cyanide, strontium metastannate, strontium hexahydroxytin (IV) acid, strontium hexacyanoferrous (II) acid, strontium permanganate, strontium chromate, strontium dichromate,
[0123] Barium sulfate, barium sulfite, barium thiosulfate, barium nitrite, barium nitrate, barium carbonate, barium bicarbonate, barium phosphate, barium acetate, barium formate, barium citrate, barium oxalate, barium fluoride, barium chloride, barium bromide, barium iodide, barium sulfide, barium silicate, barium metasilicate, barium tetraborate, barium chlorate, barium perchlorate, barium cyanide, barium metastannate, barium hexahydroxytin (IV) acid, barium hexacyanoferrous (II) acid, barium permanganate, barium chromate, barium dichromate, etc.
[0124] [Alkali source]
[0125] Alkali source is used for the purpose of adjusting the alkalinity (pH) in the mixed gel in order to promote crystallization into a zeolite structure when manufacturing zeolite. The alkali used can be any compound showing alkalinity, and both inorganic compounds and organic compounds are acceptable. From the perspective of cost, inorganic compounds are preferred, and alkali metal hydroxides can be more preferably cited. As alkali metal hydroxides, lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, etc. can be cited, and sodium hydroxide and potassium hydroxide can be preferably cited, and sodium hydroxide can be more preferably cited. These compounds can be used alone, or a plurality of them can be used in combination.
[0126] The phosphorus source is not particularly limited as long as it is a commonly used phosphorus source, and specific examples include aqueous phosphoric acid solution, sodium phosphate, aluminum phosphate, potassium phosphate, lithium phosphate, calcium phosphate, barium phosphate, etc. These compounds may be used alone or in combination of plural types.
[0127] Among these, phosphoric acid aqueous solution, sodium phosphate, and aluminum phosphate are preferred because they tend to produce zeolite with high crystallinity. From the same viewpoint, phosphoric acid aqueous solution and sodium phosphate are more preferred, and phosphoric acid aqueous solution is still more preferred.
[0128] [Organic structure directing agent]
[0129] When zeolite is produced by hydrothermal synthesis of a mixed gel, the organic structure-directing agent is a compound that promotes crystallization into a zeolite structure. The organic structure-directing agent may be used as necessary in the crystallization of zeolite.
[0130] The organic structure directing agent may be of any type as long as it can form the desired GIS-type zeolite. The organic structure directing agent may be used alone or in combination of two or more.
[0131] As the organic structure directing agent, for example, amines, quaternary ammonium salts, alcohols, ethers, amides, alkyl ureas, alkyl thioureas, cyanoalkanes, and alicyclic heterocyclic compounds containing nitrogen as a heteroatom can be used, but are not limited thereto. Preferably, alkylamines are used, and more preferably, isopropylamine is used.
[0132] Such salts may be accompanied by anions. Representative examples of such anions include, but are not limited to, Cl - Br - ,I - Halogen ions, hydroxide ions, acetate ions, sulfate ions, nitrate ions, carbonate ions, and bicarbonate ions are preferred. Among these, halogen ions and hydroxide ions are preferred, and halogen ions are more preferred, because crystal formation of the GIS-type skeleton becomes easier.
[0133] [Composition ratio of mixed gel]
[0134] In this embodiment, in order to synthesize GIS type zeolite with a suitable structure, it is most important to add a salt compound containing an alkali metal and / or an alkaline earth metal. In the formation of zeolite, the silicon oxide source and the aluminum source dissolved in the water solvent react while dissolving, thereby crystallizing. However, by adding the salt compound, the bonding mode or the existence ratio of Si and Al in the zeolite framework can be adjusted, and a GIS with an ideal crystal structure can be synthesized.
[0135] In addition, the ratio of cations brought by the addition of salt compounds to the aluminum source is particularly important. The ratio of cations brought by the salt compounds in the mixed gel to the aluminum source is expressed as the total molar ratio of the amount of cations E to Al2O3, that is, E / Al2O3. Here, E represents the molar amount of cations brought by the salt compound. For example, when sodium nitrate is added, Na2O3 is generated as a cationic species. + , generates 2Na in sodium carbonate + , the total molar amount of cationic species generated by the addition of salt compounds is represented by E. The aggregation state of Al in the mixed gel can be changed by E / Al2O3, thereby controlling the randomness of Al when forming zeolite crystals, and synthesizing GIS type zeolite with an ideal crystal structure. From the above aspects, it is necessary to optimally control E / Al2O3, and E / Al2O3 is preferably 0.1 to 100.0, more preferably 0.5 to 80.0, and further preferably 0.8 to 50.0.
[0136] In addition, in order to synthesize GIS-type zeolites with suitable SAR, water in the mixed gel was mixed with OH - Ratio (H2O / OH - ) is important. - It is OH derived from inorganic hydroxides such as NaOH and Ca(OH)2, and organic hydroxides such as tetraethylammonium hydroxide used as alkali sources. - , excluding OH released when substances expressed as oxides such as sodium aluminate and sodium silicate, or their hydrates are dissolved in water. - In the formation of zeolite, the silicon oxide source, aluminum source, and alkali source dissolved in the water solvent form crystals and react, and a portion of them dissolves into the alkaline solvent, causing a balance between crystallization and redissolution. - Adding to the mixed gel means shifting the balance between crystallization and redissolution to the redissolution side. Regarding redissolution, dissolution starts from the amorphous or low-crystalline part. Therefore, the process is repeated by appropriately increasing the OH -The operation of re-dissolving the incomplete crystallized part and re-crystallizing it can increase the formation of the ideal crystal structure. - If the amount is increased too much, excessive dissolution will occur, and crystals may not be obtained, or other crystal phases, such as ANA type zeolite, which is a more stable structure, will be generated. In addition, the reactivity of dissolved alumina is higher than that of silicon oxide, and alumina is easy to enter the crystal. Therefore, by properly adjusting the OH - The crystallization and redissolution rates can be adjusted to optimize the ratio of silicon oxide to aluminum oxide that enters the crystals, thereby optimizing the SAR of the synthesized GIS-type zeolite.
[0137] If the ratio of water to alumina (H2O / Al2O3) is high, the components in the mixed gel are more easily dispersed, but if it is too high, the crystallization rate will be significantly reduced. Therefore, in order to synthesize GIS-type zeolite with the best SAR and the best crystal structure, it is necessary to control the H2O / OH ratio. - While controlling H2O / Al2O3 to the optimum level.
[0138] Based on the above aspects, H2O / Al2O3 and H2O / OH - Preferably, 100≦H2O / Al2O3≦780 and 50≦H2O / OH-≦1000, more preferably 120≦H2O / Al2O3≦778 and 60≦H2O / OH-≦800, and further preferably 150≦H2O / Al2O3≦775 and 70≦H2O / OH- - ≦700.
[0139] The ratio of the silica source to the aluminum source in the mixed gel is expressed as the molar ratio of the oxides of each element, i.e., SiO2 / Al2O3. (It should be noted that the ratio in the synthesized zeolite is not consistent with the silica-alumina ratio of the mixed gel. The silica-alumina ratio of the synthetic zeolite is determined by other compositions and synthesis conditions.)
[0140] The SiO2 / Al2O3 ratio in the mixed gel is not particularly limited as long as it can form zeolite. It is preferably 3.0 to 70.0, more preferably 3.5 to 65.0, and even more preferably 4.0 to 60.0, because it tends to suppress the formation of zeolite having a skeleton different from the GIS-type skeleton.
[0141] The ratio of the aluminum source to the alkali metal and alkaline earth metal in the mixed gel is expressed as the molar ratio of the sum of M12O and M2O to Al2O3, i.e., (M12O+M2O) / Al2O3 (here, M1 represents an alkali metal and M2 represents an alkaline earth metal. They are calculated in the form of oxides). It should be noted that from the perspective of making it easier to crystallize a GIS-type framework, the (M12O+M2O) / Al2O3 is preferably greater than 1.5, more preferably greater than 1.6, and further preferably 1.65. From the perspective of being able to inhibit the formation of zeolites having a framework different from the GIS-type framework, the (M12O+M2O) / Al2O3 is preferably less than 15.0, more preferably less than 12.0, and further preferably less than 10.0.
[0142] The ratio of the phosphorus source to the aluminum source in the mixed gel is expressed as the molar ratio of the oxides of each element, i.e., P2O5 / Al2O3. The P2O5 / Al2O3 ratio is not particularly limited as long as it is a ratio capable of forming zeolite, but is preferably less than 1.0, more preferably 0.6 or less, further preferably 0.4 or less, and particularly preferably 0, because it tends to suppress the formation of zeolite having a framework different from the GIS-type framework.
[0143] When the mixed gel contains an organic structure directing agent, the ratio of the aluminum source to the organic structure directing agent in the mixed gel is expressed as the molar ratio of the organic structure directing agent to Al2O3, i.e., R / Al2O3 (here, R represents the organic structure directing agent). From the perspective of making the crystal formation of the GIS-type skeleton easier, and / or shortening the synthesis time, and improving the economic efficiency when manufacturing zeolite, it is preferably less than 7.0, more preferably less than 6.0, and further preferably less than 5.0. When an organic structure directing agent is used, the organic structure directing agent remains in the pores of the zeolite, carbon dioxide does not enter the pores, and the adsorption amount is reduced. In order to remove the organic structure directing agent, it is necessary to heat to at least 400°C, but GIS-type zeolite will undergo crystal fragmentation and become amorphous at above 350°C, so it is preferably less than the organic structure directing agent. From this perspective, R / Al2O3 is preferably less than 4.0, more preferably less than 3.5, and further preferably less than 3.0.
[0144] As described above, the method for producing GIS type zeolite of the present embodiment includes a step of preparing a mixed gel, wherein the mixed gel contains a silicon oxide source containing silicon, an aluminum source containing aluminum, an alkali source containing at least one selected from alkali metals (M1) and alkaline earth metals (M2), a salt compound containing at least one selected from alkali metals (M1) and alkaline earth metals (M2), a phosphorus source, and water, wherein the molar ratio of each component in the mixed gel is calculated in the form of oxides of each element with respect to the silicon, aluminum, alkali metal (M1) and alkaline earth metal (M2), and phosphorus source, and is given by the following formulas (1), (2), (3), (4), (5), and (6): The molar ratios α, β, γ, δ, ε, and ζ preferably satisfy 0.1≦α≦100.0, 3.0≦β≦70.0, 1.5≦γ≦15.0, 0≦δ<1.0, 100≦ε≦780, and 50≦ζ≦1000, and more preferably satisfy 0.5≦α≦80.0, 3.5≦β≦65 .0, 1.6≦γ≦12.0, 0≦δ≦0.6, 120≦ε≦778 and 60≦ζ≦800, and more preferably 0.8≦α≦50, 4.0≦β≦60.0, 1.65≦γ≦10.0, 0≦δ≦0.4, 150≦ε≦775 and 70≦ζ≦700. The GIS type zeolite of the present embodiment is particularly preferably obtained by the method for producing the GIS type zeolite of the present embodiment described above.
[0145] α=E / Al2O3 (1)
[0146] β=SiO2 / Al2O3 (2)
[0147] γ=(M12O+M2O) / Al2O3 (3)
[0148] δ=P2O5 / Al2O3 (4)
[0149] ε=H2O / Al2O3 (5)
[0150] ζ=H2O / OH- (6)
[0151] In the method for producing GIS-type zeolite of the present embodiment, when the molar ratios α, β, γ, δ, ε, and ζ satisfy the above ranges and the mixed gel further contains an organic structure directing agent R, the molar ratio η represented by the following formula (7) preferably satisfies η≦4.
[0152] η=R / Al2O3 (7)
[0153] The mixed gel does not necessarily need to contain seed crystals, and a preliminarily produced GIS type zeolite may be added as seed crystals to the mixed gel to obtain the GIS type zeolite of the present embodiment.
[0154] [Hybrid Gel Preparation Process]
[0155] The preparation process of the mixed gel is not particularly limited, and may include, for example, the following steps: a mixing process of mixing a silicon oxide source, an aluminum source, a salt compound, water, and, if necessary, a phosphorus source, an alkali source, and an organic structure directing agent at one time or in multiple stages; and a aging process of the mixture obtained in the mixing process.
[0156] In the mixing step, the components including the silicon oxide source, the aluminum source, the salt compound, water, and, if necessary, the phosphorus source, the alkali source, and the organic structure-directing agent may be mixed at once or in multiple stages.
[0157] The order when mixing in multiple stages is not limited, and can be suitably selected according to the conditions used. When mixing in multiple stages, it can be carried out with or without stirring. When stirring, as long as it is a commonly used stirring method, it is not particularly limited. As a specific example, a method using paddle stirring, vibration stirring, swing stirring, centrifugal stirring, etc. can be cited.
[0158] The rotation speed of stirring is not particularly limited as long as it is a stirring speed generally used, and for example, it may be 1 rpm or more and less than 2000 rpm.
[0159] The temperature in the mixing step is not particularly limited as long as it is a temperature generally used, and for example, it may be -20°C or higher and lower than 80°C.
[0160] The time of the mixing step is not particularly limited and can be appropriately selected according to the temperature of the mixing step. For example, it can be greater than 0 minutes and 1000 hours or less.
[0161] The aging process can be carried out under standing or stirring. When stirring is carried out in the aging process, there is no particular limitation as long as it is a commonly used stirring method. Specific examples include methods using paddle stirring, vibration stirring, swing stirring, centrifugal stirring, and the like.
[0162] The rotation speed of stirring is not particularly limited as long as it is a stirring speed generally used, and for example, it may be 1 rpm or more and less than 2000 rpm.
[0163] The temperature of the aging step is not particularly limited as long as it is a temperature generally used, and for example, it may be -20°C or higher and lower than 80°C.
[0164] The time of the aging step is not particularly limited and can be appropriately selected according to the temperature of the aging step. For example, it can be greater than 0 minutes and 1000 hours or less.
