Stretchable resin composition, and resin sheet material, metal foil with resin, metal foil-clad laminate, and wiring board using same
By controlling the molecular weight and structure of epoxy resin and crystalline curing agent, and combining specific polymerization units, a stretchable resin composition with high tear strength and heat resistance is formed, which solves the problem of flexibility and tear strength in the existing technology. Taking into account the problem, it applies to a variety of technical fields.
Patent Information
- Application Number
- CN202280093096.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-18
AI Technical Summary
Existing stretchable resin substrates have difficulty balancing flexibility and tear strength, and suffer from metal corrosion and high cross-linking density, resulting in poor performance in applications such as circuit substrates.
A combination of epoxy resin and crystalline curing agent is used to control the weight average molecular weight of the epoxy resin between 50,000 and 3 million, and the polydispersity between 1.1 and 3.0, and introduce epoxy groups, Polymeric units of cyano and isobornyl groups, combined with conductive powder, form a resin composition with high tear strength and heat resistance.
It achieves a combination of flexibility, heat resistance and high tear strength, and is suitable for IoT, flexible display devices, optics and electronic fields, etc., improving the flexibility and reliability of industrial applications.
Smart Images

Figure BDA0005024733390000061 
Figure BDA0005024733390000141 
Figure BDA0005024733390000151
Abstract
Description
Technical Field
[0001] The present invention relates to a stretchable resin composition, and a resin sheet material, a resin-coated metal foil, a metal foil-clad laminate, and a wiring board using the same. Background Art
[0002] Thermosetting resins have excellent heat resistance, chemical resistance, formability, insulation reliability, etc., and are therefore used in a wide range of fields such as electronic materials and optical materials. In particular, in recent years, research has been conducted to give thermosetting resins flexibility and use them in flexible devices that can be configured on curved surfaces or concave and convex surfaces, or can be freely deformed, depending on the application. The materials used in this application (stretchable resin substrates, resin films, etc.) are required to have wearability and shape tracking properties, and shape recovery during stretching and before and after stretching is important.
[0003] As a substrate that meets this requirement, for example, a resin composition has been proposed, which contains a polyrotaxane (A), an epoxy resin (B) and a curing agent (C), wherein the curing agent (C) contains 0.1 parts by mass or more and less than 10 parts by mass of an acid anhydride (C-1) relative to 100 parts by mass of the total of the polyrotaxane (A), the epoxy resin (B) and the curing agent (C) (Patent Document 1).
[0004] In addition, for example, a thermosetting composition for forming a stretchable resin is disclosed, which contains (A) an epoxy resin and (B) a thiol compound having two or more thiol groups, wherein (A) the epoxy resin contains a copolymerized epoxy resin, and the copolymerized epoxy resin is a copolymer containing a structural unit having (A1) an aromatic group or an alicyclic group and a structural unit having an oxyalkylene group or an alkylene group having more than 4 carbon atoms (Patent Document 2). In addition, an epoxy resin composition is proposed, which contains an epoxy resin and a curing agent having an alicyclic structure, wherein the epoxy resin is obtained by reacting a bifunctional aliphatic epoxy compound (X) and a dihydric phenol compound (Y) in the presence of a catalyst, and the bifunctional aliphatic epoxy compound (X) is obtained by distilling and refining a reaction product of a diol having 2 to 12 carbon atoms and an epihalohydrin, and in the bifunctional aliphatic epoxy compound (X), the purity of the diglycidyl compound is 90% by mass or more and the total chlorine content is 0.3% by mass or less (Patent Document 3).
[0005] However, the substrate obtained by the method described in the above-mentioned patent document 1 is indeed excellent in flexibility, but has low tear strength and is difficult to be applied to circuit substrates. In addition, it is believed that: the retractable resin substrate described in the above-mentioned patent document 2 has retractability, but has the problem of metal corrosion. In addition, the cross-linking density is high and the tear strength is poor. Although the epoxy resin described in the above-mentioned patent document 3 is excellent in flexibility, the molecular weight is small, so it is difficult to form a sheet form. Even if it can be formed, the curing time is long and the production efficiency is poor. In addition, the cross-linking density is high and the tear strength is poor.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Publication No. 6851035
[0009] Patent Document 2: Japanese Patent Publication No. 2020-23601
[0010] Patent Document 3: Japanese Patent Publication No. 2019-189798 Summary of the invention
[0011] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a stretchable resin composition having flexibility, heat resistance and high tear strength.
[0012] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned problems can be solved by a stretchable resin composition having the following structure. Based on this finding, the present inventors have further conducted studies and have completed the present invention.
[0013] That is, one aspect of the present invention relates to a stretchable resin composition comprising at least an epoxy resin and a curing agent, wherein the weight average molecular weight of the epoxy resin is 50,000 to 3,000,000, and the polydispersity of the average molecular weight of the epoxy resin, i.e., Mw / Mn, satisfies the following formula (1