[0165] It is believed that zeolite produces the dissolution of raw materials, the generation and redissolution of zeolite precursors in the mixing process and the aging process of raw materials. In order to form a large periodic structure containing 8-membered rings without generating defects, it is preferred not to excessively form the zeolite precursor. In addition, in the case of excessively forming the zeolite precursor, the generation of ANA type zeolite, which is a more stable structure, tends to increase, so it is also preferred not to over-mature. On the other hand, it is preferred that the raw materials are fully mixed and the raw material gel is in a uniform state. Regarding the time for the mixing process and the aging process to be combined, as long as it is appropriately adjusted based on the composition of the raw materials to obtain a zeolite of a suitable structure, there is no particular limitation. The above time is representatively preferably more than 1 minute and less than 24 hours, more preferably more than 3 minutes and less than 23 hours, more preferably more than 10 minutes and less than 18 hours, more preferably more than 12 minutes and less than 15 hours, and more preferably more than 20 minutes and less than 6 hours.
[0166] [Hydrothermal synthesis process]
[0167] The method for producing GIS-type zeolite of the present embodiment preferably further comprises a hydrothermal synthesis step at a hydrothermal synthesis temperature of 80° C. to 200° C., and the hydrothermal synthesis temperature is more preferably 100° C. to 180° C. That is, the mixed gel obtained by the preparation step is preferably subjected to hydrothermal synthesis by being kept at a predetermined temperature for a predetermined time in a stirring or static state.
[0168] The temperature of the hydrothermal synthesis is not particularly limited as long as it is a temperature commonly used, but is preferably 80° C. or higher from the perspective of shortening the synthesis time and being economical in the production of zeolite. From the perspective of being able to suppress the formation of zeolites having a framework different from the GIS-type framework, it is more preferably 90° C. or higher, and even more preferably 100° C. or higher. From the perspective of being able to suppress the formation of zeolites having a framework different from the GIS-type framework, it is more preferably 200° C. or lower, even more preferably 180° C. or lower, and even more preferably 170° C. or lower. The temperature of the hydrothermal synthesis may be constant or may be changed in stages.
[0169] The time of the hydrothermal synthesis is not particularly limited as long as it is a time commonly used, and can be appropriately selected according to the temperature of the hydrothermal synthesis. The time of the hydrothermal synthesis is preferably 3 hours or more, more preferably 10 hours or more, from the aspect of forming the GIS skeleton. From the aspect of obtaining a highly crystalline GIS-type zeolite, it is further preferably 24 hours or more. From the aspect of excellent economic efficiency during zeolite production, the time of the hydrothermal synthesis is preferably 30 days or less, more preferably 20 days or less, and further preferably 10 days or less.
[0170] In the hydrothermal synthesis step, the container for placing the mixed gel is not particularly limited as long as it is a commonly used container, but when the pressure in the container is increased at a predetermined temperature, or when the gas that does not hinder crystallization is pressurized, it is preferably placed in a pressure-resistant container for hydrothermal synthesis. The pressure-resistant container is not particularly limited, and various shapes such as spherical, vertically elongated, and horizontally elongated can be used.
[0171] When the mixed gel in the pressure-resistant container is stirred, the pressure-resistant container is rotated in the vertical direction and / or the horizontal direction, preferably in the vertical direction. When the pressure-resistant container is rotated in the vertical direction, the rotation speed is not particularly limited as long as it is within the commonly used range, preferably 1 to 50 rpm, more preferably 10 to 40 rpm.
[0172] In the hydrothermal synthesis step, when the mixed gel is preferably stirred, there can be mentioned a method of using a vertically long container as a pressure-resistant container and rotating the container in the up-and-down direction.
[0173] [Separation and drying process]
[0174] After the hydrothermal synthesis step, the solid product and the liquid containing water are separated. The separation method is not particularly limited as long as it is a common method, and filtration, decantation, spray drying (rotary spray, nozzle spray and ultrasonic spray, etc.), drying using a rotary evaporator, vacuum drying, freeze drying or natural drying, etc. can be used. Separation can usually be carried out by filtration or decantation.
[0175] The separated product can be used directly or washed with water or a prescribed solvent. The separated product can be dried if necessary. The temperature for drying the separated product is not particularly limited as long as it is a temperature at which drying is usually performed, and is usually room temperature to below 150° C. The atmosphere during drying is not particularly limited as long as it is a commonly used atmosphere, and an air atmosphere or an atmosphere containing an inert gas such as nitrogen or argon or oxygen is usually used.
[0176] [Firing process]
[0177] GIS type zeolite can be used after being calcined as needed. The calcination temperature is not particularly limited as long as it is a commonly used temperature. When it is desired to remove the organic structure directing agent, it is preferably 300°C or more, more preferably 350°C or more, because it can reduce the residual ratio. From the perspective of shortening the calcination time and excellent economic efficiency when manufacturing zeolite, it is more preferably 360°C or more. Because it tends to maintain the crystallinity of the zeolite, it is preferably less than 450°C, more preferably 420°C or less, and even more preferably 400°C or less.
[0178] The calcination time is not particularly limited as long as it is a time that can sufficiently remove the organic structure directing agent, and can be appropriately selected according to the calcination temperature. Since it tends to reduce the residual ratio of the organic structure directing agent, it is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 3 hours or more. Since it tends to maintain the crystallinity of the zeolite, it is preferably 10 days or less, more preferably 7 days or less, and even more preferably 5 days or less.
[0179] The firing atmosphere is not particularly limited as long as it is a commonly used atmosphere, and an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is usually used.
[0180] [Cation Exchange]
[0181] Cation exchange can be performed as needed to make the GIS type zeolite a desired cationic type. Cation exchange can use, but is not limited to, carbonates such as sodium carbonate, potassium carbonate, lithium carbonate, rubidium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, and ammonium carbonate; or nitrates such as sodium nitrate, potassium nitrate, lithium nitrate, rubidium nitrate, cesium nitrate, magnesium nitrate, calcium nitrate, strontium nitrate, barium nitrate, and ammonium nitrate; or salts formed by changing carbonate ions and nitrate ions contained in the above carbonates and nitrates to halide ions, sulfate ions, carbonate ions, bicarbonate ions, acetate ions, phosphate ions, or hydrogen phosphate ions; acids such as nitric acid or hydrochloric acid.
[0182] The temperature for cation exchange is not particularly limited as long as it is a normal cation exchange temperature, and is usually room temperature to 100° C. or lower.
[0183] When separating the zeolite after cation exchange, the separation method is not particularly limited as long as it is a common method, and filtration, decantation, spray drying (rotary spray, nozzle spray and ultrasonic spray, etc.), drying using a rotary evaporator, vacuum drying, freeze drying or natural drying, etc. can be used. Separation can usually be carried out by filtration or decantation.
[0184] The separated product can be used directly or washed with water or a specified solvent. If necessary, the separated product can be dried.
[0185] The temperature for drying the separated product is not particularly limited as long as it is a normal drying temperature, and is usually room temperature to 150° C. or lower.
[0186] The atmosphere during drying is not particularly limited as long as it is a commonly used atmosphere, and generally, an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is used.
[0187] Furthermore, the ammonium-type zeolite can be converted into the proton-type zeolite by calcining the zeolite.
[0188] (Carrier)
[0189] The zeolite molded body of the present embodiment preferably includes a carrier. Examples of the carrier include inorganic binders and organic binders.
[0190] As inorganic binders, for example, inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, titanium dioxide, clay minerals such as bentonite and kaolin, calcium silicate, and calcium aluminate can be cited. As aluminum oxide, for example, α-alumina, γ-alumina, boehmite, pseudo-boehmite, bayerite, gibbsite, and diaspore can be cited. As silicon oxide, for example, colloidal silica, water glass, gas phase silica, silica sol, wet silica, dry silica, and natural silica can be cited. These inorganic binders can be used alone or in combination. Among these inorganic binders, aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium dioxide are preferred from the aspect of improving the strength of the zeolite molded body, and silicon oxide and aluminum oxide are more preferred.
[0191] The content of the inorganic binder is preferably 1 to 99% by mass, more preferably 5 to 90% by mass, and even more preferably 8 to 80% by mass, based on the total amount (100% by mass) of the zeolite molded body.
[0192] As organic binder, for example, cellulose, methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, latex, polyvinyl alcohol, vinyl acetate, polyvinyl acetal, vinyl chloride, acrylic, polyamide, urea, melamine, phenol resin, polyester, polyurethane, polyamide, polybenzimidazole, chloroprene rubber, acrylonitrile-butadiene rubber, styrene-butadiene rubber, polysulfide, butyl rubber, silicone rubber, acrylic rubber, urethane rubber can be enumerated. These organic binders can be used alone, and a plurality of combinations can also be used. Among these organic binders, from the aspect of the surface bonding with GIS type zeolite, preferred cellulose, methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, polyvinyl alcohol, more preferably cellulose, methylcellulose and polyvinyl alcohol.
[0193] The content of the organic binder is preferably 1 to 99% by mass, more preferably 5 to 90% by mass, and even more preferably 8 to 80% by mass, based on the total amount (100% by mass) of the zeolite molded body.
[0194] From the viewpoint of obtaining a desired density, the carrier preferably contains an inorganic binder and an organic binder. That is, it is preferred that the carrier contains one or more of each of the inorganic binder and the organic binder.
[0195] The total content of the carrier is preferably 1 to 99% by mass, more preferably 5 to 90% by mass, and further preferably 8 to 80% by mass relative to the total amount (100% by mass) of the zeolite molded body. If the content of the carrier is increased, the strength of the molded body tends to increase, but the content of the zeolite itself tends to decrease. Therefore, the content of the carrier can be adjusted according to the strength and performance required by the application.
[0196] The shape of the zeolite molded body is not particularly limited, and examples thereof include spherical, cylindrical, elliptical, straw-bale, trilobal, ring, powder, etc. Among these, spherical and cylindrical shapes are more preferred.
[0197] Spherical means that the aspect ratio of the molded body is in the range of 1 to 1.1. The aspect ratio of the molded body means that when the molded body is stably stationary on a horizontal plane, a projection image is taken in the vertical direction of the molded body, the projection image is sandwiched between two parallel straight lines that are connected to the projection image, and the interval between the parallel lines when the interval is the largest is the major diameter, and the interval between the parallel lines when the interval is the smallest is the minor diameter. The ratio of the major diameter to the minor diameter at this time is the aspect ratio. The above-mentioned roundness refers to the value obtained by dividing the difference between the maximum and minimum values of the diameters at any three locations measured with a micrometer with a minimum reading of 0.01 mm or less by 2.
[0198] The cross section obtained by cutting the molded body with a plane passing through any two points on the outer circumference of the molded body is preferably a circle with a roundness of 0.5 or less, more preferably a circle with a roundness of 0.4 or less, and even more preferably a circle with a roundness of 0.3 or less.
[0199] The size of the molded body is not particularly limited and varies depending on the state in which the molded body is used. For example, in a process using a molded body other than a fluidized state such as a fixed bed or a moving bed, a spherical shape with a diameter of 3 mm to 10 mm or a cylindrical shape with a length of 3 mm to 30 mm and a diameter of 1 mm to 30 mm is preferred.
[0200] The diameter of the sphere is more preferably 5 mm or more and 8 mm or less. The diameter of the sphere is the average value of the major axis and the minor axis used in calculating the aspect ratio of the molded product, and can be adjusted to the above range by, for example, classification or the like.
[0201] The length of the cylinder is more preferably 3 mm to 10 mm, and even more preferably 3 mm to 8 mm. The diameter of the cylinder is more preferably 2 mm to 4 mm.
[0202] The length and diameter can be measured by the vernier caliper method using a vernier caliper with a minimum reading of 0.1 mm or less for three samples, and the average values can be measured as the length and diameter, which can be adjusted to the above range by operations such as classification.
[0203] In a process in which the molded body is made to flow using a fluidized bed or the like, particles having a particle size of 20 μm or more and 300 μm or less are preferred. The particle size is more preferably 20 μm or more and 200 μm or less, and further preferably 30 μm or more and 100 μm or less. The particle size can be measured using a laser diffraction / scattering particle size analyzer (MT3000 manufactured by Microtrac) according to the attached operating manual in terms of median diameter (D 50 ) form for determination.
[0204] The compressive strength of the zeolite molded body of the present embodiment is preferably 1.0 MPa or more, more preferably 2.2 MPa or more, and even more preferably 3.4 MPa or more. In particular, when the zeolite molded body of the present embodiment is in powder form, it preferably satisfies the above range.
[0205] The compressive strength can be measured 20 times using a micro compression tester (MCT-W500 manufactured by Shimadzu Corporation, compression strength measurement) and measured as an average of the obtained values, and can be adjusted to the above range by, for example, the firing temperature and firing time.
[0206] The breaking strength of the zeolite molded body of the present embodiment is preferably 5 N or more, more preferably 10 N or more, and further preferably 20 N or more. In particular, when the zeolite molded body of the present embodiment is a pellet, it preferably satisfies the above range.
[0207] The above-mentioned breaking strength can be measured 20 times using a digital hardness meter (KHT-40N manufactured by Fujiwara Manufacturing Co., Ltd., with a 3 mm indenter and breaking strength measurement), and the measurement is performed as an average value of the obtained values. The above-mentioned range can be adjusted by, for example, the firing temperature and the firing time.
[0208] [Method for producing zeolite molded body]
[0209] The method for producing the zeolite molded body of the present embodiment is not particularly limited and may include the following steps: a raw material mixing step (X), in which the zeolite of the present embodiment is mixed with other optional components (e.g., a carrier) for preparation; a molding treatment step (Y), in which the prepared raw materials are subjected to molding treatment to obtain a precursor; and a firing step (Z), in which the above-mentioned precursor is fired to obtain a zeolite molded body.
[0210] In addition, as a method for producing a zeolite molded body, when obtaining the desired zeolite molded body, molding can be performed, for example, by extrusion molding, injection molding, injection casting, tumbling granulation, compression molding, spray drying, or a method in which two or more of these methods are combined.
[0211] In the zeolite molded body of the present embodiment, the apparent density da , true density d t , apparent density d / true density d t , bulk density d b , bulk density d b / True density d t The apparent density d is adjusted by the selection of the carrier, the selection of the granulation method, etc. a The method is not particularly limited to the range specified, and there is a method of selecting a carrier with high affinity for zeolite. By selecting a carrier with high affinity, the mixture of zeolite and the carrier shows excellent shape retention, and the apparent density d of the molded body is a improve.
[0212] In order to make the true density d t The method for achieving the predetermined range is not particularly limited, and there is a method of adjusting the type and amount of the carrier, for example.
[0213] In order to make the apparent density d a / True density d t The method is not particularly limited to the range specified. For example, there are the following methods: when mixing with the zeolite in the present embodiment, a method of selecting a carrier that can be granulated into any shape with a lower water content, or a method of selecting a granulation method that can be granulated with a lower water content. The lower the water content during granulation, the smaller the distance between the zeolite and carrier particles, and the smaller the voids in the molded body, so the apparent density d a / True density d t improve.
[0214] In order to make the packing density d b The method is not particularly limited to the predetermined range. For example, there is a method of adjusting the size of the molded body. By adjusting the size of the molded body to be sufficiently small relative to the size of the container to be filled, the molded body can be densely filled in the container, and the bulk density d b improve.
[0215] In order to make the packing density d b / True density d t The method is not particularly limited to the predetermined range. For example, there is a method of granulating a molded body that is sufficiently small relative to the size of the container to be filled with a smaller water content. By granulating with a small water content, the voids inside the molded body are reduced, and the molded body is made sufficiently small relative to the size of the container to be filled, so that it can be densely filled in the container, and the bulk density d b / True density d t improve.
[0216] [Raw material mixing step (X)]
[0217] In the raw material mixing step (X), the raw materials used can be used in a state corresponding to the preparation method, such as powder, solvent dispersion, sol, liquid, etc. Among the raw materials used, for example, when an inorganic adhesive is used, it is used in a state corresponding to the preparation method, such as powder, solvent dispersion, sol, liquid, etc., but from the perspective of ease of handling, powder and sol are preferred. These inorganic adhesives can be used alone or in combination. The temperature for mixing the raw materials is not particularly limited, for example, preferably 10°C to 80°C, more preferably 15°C to 60°C. For example, if the state of the raw materials after mixing is a slurry, such as spray drying, when the temperature of the raw materials is below 80°C, there is a tendency to suppress the evaporation of water in the raw materials, and when the temperature of the raw materials is above 10°C, there is a tendency to suppress freezing in the slurry. In addition, for example, if the raw materials are mixed in a clay state from a chain state to a capillary state, such as in an extrusion molding process, when the temperature of the raw materials is below 80°C, there is a tendency to suppress the evaporation of water from the clay and easily keep the water content in the clay constant. When the temperature of the raw materials is above 10°C, there is a tendency to suppress the freezing of water in the clay. As a stirring means when preparing the raw materials, any means can be used. For example, if the state of the raw materials after mixing is a slurry, such as in a spray drying process, a stirring paddle is preferably cited. As the paddle used in stirring, specifically, a propeller shape, an impeller shape, a flat blade paddle shape, a turbine shape, a cone shape, etc. can be cited. In addition, in order to perform effective stirring, a baffle plate, etc. can be set in the tank. Regarding the number of stirrers, the optimal conditions can be selected according to the size of the catalyst raw material liquid tank, the shape of the stirring paddle, etc. In this embodiment, the total stirring time of the raw materials is preferably 1 minute to 24 hours, more preferably 10 minutes to 5 hours, and further preferably 15 minutes to 3 hours. When the stirring time of the mixed solution is more than 1 minute, the composition of the raw materials tends to become uniform; when it is less than 24 hours, the influence of the evaporation of water in the raw materials tends to decrease. In addition, for example, in the case of a clay-like state from a chain state to a capillary state after the raw materials are mixed, such as in an extrusion molding process, it is preferred to select a mixer, a kneading machine, etc. according to the state of the raw materials. In the present embodiment, the total mixing and kneading time of the raw materials is preferably 1 minute to 24 hours, more preferably 2 minutes to 5 hours, and further preferably 3 minutes to 3 hours. When the stirring time of the mixed solution is more than 1 minute, the composition of the raw materials tends to become uniform, and when it is less than 24 hours, the influence of the evaporation of water in the raw materials tends to decrease. In addition, in the case of an organic binder such as methyl cellulose that is easily gelled due to heat, the gelation of the organic binder can be suppressed by maintaining the internal temperature of the mixer, the kneading machine, etc. at a value lower than the thermal gelation temperature of the organic binder, and there is a tendency to easily obtain a raw material of uniform composition.
[0218] The clay-like raw material may be left to stand and mature. By aging, water can easily reach between the raw zeolites, which tends to improve the moldability. In addition, water can be replaced with air or other gas existing between the zeolites to obtain a denser molded body.
[0219] [Molding process (Y)]
[0220] Examples of the molding treatment in the molding treatment step (Y) include extrusion molding treatment, compression molding treatment, and spray drying treatment.
[0221] The extrusion molding process is not particularly limited. For example, depending on the properties of the raw material used (also referred to as "raw clay" in the extrusion molding process), the temperature during extrusion molding is preferably 10° C. to 80° C., and more preferably 15° C. to 75° C. The water content in the raw clay is preferably 35% to 50% by mass, and more preferably 38% to 45% by mass. When the water content is 50% by mass or less, the softness of the raw clay can be prevented from being excessively increased, and the moldability tends to be improved. When the water content is 35% by mass or more, the softness of the raw clay can be prevented from being moderately reduced, and the moldability tends to be improved.
[0222] When extrusion molding is used as the molding process step (Y), there is no particular limitation on the extrusion molding machine, and examples thereof include screw type, roller type, scraper type, self-molding type, plunger type, disc granulation type, etc. Among these, it is particularly preferred to implement the extrusion molding process using a roller type, screw type, or disc granulation type extrusion molding machine.
[0223] When compression molding is used as the molding step (Y), the compression molding machine is not particularly limited, and examples thereof include uniaxial press molding, hot press molding, and the like.
[0224] In the spray drying process, for example, the atomization of the slurry can be carried out by methods such as a rotating disk method, a two-fluid nozzle method and a high-pressure nozzle method which are usually implemented in industry, and is particularly preferably carried out by a rotating disk method. As a drying heat source in the drying of the droplets obtained by spraying, air heated by steam, an electric heater, etc. is preferably used. The temperature at the inlet of the dryer can be in the range of 100°C to 400°C, preferably 150°C to 300°C. The temperature at the outlet of the dryer can be in the range of 40°C to 150°C, preferably 50°C to 130°C.
[0225] [Firing process (Z)]
[0226] The firing temperature in the firing step (Z) is not particularly limited as long as it is a temperature commonly used, but is preferably less than 550° C., more preferably 530° C. or less, and even more preferably 500° C. or less, because it tends to maintain the crystallinity of the zeolite while ensuring strength. The firing temperature is preferably 110° C. or more, and more preferably 120° C. or more.
[0227] The calcination time in the calcination step (Z) is not particularly limited as long as it is a time for the carrier to be fully dried or sintered, and can be appropriately selected according to the calcination temperature. Since it tends to be able to maintain the crystallinity of the zeolite while ensuring the strength, it is preferably 20 days or less, more preferably 10 days or less, and even more preferably 7 days or less.
[0228] The firing atmosphere in the firing step (Y) is not particularly limited as long as it is an atmosphere commonly used, and an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is usually used.
[0229] The firing in the firing step (Z) can be performed using a firing furnace such as a rotary furnace, a tunnel furnace, or a muffle furnace.
[0230] The use of the zeolite molded body of this embodiment is not particularly limited, and it can be used, for example, as a separator or separation membrane for various gases and liquids, an electrolyte membrane for fuel cells, etc., a filler for various resin molded bodies, a membrane reactor, or a catalyst for hydrogen cracking, alkylation, etc., a catalyst carrier for loading metals, metal oxides, etc., an adsorbent, a desiccant, a detergent builder, an ion exchanger, a wastewater treatment agent, a fertilizer, a food additive, a cosmetic additive, etc.
[0231] Among the above, the zeolite molded body of the present embodiment can be suitably used as an adsorbent.
[0232] [Adsorption device]
[0233] The adsorption device of the present embodiment includes the zeolite molded body of the present embodiment. Since the adsorption device of the present embodiment is configured as described above, carbon dioxide can be sufficiently adsorbed, and the selectivity of carbon dioxide adsorption relative to the adsorption amount of methane is high. Therefore, for example, it can be particularly preferably used for the purpose of selectively removing carbon dioxide from natural gas.
[0234] The adsorption device of the present embodiment includes a zeolite molded body including the zeolite of the present embodiment, which can be Figure 1 The configuration example shown. Figure 1The adsorption device 2 of the present embodiment illustrated in the example has filters 23 arranged at two locations, the inlet side and the outlet side, and a plurality of zeolite molded bodies 24 filled between the two filters 23, inside the container 21. As the filter 23, for example, a filter made of quartz can be used. For example, when the adsorption device 2 is used to separate carbon dioxide from natural gas, natural gas can be introduced from an upper pipeline, and after impurities are removed by the filter 23, carbon dioxide is further selectively adsorbed and removed by the zeolite molded body 24, and methane-rich gas is taken out from the lower pipeline. However, the object supplied to the adsorption device is not limited to natural gas, and the internal structure of the adsorption device is not limited to natural gas. Figure 1 The adsorption device 2 of the present embodiment may be the purified gas production device 100 described later.
[0235] [Method for producing purified gas]
[0236] In the method for producing a purified gas according to the present embodiment, an adsorption device including the zeolite according to the present embodiment is used to separate one or more selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, CO and hydrocarbons. In the present embodiment, it is preferred to separate one or more selected from the group consisting of CO2 and H2O from one or more gases selected from the group consisting of N2, O2, CO and hydrocarbons. It should be noted that the hydrocarbon is not particularly limited, and examples thereof include methane, ethane, ethylene, propane, propylene, 1-butene, 2-butene, 2-methylpropylene, dimethyl ether, acetylene and the like.
[0237] In the GIS type zeolite of the present embodiment, the adsorption capacity of CO2 is particularly large, and physical adsorption without chemical bonding is observed. There is no particular limitation on the separation method using the zeolite of the present embodiment, and a method with low energy and excellent economic efficiency during the regeneration of the adsorbent material is preferred. There is no particular limitation on the specific example of the method, and it is preferred to use any one of a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method. The pressure swing adsorption separation method (PSA: Pressure Swing Adsorption) refers to the following method: the pressure during gas desorption is lower than the pressure during adsorption, and the gas is separated by using the difference between the adsorption amount at high pressure and the adsorption amount at low pressure. In addition, the temperature swing adsorption separation method (TSA: Thermal Swing Adsorption) refers to the following method: the temperature during gas desorption is higher than the temperature during adsorption, and the gas is separated by using the difference between the adsorption amount at low temperature and the adsorption amount at high temperature. In addition, the method of combining them is a pressure swing-temperature swing adsorption separation method (PTSA: Pressure and Thermal Swing Adsorption). These methods can be implemented under various known conditions.
[0238] The method for producing a purified gas according to the present embodiment is a method for producing a purified gas by using an adsorption tower filled with an adsorbent including zeolite to separate the carbon dioxide and the second component gas from a mixed gas including carbon dioxide and a second component gas different from carbon dioxide, wherein the method comprises the following steps:
[0239] an adsorption step of introducing the mixed gas into the adsorption tower, allowing the carbon dioxide to be adsorbed on the adsorbent, and taking out the second component gas; and
[0240] In the desorption step, the carbon dioxide is exhausted from the adsorption tower under reduced pressure, thereby removing the carbon dioxide from the adsorbent.
[0241] In the purified gas production method of this embodiment, the above-mentioned zeolite molded body is used as an adsorbent. By using a zeolite molded body having excellent embrittlement resistance to carbon dioxide adsorption, the purified gas production method of this embodiment can reduce the replacement frequency of the zeolite molded body, etc., and the maintenance management of the device becomes easy.
[0242] In the method for producing a purified gas according to the present embodiment, it is preferable to use as the adsorbent an adsorbent having an apparent density d a / True density d t A zeolite molded body having a ratio of 0.36 or more, or a bulk density d b / True density d tThe ratio of zeolite to carbonyl ether is 0.25 or more. By the above configuration, the second component gas can be obtained at a high yield, and high-purity CO2 can be recovered.
[0243] The above apparent density d a , bulk density d b , and true density d t , apparent density d a / True density d t ratio, bulk density d b / True density d t The ratio is preferably in the same range as described for the zeolite molded body.
[0244] <Second Component Gas>
[0245] The second component gas may be a gaseous substance different from carbon dioxide. "Gaseous substance" refers to a substance that is a gas at room temperature 25°C and normal pressure. Examples of the second component gas include methane, ethane, nitrogen, carbon monoxide, hydrogen, argon, and dimethyl ether. Among these second component gases, methane, ethane, and nitrogen are preferred, methane and ethane are more preferred, and methane is further preferred.
[0246] <Mixed gas>
[0247] The mixed gas used as a raw material contains carbon dioxide and a second component gas.
[0248] The content of carbon dioxide in the mixed gas may be 1% to 99% by volume, 5% to 90% by volume, 10% to 80% by volume, 20% to 70% by volume, or 30% to 70% by volume.
[0249] The content of the second component gas in the mixed gas may be 1% to 99% by volume, 5% to 90% by volume, 10% to 80% by volume, 20% to 70% by volume, or 30% to 70% by volume.
[0250] The water content of the mixed gas is preferably 1000 volume ppm or less, more preferably 500 volume ppm or less, and further preferably 100 volume ppm or less. With the water content in this range, the adsorption performance of the adsorbent can be exerted to a high degree. The water content of the mixed gas is measured by, for example, a dew point meter, and can be converted into a water content using the method described in JIS Z8806:2001.
[0251] <Adsorption Tower>
[0252] The adsorption tower is filled with an adsorbent. The adsorption tower is constructed in such a way that a mixed gas can be introduced and the adsorbent can be brought into contact with the mixed gas. By bringing the mixed gas into contact with the adsorbent in the adsorption process, carbon dioxide in the mixed gas can be adsorbed on the adsorbent. Since the carbon dioxide in the mixed gas is adsorbed, the second component gas can be taken out. In addition, after the adsorption process, the carbon dioxide can be taken out by reducing the pressure of the adsorption tower in the desorption process. In this way, a purified gas of the second component gas and a purified gas of carbon dioxide are obtained by utilizing the adsorption process and the desorption process. It should be noted that the adsorption tower may also be provided with a heater to increase the temperature inside the adsorption tower.
[0253] <Conditions of Adsorption and Desorption Processes>
[0254] The adsorption process and the desorption process can be repeated more than one time. The mixed gas is circulated in the adsorption tower, and the adsorption process of carbon dioxide is performed at a pressure close to normal pressure. Next, the adsorption tower is reduced in pressure, and a desorption process of desorbing carbon dioxide from the adsorbent is performed. By repeatedly performing the adsorption process and the desorption process in this way, carbon dioxide and the second component gas are separated. By using the zeolite molded body of this embodiment, the recovery purity of carbon dioxide and the recovery rate of the second component gas can be improved.
[0255] Final pressure P in the desorption process b It is preferably 50 kPa or less, more preferably 30 kPa or less, further preferably 20 kPa or less, further preferably 15 kPa or less, further preferably 10 kPa or less, further preferably 5 kPa or less, further preferably 3 kPa or less. The final pressure P b It refers to the pressure near the exhaust outlet of the adsorption tower filled with adsorbent when the pressure is reduced and exhausted. It means that the pressure of the adsorption tower is gradually reduced by the pressure reduction and exhaust and finally reaches a constant pressure.
[0256] From the perspective of improving the desorption efficiency of carbon dioxide and reducing the power of each unit of mixed gas to be treated, the average temperature in the desorption process is preferably above 0°C, preferably 10°C to 400°C, more preferably 25°C to 300°C, and more preferably 25°C to 200°C. The average temperature in the desorption process refers to the average temperature of the desorbed gas (carbon dioxide) near the outlet of the adsorption tower in the desorption process. It should be noted that in the desorption process, there is heat absorption due to the desorption of carbon dioxide from the adsorbent, so the temperature may change slowly.
[0257] Adsorption pressure P in the adsorption process a It is preferably 50 to 3000 kPa, more preferably 60 to 500 kPa or less, and even more preferably 70 to 200 kPa or less. aIt refers to the pressure near the inlet of the adsorption tower where the mixed gas is introduced.
[0258] From the perspective of improving the desorption efficiency of carbon dioxide in the subsequent desorption process and reducing the power per unit of mixed gas to be treated, the average temperature in the adsorption process is preferably above 0°C, preferably 10°C to 400°C, more preferably 25°C to 300°C, and more preferably 25°C to 200°C. The average temperature in the adsorption process refers to the average temperature of the gas near the outlet of the adsorption tower in the adsorption process. It should be noted that in the adsorption process, heat is released due to the adsorption of carbon dioxide to the adsorbent, so the temperature may change slowly.
[0259] In the method for producing purified gas of the present embodiment, the total recovery rate of carbon dioxide from the mixed gas is preferably 90% or more, more preferably 93% or more, and further preferably 95% or more. The total recovery rate here refers to the total amount of carbon dioxide recovered relative to the total amount of carbon dioxide in the mixed gas introduced into the adsorption tower.
[0260] In the method for producing a purified gas according to the present embodiment, the total recovery rate of the second component gas from the mixed gas is 90% or more, more preferably 93% or more, and even more preferably 95% or more.
[0261] The total recovery rate herein refers to the total amount of the second component gas recovered relative to the total amount of the second component gas in the mixed gas introduced into the adsorption tower.
[0262] In the method for producing a purified gas of the present embodiment, it is preferred that the total recovery rate of carbon dioxide from the mixed gas is 90% or more, and the total recovery rate of the second component gas from the mixed gas is 90% or more, more preferably the total recovery rate of carbon dioxide from the mixed gas is 93% or more, and the total recovery rate of the second component gas from the mixed gas is 93% or more, and further preferably the total recovery rate of carbon dioxide from the mixed gas is 95% or more, and the total recovery rate of the second component gas from the mixed gas is 95% or more.
[0263] The purity of the second component gas obtained by the method for producing a purified gas according to the present embodiment is preferably 90% by volume or more, more preferably 93% by volume or more, and even more preferably 95% by volume or more.
[0264] The purity of carbon dioxide obtained by the method for producing a purified gas according to the present embodiment is preferably 90% by volume or more, more preferably 92% by volume or more, and even more preferably 95% by volume or more.
[0265] The water content in the carbon dioxide obtained by the method for producing a purified gas of the present embodiment is preferably 500 volume ppm or less, more preferably 300 volume ppm or less, and further preferably 100 volume ppm or less. The water content in the carbon dioxide can be measured using, for example, a dew point meter. In the method for producing a purified gas, by using zeolite as an adsorbent, the water content in the carbon dioxide can be made lower than the above value.
[0266] The method for producing a purified gas according to the present embodiment can obtain a purified second component gas or purified carbon dioxide.
[0267] <Activation process>
[0268] The method for producing purified gas of the present embodiment preferably includes an activation step of increasing the temperature and reducing the pressure in the adsorption tower to separate the moisture from the above-mentioned adsorbent. The activation step can be used to activate the adsorbent, adsorb the moisture in the gas to be treated, and reduce the moisture in the obtained carbon dioxide and the second component gas. The activation step is preferably implemented before the above-mentioned adsorption step and desorption step. In addition, the adsorption step and the desorption step can be repeated, and the activation step can be implemented after the adsorbent has adsorbed a large amount of moisture.
[0269] Final pressure P in the activation process e It is preferably 50 kPa or less, more preferably 30 kPa or less, further preferably 20 kPa or less, further preferably 15 kPa or less, further preferably 10 kPa or less, further preferably 5 kPa or less, further preferably 3 kPa or less. The final pressure P e It refers to the pressure near the exhaust outlet of the adsorption tower filled with adsorbent when the pressure is reduced and exhausted. It means that the pressure of the adsorption tower is gradually reduced by the pressure reduction and exhaust and finally reaches a constant pressure.
[0270] The temperature in the adsorption tower in the activation step is preferably 150°C or higher, more preferably 180°C to 300°C, and even more preferably 200°C to 280°C.
[0271] [Pure gas production equipment]
[0272] Reference Figure 2 , a schematic structure of the purified gas manufacturing device 100 of this embodiment is described. The purified gas manufacturing device 100 has a mixed gas supply line 1, a carbon dioxide adsorption tower 3a and a carbon dioxide adsorption tower 3b, a carbon dioxide recovery line 5, a second component gas recovery line 7, and a decompression device 9.
[0273] The carbon dioxide adsorption tower 3a has a fixed bed 31a filled with an adsorbent that can be formed in contact with the mixed gas introduced into the interior. One end of the carbon dioxide adsorption tower 3a is connected to the mixed gas supply pipeline 1, and the other end is connected to the second component gas recovery pipeline 7. The second component gas recovery pipeline 7 is provided with an automatic valve AV3. In addition, the second component gas recovery pipeline 7 is provided with a flow meter 71, a moisture meter 72 and a component analyzer 73. As the component analyzer 73, an analyzer that can measure the concentration of carbon dioxide and the concentration of the second component gas can be used.
[0274] The carbon dioxide adsorption tower 3a is connected to the carbon dioxide recovery pipeline 5 at the end in the same direction as the end connected to the mixed gas supply pipeline 1. The mixed gas supply pipeline 1 is provided with a flow meter 11, a moisture meter 12, and a component analyzer 13. An automatic valve AV1 is provided at the entrance of the carbon dioxide adsorption tower 3a. On the other hand, a pressure reducing device 9 is connected to the carbon dioxide recovery pipeline 5, so that the carbon dioxide adsorption tower 3a has a structure capable of reducing pressure. It should be noted that the pressure reducing device 9 can also be a vacuum pump. In addition, the carbon dioxide recovery pipeline 5 connected to the carbon dioxide adsorption tower 3a is provided with an automatic valve AV5 and a pressure gauge 53a. Furthermore, the carbon dioxide recovery pipeline 5 is provided with a flow meter 51, a moisture meter 52 and a component analyzer 54. As the component analyzer 54, an analyzer capable of measuring the concentration of carbon dioxide and the concentration of the second component gas can be used.
[0275] The carbon dioxide adsorption tower 3b has a fixed bed 31b containing an adsorbent that can be formed in contact with the mixed gas introduced into the interior. An automatic valve AV2 is provided at the inlet of the carbon dioxide adsorption tower 3b. One end of the carbon dioxide adsorption tower 3b is connected to the mixed gas supply pipeline 1, and the other end is connected to the second component gas recovery pipeline 7. An automatic valve AV4 is provided in the second component gas recovery pipeline 7. The carbon dioxide adsorption tower 3b is also connected to the carbon dioxide recovery pipeline 5 at the end in the same direction as the end connected to the mixed gas supply pipeline 1. In addition, the carbon dioxide recovery pipeline 5 connected to the carbon dioxide adsorption tower 3b is provided with an automatic valve AV6 and a pressure gauge 53b.
[0276] Next, refer to Figure 2 , the operation of the purified gas manufacturing device 100 of the present embodiment is described. The mixed gas is supplied to the carbon dioxide adsorption tower 3a via the mixed gas supply pipeline 1. In addition, the carbon dioxide (CO2) contained in the mixed gas is adsorbed by the adsorbent filled in the carbon dioxide adsorption tower 3a, and the second component gas such as methane (CH4) is recovered by the second component gas recovery pipeline 7. That is, the adsorption process is performed in the carbon dioxide adsorption tower 3a, the mixed gas is introduced into the adsorption tower, the carbon dioxide is adsorbed by the adsorbent, and the second component gas is taken out.
[0277] The carbon dioxide adsorption tower 3a containing the adsorbent adsorbing carbon dioxide is decompressed and exhausted by the decompression device 9, thereby regenerating the adsorbent in the carbon dioxide adsorption tower 3a and taking out the purified carbon dioxide. That is, the carbon dioxide desorption process is performed to take out carbon dioxide by decompressing and exhausting carbon dioxide from the adsorption tower.
[0278] As described above, the carbon dioxide adsorption tower 3a and the carbon dioxide adsorption tower 3b repeatedly perform carbon dioxide adsorption based on the introduction of the mixed gas and carbon dioxide desorption based on the reduced pressure. Therefore, during the period when the carbon dioxide adsorption tower 3a performs the desorption of carbon dioxide, the mixed gas is introduced into the carbon dioxide adsorption tower 3b to adsorb carbon dioxide. After the desorption of carbon dioxide in the carbon dioxide adsorption tower 3a is completed, the mixed gas is introduced into the carbon dioxide adsorption tower 3a again, and the carbon dioxide absorption tower 3b is reduced in pressure to perform the desorption of carbon dioxide. In this way, the adsorption-desorption of carbon dioxide can be repeatedly performed by each tower, and the mixed gas can be continuously processed.
[0279] More specifically, it can work through the following steps. Figure 3 Schematic diagram showing the temporal change of the pressure fluctuations in the carbon dioxide adsorption tower 3a and the carbon dioxide adsorption tower 3b due to the operation of the purified gas production device 100. Figure 3 The moment T 1a , starting from the state where all automatic valves AV1 to AV6 are closed, open the automatic valves AV1 and AV3, check the flowmeter 11 in such a way that the mixed gas supply pipeline 1 reaches a predetermined flow rate, and supply the mixed gas at the adsorption pressure P a (e.g. 105 kPa) is supplied to the carbon dioxide adsorption tower 3a. When the carbon dioxide concentration in the component analyzer 73 exceeds 5 volume % (e.g. Figure 3 The moment T 1b ), the automatic valves AV1 and AV3 can be closed, and the automatic valves AV2 and AV4 can be opened at the same time to switch the supply of the mixed gas from the carbon dioxide adsorption tower 3a to the carbon dioxide adsorption tower 3b. By switching, the mixed gas is adsorbed at an adsorption pressure P a (e.g., 105 kPa) is supplied to the carbon dioxide adsorption tower 3b. In addition, in the carbon dioxide adsorption tower 3a, the pressure in the carbon dioxide adsorption tower 3a is reduced by opening the automatic valve AV5 while the automatic valve AV3 is closed and reducing the pressure by the pressure reducing device 9, so that the pressure in the carbon dioxide adsorption tower 3a is reduced to the final pressure P b (e.g. 2 kPa) to perform desorption operation, thereby recovering carbon dioxide from the carbon dioxide adsorption tower 3a. b The moment is T 1cSince the carbon dioxide adsorbed by the adsorbent in the carbon dioxide adsorption tower 3a is desorbed, the carbon dioxide is recovered and the adsorbent is regenerated.
[0280] Next, when the carbon dioxide concentration of the gas flowing out of the carbon dioxide adsorption tower 3b exceeds 5 volume %, the automatic valves AV2 and AV4 can be closed, and the automatic valves AV1 and AV3 can be opened at the same time to switch the supply of the mixed gas from the carbon dioxide adsorption tower 3b to 3a (this time is referred to as T 1d ). In addition, in the carbon dioxide adsorption tower 3b, the pressure of the carbon dioxide adsorption tower 3b is reduced to 2 kPa by opening the automatic valve AV6 and using the pressure reducing device 9 to perform desorption operation, thereby recovering carbon dioxide from the carbon dioxide adsorption tower 3b. Thereafter, when the carbon dioxide concentration in the component analyzer 73 exceeds 5 volume % (for example, Figure 3 The moment T 1e ), close the automatic valve AV1 and the automatic valve AV3, and open the automatic valve AV2 and the automatic valve AV4 at the same time, and switch the supply of the mixed gas from the carbon dioxide adsorption tower 3a to the carbon dioxide adsorption tower 3b again.
[0281] The time T shown above 1a ~T 1d The series of operations up to this point is one cycle C1 of the pressure change in the carbon dioxide adsorption tower 3a. 1b ~T 1e The series of operations up to this point is the operation of one cycle C1 of pressure fluctuation in the carbon dioxide adsorption tower 3b. That is, cycle C1 includes one adsorption step and one desorption step. By repeating the same operation, the adsorption step and desorption step such as the second cycle C2 and the third cycle C3 of pressure fluctuation can be repeated.
[0282] The purified gas production device 100 can be applied to, for example, purification of industrial off-gas containing carbon dioxide, biogas obtained by fermentation of organic matter, etc. Among these, it is preferably used for purification of biogas.
[0283] Example
[0284] The present embodiment will be described in more detail below with reference to Examples and the like, but these are merely illustrative and the present embodiment is not limited to the following Examples.
[0285] [Apparent density d a Determination of
[0286] The apparent density of the zeolite body is a Use the following steps.
[0287] (1) Add 100 mL of liquid paraffin into a 250 mL measuring cylinder and measure the initial liquid level.
[0288] (2) The mass W (g) of about 80 mL of the zeolite molded body is measured.
[0289] (3) The water content u (unit: mass %) of the zeolite molded body was measured using an infrared moisture meter "FD-660" (trade name) manufactured by KETT Scientific Laboratory.
[0290] (4) Add the weighed zeolite molded body to the liquid paraffin in the measuring cylinder, and calculate the volume V of the added zeolite molded body according to the amount of liquid paraffin liquid level rise after 10 minutes. a (cm 3 ). The mass W (g) and volume V of the zeolite molded body put in a (cm 3 ) Calculate the apparent density d according to the following formula a .
[0291] d a =(W-W×u / 100) / V a (g / cm 3 )
[0292] [Bulk density d b Determination of
[0293] Bulk density of zeolite shaped body d b The determination was carried out using the following steps.
[0294] (1) A 1000 mL measuring cylinder is filled with about 800 mL of a zeolite molded body. During the filling, the zeolite molded body is hammered with a rubber hammer every time about 50 mL of the zeolite molded body is added until the filling height of the molded body does not change.
[0295] (2) Read the filling volume Vb (cm2) of the zeolite molded body from the scale line of the measuring cylinder. 3 ).
[0296] (3) The mass W (g) of the filled zeolite molded body is measured using an electronic balance with a minimum measurement value of 0.01 g.
[0297] (4) The water content u (unit: mass %) of the zeolite molded body was measured using an infrared moisture meter "FD-660" (trade name) manufactured by KETT Scientific Laboratory.
[0298] (5) The mass W and water content u measured in (3) and (4) above and the filling volume V read in (2) above are used to calculate the water content u. b , the bulk density d is obtained according to the following formula b (g / cm 3 ).
[0299] db =(W-W×u / 100) / V b (g / cm 3 )
[0300] [True density d t Determination of
[0301] True density of zeolite shaped body d t The determination was carried out using the following steps.
[0302] (1) Using the high-precision gas adsorption measurement device "BELSORP MAXII" (trade name) manufactured by Microtrac BEL, the volume V1 (cm2) of the blank measurement cell was measured in a water tank controlled at 25°C using high-purity helium gas with a purity of 99.9% or more. 3 ).
[0303] (2) The measuring cell whose volume was measured in (1) above was filled with about 0.2 g of the zeolite molded body and vacuum dried at 250° C. for more than 3 hours using a pretreatment device “BELPREP-VACIII” (trade name) manufactured by Microtrac BEL.
[0304] (3) The dried measuring cell is cooled to room temperature while maintaining the vacuum state, and the volume V2 (cm2) of the measuring cell when the zeolite molded body is filled is measured in the same manner as in (1) above. 3 ) for determination.
[0305] (4) The mass W (g) of the zeolite molded body in the cell after the volume V2 is measured is measured using a precision balance with a minimum measurement value of 0.0001 g.
[0306] (5) Passage pool volume V1 (cm 3 )、V2(cm 3 ) and the filling mass W (g) of the zeolite molded body, the true density d of the zeolite molded body is calculated according to the following formula t (g / cm 3 ).
[0307] True density d t =W / (V1-V2)
[0308] [X-ray diffraction; crystal structure analysis]
[0309] X-ray diffraction was performed by the following steps.
[0310] (1) The zeolite molded body obtained in each example and comparative example (dried product after treatment at 350°C for 24 hours) was used as a sample and crushed using an agate mortar. Furthermore, 10% by mass of crystalline silicon (manufactured by Rare Metallic Co., Ltd.) was added to the zeolite molded body (dried product), and mixed using an agate mortar until it became uniform, and the mixture was used as a sample for structural analysis.
[0311] (2) The sample of (1) above was uniformly fixed on a non-reflective sample plate for powder, and the crystal structure was analyzed by X-ray diffraction under the following conditions.
[0312] X-ray diffraction apparatus (XRD): Powder X-ray diffraction apparatus "RINT2500" (trade name) manufactured by Rigaku Corporation
[0313] X-ray source: Cu tube (40kV, 200mA)
[0314] Measurement temperature: 25℃
[0315] Measuring range: 5~60°(0.02° / step)
[0316] Measuring speed: 0.2° / min
[0317] Slit width (scattering, divergence, light receiving): 1°, 1°, 0.15mm
[0318] [ 29 Si-MAS-NMR spectrum, SAR measurement]
[0319] The SAR of the zeolite in the zeolite molded body can be determined by 29 First, as a humidity control for the zeolite, the bottom of the desiccator was filled with water, and the zeolite placed in the sample tube was kept at the top for 48 hours. After the humidity control, the zeolite was tested under the following conditions. 29 Determination of Si-MAS-NMR.
[0320] Device: JEOL RESONANCE ECA700
[0321] Magnetic field strength: 16.44T( 1 H resonance frequency 700MHz)
[0322] Determination of the core: 29 Si
[0323] Resonance frequency: 139.08MHz
[0324] NMR tube: 4mm Ф (zirconia rotor)
[0325] Measurement method: DD / MAS (dipolar decoupling magic angle spinning)
[0326] Pulse width: 45°
[0327] Waiting time: 50 seconds
[0328] Integration times: 800 times (measurement time: about 22 hours)
[0329] MAS: 10,000Hz
[0330] Chemical shift standard: Silicone rubber (-22.34ppm) external standard
[0331] In the molded body comprising GIS type zeolite, 29 The Si-MAS-NMR spectrum showed the following five peaks.
[0332] (1) Q4 (0Al): Peak of Si that is not bonded to Al via oxygen
[0333] (2) Q4 (1Al): Peak of Si bonded to one Al via oxygen
[0334] (3) Q4 (2Al): Peak of Si bonded to two Al atoms via oxygen
[0335] (4) Q4 (3Al): Peak of Si bonded to three Al atoms via oxygen
[0336] (5) Q4 (4Al): Peak of Si bonded to four Al atoms via oxygen
[0337] In addition, 29 In the Si-MAS-NMR spectrum, these peak positions are usually present in the range of -112ppm to -80ppm, and can be assigned to Q4(0Al), Q4(1Al), Q4(2Al), Q4(3Al), and Q4(4Al) from the high magnetic field side. The peak positions may vary depending on the cationic species present in the zeolite framework, but the peak positions are usually present in the following ranges.
[0338] (1) Q4(0Al): -105ppm to -112ppm
[0339] (2) Q4(1Al): -100ppm to -105ppm
[0340] (3) Q4 (2Al): -95ppm to -100ppm
[0341] (4) Q4 (3Al): -87ppm to -95ppm
[0342] (5) Q4 (4Al): -80 ppm to -87 ppm
[0343] about 29 The peak area intensity of the Si-MAS-NMR spectrum was analyzed by Gaussian and Lorentzian functions using the analysis program dmfit (version #202000113), and the four parameters of amplitude (height of the maximum value of the spectrum), position (spectral position, ppm), width (full width at half maximum of the spectrum, ppm), and Gaussian / Lorentzian ratio (xG / (1-x)L) were optimized and calculated by the least squares algorithm. When the peak areas of Q4(0Al), Q4(1Al), Q4(2Al), Q4(3Al), and Q4(4Al obtained in this way are each taken as A_Q4(0Al), A_Q4(1Al), A_Q4(2Al), A_Q4(3Al), and A_Q4(4Al), and the total value of A_Q4(0Al), A_Q4(1Al), A_Q4(2Al), A_Q4(3Al), and A_Q4(4Al) is taken as A_total, SAR can be obtained as follows.
[0344] SAR=100 / [A_Q4(1Al) / 4+2×A_Q4(2Al) / 4+3×A_Q4(3Al) / 4+4×A_Q4(4Al) / 4]×2
[0345] [Evaluation of embrittlement resistance of zeolite molded bodies in CO2 atmosphere]
[0346] The embrittlement resistance of the zeolite molded bodies obtained in Examples and Comparative Examples in a CO 2 atmosphere was evaluated by the following procedure.
[0347] (1) 100 g of a zeolite molded body is weighed and the short diameter of the zeolite molded body is measured. The average value of the short diameter of the zeolite molded body is taken as ds. A sieve having a mesh size smaller than ds and having a maximum mesh size is selected and prepared according to the mesh size disclosed in JIS Z 8801-1, and the zeolite molded body remaining on the sieve after the sieving is used as a test sample for evaluating embrittlement resistance under a CO2 atmosphere.
[0348] (2) The test sample was dried in a N2 atmosphere at 200°C for 3 hours. After cooling to room temperature in the N2 atmosphere, it was exposed to CO2 at room temperature for 30 minutes.
[0349] (3) After measuring the mass W1 of the test sample after CO2 exposure, the sample is sieved using the above-mentioned mesh size sieve, and the mass W2 of the zeolite molded body that has passed the sieve is measured. The value calculated using formula (1) is defined as the pulverization rate [mass %] of the zeolite molded body. The lower the pulverization rate of the zeolite molded body, the more resistant it is to embrittlement in a CO2 atmosphere.
[0350] [Number 1]
[0351]
[0352] [Alkali metal content]
[0353] The concentration of alkali metals in zeolite is measured by ICP-AES (hereinafter referred to as "ICP-AES", SPS3520UV-DD manufactured by Hitachi High-Tech Science Co., Ltd.: device name) using a liquid obtained by heat-dissolving zeolite with sodium hydroxide aqueous solution or aqua regia and then diluting it appropriately. The content of potassium and lithium in zeolite is calculated as the ratio (Z / T) of the total amount of potassium and lithium in zeolite (Z) to the total amount of each amount of alkali metal (T). K / T is calculated in the same manner.
[0354] [CO2 adsorption and hysteresis; gas adsorption-desorption isotherm determination]
[0355] The gas adsorption-desorption isotherm measurement was performed by the following procedure.
[0356] (1) The dried product obtained in each of the Examples and Comparative Examples was used as a sample, and 0.2 g of the dried product was added to a 12 mm sample cell (manufactured by MicroMeritics).
[0357] (2) The sample put into the sample cell in (1) above was placed in a gas adsorption measuring device "3-Flex" (trade name) manufactured by Micro Meritics, and subjected to a heating vacuum degassing treatment at 250°C and 0.001 mmHg or less for 12 hours.
[0358] (3) The sample added to the sample cell after the treatment in (2) above is placed in a constant temperature circulating water at 25°C. After the temperature of the sample reaches 25±0.2°C, it is measured using liquefied carbon dioxide (manufactured by Sumitomo Seika Co., Ltd., purity 99.9% by mass or more) at an absolute pressure of 0.25 to 760 mmHg. It should be noted that in the above measurement, the pressure is measured over time, and when the pressure change is less than 0.001% / 10sec, it is determined that the saturated adsorption amount has been reached, and this is taken as the CO2 adsorption amount at 25°C (unit: cm 3 / g).
[0359] (4) Following the measurement in (3), the pressure was reduced over time at an absolute pressure of 760 to 0.25 mmHg to measure the desorption isotherm of carbon dioxide. It should be noted that, as a balance judgment, the pressure change was set to 0.001% / 10 sec or less and the measurement was performed in the same manner as in (3).
[0360] (5) As an index indicating the hysteresis amount in the carbon dioxide adsorption-desorption isotherm, when the equilibrium adsorption amount at 75 mmHg of the adsorption isotherm measured in (3) and the equilibrium adsorption amount at 75 mmHg of the desorption isotherm measured in (4) are respectively set to q(Ad) and q(De), q(Ad) / q(De) is used as an index indicating the hysteresis amount. When q(Ad) / q(De)=1.00, it indicates no hysteresis, and the smaller q(Ad) / q(De), the larger the hysteresis.
[0361] [CH4 adsorption; gas adsorption isotherm determination]
[0362] The gas adsorption isotherm measurement was performed by the following procedure.
[0363] (1) The dried product obtained in each of the Examples and Comparative Examples was used as a sample, and 0.2 g of the dried product was added to a 12 mm sample cell (manufactured by MicroMeritics).
[0364] (2) The sample put into the sample cell in (1) above was placed in a gas adsorption measuring device "3-Flex" (trade name) manufactured by Micro Meritics, and subjected to a heating vacuum degassing treatment at 250°C and 0.001 mmHg or less for 12 hours.
[0365] (3) The sample added to the sample cell after the treatment in (2) above is placed in a constant temperature circulating water at 35°C. After the temperature of the sample reaches 25±0.2°C, methane gas (manufactured by Fujii Shoji Co., Ltd., purity 99.99% by mass or more) is used for measurement at an absolute pressure of 0.25 to 760 mmHg. It should be noted that in the above measurement, the pressure is measured over time, and when the pressure change is less than 0.001% / 10sec, it is determined that the saturated adsorption amount has been reached, and this is taken as the CH4 adsorption amount at 25°C (unit: cm 3 / g).
[0366] [N2 adsorption; gas adsorption isotherm determination]
[0367] The gas adsorption isotherm measurement was performed by the following procedure.
[0368] (1) The dried product obtained in each of the Examples and Comparative Examples was used as a sample, and 0.2 g of the dried product was added to a 12 mm sample cell (manufactured by MicroMeritics).
[0369] (2) The sample put into the sample cell in (1) above was placed in a gas adsorption measuring device "3-Flex" (trade name) manufactured by Micro Meritics, and subjected to a heating vacuum degassing treatment at 250°C and 0.001 mmHg or less for 12 hours.
[0370] (3) The sample added to the sample cell after the treatment in (2) above is placed in a constant temperature circulating water at 35°C. After the temperature of the sample reaches 25±0.2°C, nitrogen (manufactured by Taiyo Nippon Sanso Co., Ltd., purity 99.99% by mass or more) is used for measurement at an absolute pressure of 0.25 to 760 mmHg. It should be noted that in the above measurement, the pressure is measured over time, and when the pressure change is less than 0.001% / 10sec, it is determined that the saturated adsorption amount has been reached, and this is taken as the N2 adsorption amount at 25°C (unit: cm 3 / g).
[0371] [Gas separation performance evaluation; CO2 recovery purity and CH4 recovery rate]
[0372] use Figure 4 The gas separation performance evaluation apparatus 1000 shown measures the CO 2 recovery purity and CH 4 recovery rate of the zeolite molded body produced in the examples or comparative examples by the following procedures.
[0373] (1) The zeolite molded body produced in the Examples or Comparative Examples was heated to 2500 cm 3 The container 1008 is filled and placed in a constant temperature chamber 1007 .
[0374] (2) The thermostatic bath of (1) is maintained at 250°C for 12 hours or longer to allow water or gas molecules adsorbed on the zeolite molded body to be released, and then the thermostatic bath is cooled and maintained at 35°C.
[0375] (3) The raw material gas to be separated is filled into the raw material gas tank 1005. The composition of the raw material gas is 40 volume % of CO2 and 60 volume % of CH4.
[0376] (4) The flow rate of the raw material gas was adjusted to 15 NL / min by using the mass flow controller 1006, so that the raw material gas was circulated in a manner in contact with the zeolite molded body filled in the container 1008. The ratio of the amount of CH4 gas measured by the mass flow meter 1009 to the amount of CH4 gas flowing in the container 1008 until the CO2 concentration measured by the CO2 concentration meter 1010 reached 40 volume % was taken as the CH4 recovery rate (unit: volume %).
[0377] (5) When the CO2 concentration measured by the CO2 concentration meter 1010 reaches 40% by mass, the introduction of the raw gas into the container 1008 is stopped, and the decompression device 1011 is used to reduce the pressure of the container 1008 to 2 kPa to perform a desorption operation, thereby recovering the gas from the container 1008.
[0378] (6) The volume of the recovered gas (unit: L) is measured using an integrating flow meter.
[0379] (7) The amounts of CO 2 and CH 4 contained in the recovered gas of (5) above were measured using a gas chromatograph "GC-2014" (trade name) manufactured by Shimadzu Corporation under the following conditions.
[0380] Carrier gas: He (purity above 99.9%)
[0381] Column: "CarboBOND" (trade name) manufactured by Agilent Technologies Inc.
[0382] Column temperature: 40°C
[0383] Detector: TCD
[0384] The amounts of CO2 and CH4 were calculated from the calibration curve based on the peak areas.
[0385] (8) The volume of CO2 contained in the recovered gas is calculated based on the volume of the recovered gas measured in (6) above and the mass ratio of CO2 to CH4 measured in (7) above. The ratio of the volume of CO2 contained in the recovered gas to the volume of the recovered gas is taken as the CO2 recovery purity (unit: volume %).
[0386] [Pressure loss]
[0387] The pressure loss of the zeolite molded body was evaluated by the following procedure.
[0388] (1) A vinyl chloride tube with an inner diameter of 52 mm and a height of 1.5 m and a metal mesh with a mesh size of 1.5 mm fixed to the bottom was filled with the zeolite molded body to a height of 1 m. During the filling, the vinyl chloride tube was hammered with a rubber hammer every 10 cm until the filling height did not change.
[0389] (2) Gas circulation lines are connected to the upper and lower ends of the vinyl chloride tube in (1) above, respectively.
[0390] (3) A digital differential pressure gauge is connected at a position where the pressure difference between the upper end and the lower end of the vinyl chloride tube in (2) above can be measured.
[0391] (4) Compressed air was introduced from the gas flow line connected to the upper end in (2) above so that the superficial velocity was 1 m / s, and the display value of the digital differential pressure gauge at this time was taken as the pressure loss (unit: kPa).
[0392] [Measurement of length and diameter of zeolite molded body]
[0393] The length and diameter of the cylindrical zeolite pellets were measured by the vernier caliper method. In this measurement, three samples were measured using a vernier caliper with a minimum reading of 0.1 mm or less, and the average values were used as the length and diameter.
[0394] For the spherical zeolite molded body, the molded body is placed stably on a horizontal surface, and a projection image is taken in the vertical direction of the molded body in parallel with a precision ruler with a minimum reading value of 0.5 mm or less. The projection image of the molded body is sandwiched between two parallel straight lines connected to the projection image, and the interval when the interval between the parallel lines is the largest is taken as the major diameter, and the interval when the interval is the smallest is taken as the minor diameter. The actual major diameter and minor diameter of the molded body are calculated based on the length of the scale lines of the ruler in the image. Three samples are measured, and the average value of the calculated six diameters is taken as the diameter of the spherical molded body.
[0395] [Weight reduction measurement]
[0396] The weight loss (unit: g) per 1.2 g of the zeolite molded bodies obtained in Examples and Comparative Examples under the conditions of 300° C. and 2 hours was measured in the following procedure.
[0397] (1) 1.2 g of a zeolite molded body was weighed and dried in a N2 atmosphere at 180°C for 3 hours.
[0398] (2) The dried zeolite molded body is weighed in a glove box.
[0399] (3) The measured zeolite molded body is heated in an air atmosphere at 300° C. for 2 hours.
[0400] (4) The mixture is sealed in a manner that does not absorb moisture, and after cooling to room temperature, the zeolite molded body is measured in a glove box.
[0401] The difference between the weight of the zeolite molded body measured in step (2) and the weight of the zeolite molded body measured in step (4) is defined as the weight loss. The closer the value is to 0, the smaller the weight loss is, and the zeolite molded body is evaluated to have durability.
[0402] [Determination of powdering rate after high temperature exposure]
[0403] The pulverization rate of the zeolite molded body after the weight loss measurement was measured by the same procedure as in the above-mentioned "Durability evaluation of zeolite molded body in CO2 atmosphere". The pulverization rate measured in this way is defined as the pulverization rate after high temperature exposure [mass %], and the closer this value is to 0, the more excellent the durability of the zeolite molded body.
[0404] The apparent density d of the zeolite molded body containing the zeolite capable of adsorbing carbon dioxide is shown below. a Specific aspects of the zeolite molded body of the present embodiment where θ is 0.75 or more. These are merely examples, and the present embodiment is not limited to the following examples.
[0405] [Production Example 1]
[0406] 61.93 g of water, 0.403 g of sodium hydroxide (NaOH, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 3.39 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 1.64 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), and 10.82 g of colloidal silica (Ludox AS-40, solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) were mixed and stirred for 30 minutes to prepare a mixed gel. The composition of the mixed gel was α = E / Al2O3 = 4.53, β = SiO2 / Al2O3 = 8.17, γ = Na2O / Al2O3 = 3.99, δ = P2O5 / Al2O3 = 0.00, ε = H2O / Al2O3 = 431.0, ζ = H2O / OH - =376.7, η=R / Al2O3=0.00. The mixed gel was put into a 200mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 4 days at a stirring speed of 30rpm and 135°C in a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down direction of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. The X-ray diffraction spectrum confirmed that the obtained zeolite was a GIS type zeolite. In addition, no peaks derived from other zeolites or amorphous silica-alumina were observed, so it was evaluated as a high-purity GIS type zeolite.
[0407] The obtained zeolite is used 29 The silicon oxide-alumina ratio was calculated from the Si-MAS-NMR spectrum, and the results showed that SAR = 6.90 and (a+d) / (b+c) = 0.305. In addition, the potassium and lithium contents in the zeolite were Z / T = 0.00 (= K / T). When the adsorption isotherm and desorption isotherm of CO2 of the obtained GIS type zeolite were measured, the adsorption amount at 760 mmHg was 82.2 cm 3 / g, q(Ad) / q(De)=0.984. In addition, when the adsorption isotherm of CH4 was measured in the same way, the adsorption amount at 760 mmHg was 6.2 cm 3 / g.
[0408] [Production Example 2]
[0409] 61.65 g of water, 0.60 g of sodium hydroxide aqueous solution (NaOH, concentration 48% by mass, manufactured by Tokuyama Soda Co., Ltd.), 2.27 g of sodium carbonate (Na2CO3, manufactured by Tokuyama Soda Co., Ltd.), 1.64 g of sodium aluminate (NaAlO2, manufactured by Hokuriku Chemical Industry Co., Ltd.), and 10.82 g of colloidal silica ("Ludox AS-40" (trade name), solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) were mixed and stirred for 30 minutes to prepare a mixed gel. The composition of the mixed gel was α = E / Al2O3 = 4.86, β = SiO2 / Al2O3 = 8.17, γ = Na2O / Al2O3 = 3.99, δ = P2O5 / Al2O3 = 0.00, ε = H2O / Al2O3 = 431.2, ζ = H2O / OH - =527.8, η=R / Al2O3=0.00. The mixed gel was put into a 200mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 5 days at a stirring speed of 30rpm and 130°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down direction of the micro-storage bottle. The product was filtered out, and after drying at 120°C, a powdered zeolite was obtained. 1 g of the obtained zeolite was added to 500mL of a 0.05N potassium carbonate aqueous solution prepared using potassium carbonate (K2CO3, manufactured by Nippon Soda Co., Ltd.), and stirred at 500rpm for 3 hours at room temperature. The product was filtered out, and dried at 120°C to obtain a powdered zeolite in which part of the cations were exchanged for potassium. The XRD spectrum confirmed that the obtained zeolite was a GIS type zeolite. Furthermore, since no peaks derived from other zeolites or amorphous silica-alumina were observed, the zeolite was evaluated to be a high-purity GIS-type zeolite.
[0410] The obtained zeolite is used 29 The Si-MAS-NMR spectrum calculated the silicon oxide-alumina ratio, and the result was SAR of 6.90 and (a+d) / (b+c)=0.220. The potassium and lithium content in the zeolite Z / T=0.98 (=K / T). When the adsorption and desorption isotherms of CO2 were measured, the adsorption amount at 760 mmHg was 84.0 cm 3 / g, q(Ad) / q(De)=1.000. In addition, when the adsorption isotherm of CH4 was measured in the same manner, the adsorption amount at 760 mmHg was 0.0 cm 3 / g.
[0411] [Production Example 3]
[0412] 141.41 g of water, 2.62 g of sodium hydroxide (NaOH, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 8.53 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 3.85 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), and 17.41 g of amorphous silicon oxide (Perkasil SM500, manufactured by Grace Co., Ltd.) were mixed and stirred for 1 hour to prepare a mixed gel. The composition of the mixed gel was α=E / Al2O3=4.85, β=SiO2 / Al2O3=14.00, γ=Na2O / Al2O3=5.16, δ=P2O5 / Al2O3=0.00, ε=H2O / Al2O3=379.3, ζ=H2O / OH - =120.0, η=R / Al2O3=0.00. The mixed gel was put into a 300mL stainless steel micro-storage bottle (manufactured by HIROCOMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 4 days at a stirring speed of 30rpm and 130°C in a stirring thermostatic bath (manufactured by HIROCOMPANY) that can rotate along the up and down direction of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. The XRD spectrum confirmed that the obtained zeolite was a GIS type zeolite. In addition, no peaks derived from other zeolites or amorphous silica-alumina were observed, so it was evaluated as a high-purity GIS type zeolite.
[0413] The obtained zeolite is used 29 The Si-MAS-NMR spectrum calculated the silicon oxide-alumina ratio, and the result was SAR of 10.1, (a+d) / (b+c) = 0.519. In addition, the potassium and lithium contents in the zeolite were Z / T = 0.00 (= K / T). When the adsorption and desorption isotherms of CO2 were measured, the adsorption amount at 760 mmHg was 80.0 cm 3 / g, q(Ad) / q(De)=1.000. In addition, when the adsorption isotherm of CH4 was measured in the same way, the adsorption amount at 760 mmHg was 7.2 cm 3 / g.
[0414] [Production Example 4]
[0415] 141.41 g of water, 2.62 g of sodium hydroxide (NaOH, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 2.43 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 0.55 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), and 35.33 g of aluminum silicate (SIPERNAT820A, manufactured by Evonik) were mixed and stirred for 1 hour to prepare a mixed gel. The composition of the mixed gel was α=E / Al2O3=0.88, β=SiO2 / Al2O3=14.00, γ=Na2O / Al2O3=2.62, δ=P2O5 / Al2O3=0.00, ε=H2O / Al2O3=242.4, ζ=H2O / OH - =120.0, η=R / Al2O3=0.00. The mixed gel was put into a 300mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 5 days at a stirring speed of 30rpm and 130°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down direction of the micro-storage bottle. The product was filtered out, and after drying at 120°C, a powdered zeolite was obtained. 1 g of the obtained zeolite was added to 500mL of a 0.005N potassium carbonate aqueous solution prepared using potassium carbonate (K2CO3, manufactured by Nippon Soda Co., Ltd.), and stirred at 500rpm for 3 hours at room temperature. The product was filtered out, and dried at 120°C to obtain a powdered zeolite in which part of the cations were exchanged for potassium. The XRD spectrum confirmed that the obtained zeolite was a GIS type zeolite. Furthermore, since no peaks derived from other zeolites or amorphous silica-alumina were observed, the zeolite was evaluated to be a high-purity GIS-type zeolite.
[0416] The obtained zeolite is used 29 The Si-MAS-NMR spectrum calculated the silicon oxide-alumina ratio, and the result was SAR of 8.20, (a+d) / (b+c) = 0.356. In addition, the potassium and lithium content in the zeolite was Z / T = 0.16 (= K / T). When the adsorption and desorption isotherms of CO2 were measured, the adsorption amount at 760 mmHg was 72.7 cm 3 / g, q(Ad) / q(De)=0.991. In addition, when the adsorption isotherm of CH4 was measured in the same way, the adsorption amount at 760 mmHg was 0.5 cm 3 / g.
[0417] [Production Example 5]
[0418] 21.05 g of water, 0.53 g of sodium hydroxide (NaOH, manufactured by Junsei Chemical Co., Ltd.), 1.37 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 1.13 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.) and water glass No. 3 (Kishid a Chemical Co., Ltd.) and 15.5 g of 1,2-dihydrogen 2-acid ... - =90.2, η=R / Al2O3=0.00. The mixed gel was put into a 100mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 5 days at a stirring speed of 30rpm and 130°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down direction of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. 1g of the obtained zeolite was added to 500mL of a 0.006N lithium carbonate aqueous solution prepared using lithium nitrate (LiNO3, manufactured by Fuji Film Co., Ltd.) and stirred at 500rpm for 3 hours at room temperature. The product was filtered out and dried at 120°C to obtain a powdered zeolite in which part of the cations were exchanged for lithium. The obtained zeolite was confirmed to be a GIS type zeolite by XRD spectroscopy. In addition, no peaks derived from other zeolites or amorphous silica-alumina were observed, so it was evaluated as a high-purity GIS type zeolite.
[0419] The obtained zeolite is used 29 The Si-MAS-NMR spectrum calculated the silicon oxide-alumina ratio, and the result was SAR of 3.40, (a+d) / (b+c) = 0.192. In addition, the potassium and lithium content in the zeolite Z / T = 0.11. When the adsorption and desorption isotherms of CO2 were measured, the adsorption amount at 760 mmHg was 51.2 cm 3 / g, q(Ad) / q(De)=0.978. In addition, when the adsorption isotherm of CH4 was measured in the same way, the adsorption amount at 760 mmHg was 0.8 cm 3 / g.
[0420] [Example 1]
[0421] 40 parts by mass of the GIS type zeolite powder obtained in Production Example 1, 43 parts by mass of powdered alumina hydrate (manufactured by Nikko Catalysts & Chemicals Co., Ltd., alumina content: 70% by mass), and 17 parts by mass of ion-exchanged water were mixed.
[0422] The mixture was extruded into a cylindrical shape having a diameter of 3 mm using a wet extrusion granulator "MG-55" (manufactured by Dalton Corporation), and then calcined in an air atmosphere at 350° C. for 24 hours using an electric furnace.
[0423] The zeolite molded body obtained in this manner was subjected to various evaluations and the results are shown in Table 1.
[0424] Apparent density d a 1.4g / cm 3 , bulk density d b 0.882g / cm 3 , true density d t 2.48g / cm 3 , apparent density d a / True density d t is 0.56, bulk density d b / True density d t The weight reduction was 0.02 g.
[0425] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 0% by mass. In addition, the powdering rate after high-temperature exposure was 0% by mass.
[0426] The adsorption isotherms of CO2, CH4 and N2 of the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 46.9 cm 3 / g, CH4: 3.5cm 3 / g, N2: 4.0cm 3 / g, CO2 / CH4 adsorption selectivity is 13.4, CO2 / N2 adsorption selectivity is 11.7. The recovery purity of CO2 measured by the gas separation performance evaluation device is 98.5% by volume, the recovery rate of CH4 is 99.0% by volume, and the pressure loss at the filling height of 1m is 10.8kPa.
[0427] [Example 2]
[0428] Using the zeolite synthesized in Production Example 2, a zeolite molded body was obtained in the same manner as in Example 1.
[0429] The apparent density d of the zeolite molded body thus obtained a 1.4g / cm 3 , bulk density d b 0.882g / cm3 , true density d t 2.48g / cm 3 , apparent density d a / True density d t is 0.56, bulk density d b / True density d t The weight reduction was 0.02 g.
[0430] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. In addition, the powdering rate after high temperature exposure was 1% by mass.
[0431] The adsorption isotherms of CO2, CH4 and N2 of the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 48.0 cm 3 / g, CH4: 0.9cm 3 / g, N2: 1.3cm 3 / g, the adsorption selectivity of CO2 / CH4 is 53.3, and the adsorption selectivity of CO2 / N2 is 36.9.
[0432] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.5 vol%, and the recovery rate of CH 4 was 99.0 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.6 kPa.
[0433] [Example 3]
[0434] Using the zeolite synthesized in Production Example 3, a zeolite molded body was obtained in the same manner as in Example 1.
[0435] The apparent density d of the zeolite molded body thus obtained a 1.4g / cm 3 , bulk density d b 0.882g / cm 3 , true density d t 2.48g / cm 3 , apparent density d a / True density d t is 0.56, bulk density d b / True density d t The weight reduction was 0.02 g.
[0436] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. In addition, the powdering rate after high temperature exposure was 1% by mass.
[0437] The adsorption isotherms of CO2, CH4 and N2 of the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 46.2 cm 3 / g, CH4: 4.1cm 3 / g, N2: 4.5cm 3 / g, the adsorption selectivity of CO2 / CH4 is 11.3, and the adsorption selectivity of CO2 / N2 is 10.3.
[0438] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.5% by volume, and the recovery rate of CH 4 was 99.0% by volume. When the pressure loss at a filling height of 1 m was measured, it was 10.9 kPa.
[0439] [Example 4]
[0440] 40 parts by mass of the GIS-type zeolite powder obtained in Preparation Example 1, 10.4 parts by mass of powdered alumina hydrate (manufactured by Nikko Catalysts & Chemicals, Ltd., alumina content: 70% by mass), 1.2 parts by mass of methyl cellulose (Serander YB-132A manufactured by Highchem Co., Ltd.), 0.2 parts by mass of polyvinyl alcohol (Gohsenol N-300 manufactured by Mitsubishi Chemical Corporation), and 48.2 parts by mass of alumina sol (manufactured by Nissan Chemical Co., Ltd., alumina content: 10.5% by mass) are mixed, and the mixture is molded using a wet extrusion granulator. A zeolite molded body is obtained in the same manner as in Example 1 except that the mixture is molded using a wet extrusion granulator.
[0441] The apparent density d of the zeolite molded body thus obtained a 1.3g / cm 3 , bulk density d b 0.819 g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.56, bulk density d b / True density d t The weight loss was 0.02 g.
[0442] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. In addition, the powdering rate after high temperature exposure was 1% by mass.
[0443] The adsorption isotherms of CO2 and CH4 of the zeolite molded body of Example 4 were measured. The adsorption amounts at 760 mmHg were CO2: 62.6 cm 3 / g, CH4: 4.9cm 3 / g, the adsorption selectivity of CO2 / CH4 is 12.8.
[0444] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.3 vol%, and the recovery rate of CH 4 was 98.8 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.8 kPa.
[0445] [Example 5]
[0446] Using the zeolite synthesized in Production Example 4, a zeolite molded body was obtained in the same manner as in Example 1.
[0447] The apparent density d of the zeolite molded body thus obtained a 1.3g / cm 3 , bulk density d b 0.819 g / cm 3 , true density d t 2.48g / cm 3 , apparent density d a / True density d t is 0.52, bulk density d b / True density d t The weight loss was 0.02 g.
[0448] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. In addition, the powdering rate after high temperature exposure was 1% by mass.
[0449] The adsorption isotherms of CO2, CH4 and N2 of the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 41.6 cm 3 / g, CH4: 1.2cm 3 / g, N2: 1.5cm 3 / g, the adsorption selectivity of CO2 / CH4 is 34.7, and the adsorption selectivity of CO2 / N2 is 27.7.
[0450] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.3 vol%, and the recovery rate of CH 4 was 98.8 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.6 kPa.
[0451] [Example 6]
[0452] Using the zeolite synthesized in Production Example 5, a zeolite molded body was obtained in the same manner as in Example 1.
[0453] The apparent density d of the zeolite molded body thus obtained a 1.3g / cm 3, bulk density d b 0.819 g / cm 3 , true density d t 2.48g / cm 3 , apparent density d a / True density d t is 0.52, bulk density d a / True density d t The weight loss was 0.02 g.
[0454] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. In addition, the powdering rate after high temperature exposure was 1% by mass.
[0455] The adsorption isotherms of CO2, CH4 and N2 of the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 29.3 cm 3 / g, CH4: 1.4cm 3 / g, N2: 1.8cm 3 / g, the adsorption selectivity of CO2 / CH4 is 20.9, and the adsorption selectivity of CO2 / N2 is 16.2.
[0456] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.3% by volume, and the recovery rate of CH 4 was 98.8% by volume. When the pressure loss at a filling height of 1 m was measured, it was 10.9 kPa.
[0457] [Example 7]
[0458] A zeolite molded body was obtained in the same manner as in Example 4 except that 49.4 parts by mass of alumina sol (manufactured by Taki Chemical Co., Ltd.) having an alumina content of 7.2% by mass was used instead of the alumina sol having an alumina content of 10.5% by mass and the amount of powdered alumina hydrate was 9.2 parts by mass.
[0459] The apparent density d of the zeolite molded body thus obtained a 0.92g / cm 3 , bulk density d b 0.580g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.40, bulk density d b / True density d t The weight reduction was 0.02 g.
[0460] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 5% by mass. In addition, the powdering rate after high temperature exposure was 3% by mass.
[0461] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 65.8 cm 3 / g, CH4: 5.0cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.2.
[0462] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 96.9 volume %, and the recovery rate of CH 4 was 97.9 volume %. When the pressure loss at a filling height of 1 m was measured, it was 10.5 kPa.
[0463] [Example 8]
[0464] A zeolite molded body was obtained in the same manner as in Example 4 except that polyvinyl alcohol was not used.
[0465] The apparent density d of the zeolite molded body thus obtained a 0.91g / cm 3 , bulk density d b 0.573g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.39, bulk density d b / True density d t The weight reduction was 0.03 g.
[0466] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 8% by mass. In addition, the powdering rate after high temperature exposure was 7% by mass.
[0467] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.5 cm 3 / g, CH4: 4.8cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.0.
[0468] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 96.9 vol%, and the recovery rate of CH 4 was 97.9 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.8 kPa.
[0469] [Example 9]
[0470] A molded body was obtained in the same manner as in Example 4 except that methylcellulose was not used.
[0471] The apparent density d of the zeolite molded body thus obtained a 1.0g / cm 3 , bulk density d b 0.630g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.43, bulk density d a / True density d t The weight reduction was 0.1 g.
[0472] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 6% by mass. In addition, the powdering rate after high temperature exposure was 6% by mass.
[0473] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.5 cm 3 / g, CH4: 4.7cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.3.
[0474] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 97.3 vol%, and the recovery rate of CH 4 was 98.1 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.9 kPa.
[0475] [Example 10]
[0476] A zeolite molded body was obtained in the same manner as in Example 4 except that the wet extrusion granulator "MG-55" was not used but the extrusion molding was performed manually with a clay gun.
[0477] The apparent density d of the zeolite molded body thus obtained a 0.77g / cm 3 , bulk density d b 0.485g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.33, bulk density d a / True density d t The weight reduction was 0.04 g.
[0478] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 10% by mass. The powdering rate after high temperature exposure was 8% by mass.
[0479] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.6 cm 3 / g, CH4: 4.8cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.0.
[0480] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 96.1 vol%, and the recovery rate of CH 4 was 97.3 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.7 kPa.
[0481] [Example 11]
[0482] A molded body was obtained in the same manner as in Example 4 except that alumina sol (alumina content: 10 mass %) manufactured by Kawaken Fine Chemicals Co., Ltd. was used instead of alumina sol manufactured by Nissan Chemical Co., Ltd.
[0483] The apparent density d of the zeolite molded body thus obtained a 0.77g / cm 3 , bulk density d b 0.485g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.33, bulk density d b / True density d t The weight loss was 0.03 g.
[0484] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 10% by mass. The powdering rate after high temperature exposure was 8% by mass.
[0485] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.4 cm 3 / g, CH4: 4.8cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.0.
[0486] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 96.1 vol%, and the recovery rate of CH 4 was 97.3 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.8 kPa.
[0487] [Example 12]
[0488] Instead of using the wet extrusion granulator "MG-55", a tablet molding compressor "BRE-32" (manufactured by Maekawa Testing Equipment Manufacturing Co., Ltd.) was used to perform a pressurization treatment at 12 MPa for 20 seconds to produce a disc-shaped molded body with a diameter of 32 mm and a thickness of 5 mm. The molded body was obtained in the same manner as in Example 4, except that the above-mentioned method was used.
[0489] The apparent density d of the zeolite molded body thus obtained a 1.4g / cm 3 , bulk density d b 1.092g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.61, bulk density d a / True density d t The weight reduction was 0.01 g.
[0490] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 0% by mass. The powdering rate after high temperature exposure was 0% by mass.
[0491] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.4 cm 3 / g, CH4: 4.9cm 3 / g, the adsorption selectivity of CO2 / CH4 is 12.7.
[0492] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 99.1 vol%, and the recovery rate of CH 4 was 99.4 vol%. When the pressure loss at a filling height of 1 m was measured, it was 11.0 kPa.
[0493] [Example 13]
[0494] A molded body was obtained in the same manner as in Example 7 except that the diameter was 8 mm instead of 3 mm and then granulated using a spherical granulator (manufactured by Dalton Corporation) at 200 rpm for 10 minutes to obtain a spherical molded body of Φ8 mm.
[0495] The apparent density d of the zeolite molded body thus obtaineda 1.2g / cm 3 , bulk density d b 0.744 g / cm 3 , true density is 2.31g / cm 3 , apparent density / true density is 0.52, bulk density d b / True density d t The weight reduction was 0.03 g.
[0496] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 2% by mass. The powdering rate after high temperature exposure was 2% by mass.
[0497] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.6 cm 3 / g, CH4: 4.9cm 3 / g, the adsorption selectivity of CO2 / CH4 is 12.8.
[0498] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 97.9 vol%, and the recovery rate of CH 4 was 98.6 vol%. When the pressure loss at a filling height of 1 m was measured, it was 3.06 kPa.
[0499] [Example 14]
[0500] 40 parts by mass of the GIS type zeolite powder obtained in Production Example 1, 10 parts by mass of bentonite (manufactured by Kunimine Industries, Ltd.), 0.4 parts by mass of carboxymethylcellulose (manufactured by Nippon Paper Industries, Ltd.), and 40.6 parts by mass of ion-exchanged water were mixed.
[0501] The mixture was extruded into a cylindrical shape having a diameter of 3 mm using a wet extrusion granulator MG-55 (manufactured by Dalton Corporation), and then calcined in an air atmosphere at 600° C. for 10 hours using an electric furnace.
[0502] The apparent density d of the zeolite molded body thus obtained a 0.97g / cm 3 , bulk density d b 0.631 g / cm 3 , true density d t 2.40g / cm 3 , apparent density d a / True density d t is 0.40, bulk density d a / True density d t The weight reduction was 0.03 g.
[0503] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 0% by mass. In addition, the powdering rate after high-temperature exposure was 0% by mass.
[0504] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 65.6 cm 3 / g, CH4: 5.02cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.1.
[0505] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 98.1 vol%, and the recovery rate of CH 4 was 97.3 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.9 kPa.
[0506] [Example 15]
[0507] A molded body was obtained in the same manner as in Example 14 except that the diameter was 8 mm instead of 3 mm and then granulated using a spherical granulator (manufactured by Dalton Corporation) at 200 rpm for 10 minutes to produce a spherical molded body of Φ8 mm.
[0508] The apparent density d of the zeolite molded body thus obtained a 1.1 g / cm 3 , bulk density d b 0.693g / cm 3 , true density d t 2.40g / cm 3 , apparent density d a / True density d t is 0.46, bulk density d a / True density d t The weight reduction was 0.03 g.
[0509] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 0% by mass. In addition, the powdering rate after high-temperature exposure was 0% by mass.
[0510] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 65.9 cm 3 / g, CH4: 5.00cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.2.
[0511] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 97.6 vol%, and the recovery rate of CH 4 was 98.4 vol%. When the pressure loss at a filling height of 1 m was measured, it was 3.10 kPa.
[0512] [Comparative Example 1]
[0513] 49.5 parts by mass of the GIS zeolite powder obtained in Manufacturing Example 1 was dispersed in 50.5 parts by mass of ion exchange water to prepare a raw material slurry. The obtained raw material slurry was stirred at 25°C for 1 hour. The raw material slurry was supplied to a spray dryer (OC-16 type spray dryer manufactured by Okawara Chemical Industry Co., Ltd.) in which the fluid temperature at the inlet of the spray dryer was set to 230°C and the fluid temperature at the outlet of the spray dryer was set to 120°C, and spray-dried using a rotating disc method to obtain a spray-dried powder. A molded body was obtained in the same manner as in Example 4, except that the spray-dried powder was used instead of the GIS zeolite in Manufacturing Example 1.
[0514] The apparent density d of the zeolite molded body thus obtained a 0.70g / cm 3 , bulk density d b 0.441 g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.30, bulk density d b / True density d t The weight reduction was 0.09 g.
[0515] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 90% by mass. The powdering rate after high temperature exposure was 95% by mass.
[0516] The adsorption isotherms of CO2 and CH4 of the zeolite molded body of Comparative Example 1 were measured. The adsorption amounts at 760 mmHg were CO2: 62.5 cm 3 / g, CH4: 4.8cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.0.
[0517] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 95.6% by volume, and the recovery rate of CH 4 was 96.9% by volume. When the pressure loss at a filling height of 1 m was measured, it was 11.0 kPa.
[0518] [Comparative Example 2]
[0519] A molded body was obtained in the same manner as in Comparative Example 1 except that methylcellulose and polyvinyl alcohol were not used.
[0520] The apparent density d of the zeolite molded body thus obtained a 0.74g / cm 3 , bulk density d b 0.466g / cm 3 , true density d t 2.31 g / cm 3 , apparent density d a / True density d t is 0.32, bulk density d a / True density d t The weight reduction was 0.03 g.
[0521] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 100% by mass. The powdering rate after high temperature exposure was 100% by mass.
[0522] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 62.6 cm 3 / g, CH4: 4.9cm 3 / g, the adsorption selectivity of CO2 / CH4 is 12.8.
[0523] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 95.9 vol%, and the recovery rate of CH 4 was 97.1 vol%. When the pressure loss at a filling height of 1 m was measured, it was 10.9 kPa.
[0524] [Comparative Example 3]
[0525] 70 parts by mass of the GIS type zeolite powder obtained in Preparation Example 1 and 30 parts by mass of a polyamide resin (Zytel 101L manufactured by DuPont) were melt-kneaded at 285°C and 400 rpm using a twin-screw extruder (TEM48-SS manufactured by Toshiba Machine Co., Ltd.) to obtain a composite. The obtained composite was injected into an injection molding machine (EC75NII manufactured by Toshiba Machine Co., Ltd.) set at a barrel temperature of 285°C and a mold temperature of 70°C to obtain a zeolite molded body having a length of 80 mm, a width of 10 mm, and a thickness of 4 mm.
[0526] The apparent density d of the zeolite molded body thus obtained a 0.74g / cm 3 , bulk density d b 0.385g / cm 3 , true density dt 2.31 g / cm 3 , apparent density d a / True density d t is 0.32, bulk density d b / True density d t The weight reduction was 0.65 g.
[0527] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 12% by mass. The powdering rate after high-temperature exposure was 100% by mass.
[0528] The adsorption isotherms of CO2 and CH4 of the zeolite molded body of Comparative Example 3 were measured. The adsorption amounts at 760 mmHg were CO2: 57.5 cm 3 / g, CH4: 4.5cm 3 / g, the adsorption selectivity of CO2 / CH4 is 12.8.
[0529] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 94.8 vol%, and the recovery rate of CH 4 was 96.3 vol%. When the pressure loss at a filling height of 1 m was measured, it was 6.29 kPa.
[0530] [Comparative Example 4]
[0531] 10 parts by mass of γ-alumina powder (manufactured by Kanto Chemical Co., Ltd.) was mixed with 90 parts by mass of the GIS type zeolite powder obtained in Production Example 1, and the mixture was molded into a 3 mm diameter and 2 mm height tablet using a tablet molding machine (manufactured by Labonect Co., Ltd.). The tablet molding was heated at 335° C. for 4 hours to obtain a zeolite molded body.
[0532] The apparent density d of the zeolite molded body thus obtained a 0.70g / cm 3 , bulk density d b 0.455g / cm 3 , true density d t 2.42g / cm 3 , apparent density d a / True density d t is 0.29, bulk density d a / True density d t The weight reduction was 0.03 g.
[0533] The embrittlement resistance of the zeolite molded body in a CO2 atmosphere was evaluated and the powdering rate was measured, which was 100% by mass. The powdering rate after high temperature exposure was 100% by mass.
[0534] The adsorption isotherms of CO2 and CH4 on the zeolite were measured. The adsorption amounts at 760 mmHg were CO2: 74.0 cm 3 / g, CH4: 5.6cm 3 / g, the adsorption selectivity of CO2 / CH4 is 13.2.
[0535] The recovery purity of CO 2 measured by the gas separation performance evaluation device was 95.7 vol%, and the recovery rate of CH 4 was 97.0 vol%. When the pressure loss at a filling height of 1 m was measured, it was 18.5 kPa.
[0536] The above results are summarized in Table 1.
[0537] [Table 1-1]
[0538] Table 1(1 / 4)
[0539]
[0540] [Table 1-2] Table 1 (2 / 4)
[0541]
[0542] [Table 1-3] Table 1 (3 / 4)
[0543]
[0544] [Table 1-4]
[0545] Table 1 (4 / 4)
[0546]
[0547] Industrial Applicability
[0548] The zeolite molded body of the present invention has industrial applicability as a separator and separation membrane for various gases and liquids, an electrolyte membrane for fuel cells, etc., a filler for various resin molded bodies, a membrane reactor, or a catalyst for hydrogen cracking, alkylation, etc., a catalyst carrier for supporting metals, metal oxides, etc., an adsorbent, a desiccant, a detergent builder, an ion exchanger, a wastewater treatment agent, a fertilizer, a food additive, a cosmetic additive, etc.
[0549] Explanation of symbols
[0550] 2 Adsorption device
[0551] 21 Containers
[0552] 23 Filters
[0553] 24 Zeolite Molded Body
[0554] 100 Refined gas production equipment
[0555] 1Mixed gas supply pipeline
[0556] 11 Flow meter
[0557] 12 Moisture meter
[0558] 13. Component Analyzer
[0559] 3a,3b Carbon dioxide adsorption tower
[0560] 31a,31b fixed bed
[0561] 5 Carbon dioxide recovery pipeline
[0562] 53a,53b pressure gauge
[0563] 51 Flow Meter
[0564] 52 Moisture Meter
[0565] 54 Component Analyzer
[0566] 7. Second component gas recovery pipeline
[0567] 71 Flow Meter
[0568] 72 Moisture Meter
[0569] 73 Component Analyzer
[0570] 9. Pressure Relief Device
[0571] AV1,AV2,AV3,AV4 automatic valve
[0572] 1000 Gas Separation Performance Evaluation Device
[0573] 1005 Raw gas tank
[0574] 1006 Mass Flow Controller
[0575] 1007 Constant Temperature Bath
[0576] 1008 Containers
[0577] 1009 Mass Flow Meter
[0578] 1010CO2 concentration meter
[0579] 1011 Pressure Relief Device
Claims
1. A zeolite molded body comprising a zeolite capable of adsorbing carbon dioxide, wherein: The apparent density d of the zeolite shaped body a It is above 0.
75.
2. The zeolite molded body according to claim 1, wherein The zeolite has a 10 cm 3 / g or more carbon dioxide adsorption capacity.
3. The zeolite molded body according to claim 1, wherein The apparent density d in the zeolite shaped body a / True density d t The ratio is above 0.
36.
4. The zeolite molded body according to claim 1, wherein The bulk density d of the zeolite shaped body b / True density d t The ratio is greater than 0.
25.
5. The zeolite shaped body according to claim 1, wherein The zeolite has an adsorption selectivity of carbon dioxide adsorption / second component gas adsorption of 10 or more.
6. The zeolite shaped body according to claim 1, wherein The zeolite is GIS type zeolite.
7. The zeolite shaped body according to claim 6, wherein The silica-alumina ratio of the GIS type zeolite is 3.40 or more.
8. The zeolite shaped body according to claim 6, comprising potassium or lithium as a cationic species in the GIS type zeolite.
9. The zeolite molded body according to claim 8, wherein The ratio (Z / T) of the total amount of substance (Z) of potassium and lithium to the total amount of substance (T) of alkali metals in the GIS-type zeolite is 0.05 or more.
10. The zeolite shaped body according to claim 6, comprising GIS type zeolite, wherein 29 When the peak area intensities attributed to Q4(3Al), Q4(2Al), Q4(1Al) and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c and d respectively, the GIS-type zeolite satisfies (a+d) / (b+c)≧0.
192. The zeolite shaped body according to claim 1 , comprising a carrier.
12. The zeolite molded body according to claim 11, wherein The carrier includes an inorganic binder and an organic binder.
13. The zeolite shaped body according to claim 11, wherein The total content of the carrier is 1% by mass to 99% by mass relative to 100% by mass of the total amount of the zeolite molded body.
14. The zeolite shaped body according to claim 1, wherein Under the conditions of 300° C. and 2 hours, the weight loss per 1.2 g was 1.0 or less.
15. The zeolite shaped body according to claim 1, wherein The aspect ratio is 1 to 10.
16. The zeolite molded body according to claim 1, which has a cylindrical shape. 17 . The zeolite molded body according to claim 16 , which has a length of 3 mm to 30 mm, and a diameter of 1 mm to 30 mm. The zeolite shaped body according to claim 1 , which has a spherical shape.
19. The zeolite molded body according to claim 18, which has a diameter of 3 mm to 10 mm. 20 . An adsorption device comprising the zeolite molded body according to claim 1 .
21. A method for producing a purified gas, comprising: The separation step uses the adsorption device described in claim 20 to separate one or more gases selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, Ar, CO and hydrocarbons.
22. The method for producing a purified gas according to claim 21, wherein: In the separation step, the gas is separated by a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method.
23. A method for producing a purified gas, wherein an adsorption tower is used to separate carbon dioxide and a second component gas different from carbon dioxide from a mixed gas, wherein: The manufacturing method comprises: an adsorption step of introducing the mixed gas into the adsorption tower, allowing the carbon dioxide to be adsorbed on the adsorbent, and taking out the second component gas; and The desorption process is to decompress and exhaust the carbon dioxide from the adsorption tower, thereby removing the carbon dioxide from the adsorbent. The adsorption tower is filled with an adsorbent comprising the zeolite molded body according to any one of claims 1 to 22.
24. The method for producing a purified gas according to claim 23, wherein: The adsorption step and the desorption step are repeated a plurality of times or more.
25. A method for producing a zeolite shaped body, comprising: a raw material mixing step (X) of mixing a zeolite capable of adsorbing carbon dioxide with a carrier comprising an inorganic binder and an organic binder; A molding step (Y) of subjecting the prepared raw material to a molding process to obtain a precursor; as well as The calcining step (Z) is to calcine the precursor to obtain a zeolite molded body.
Citation Information
Patent Citations
Spherical agglomerates based on zeolite(s), process for their production and their use in adsorption processes or in catalysis
CN101772377A
GIS zeolite
CN108495813A
Upgrading process of light olefine in turbulent fcc reactor
CN88100267A
GIS-type zeolite
WO2022025247A1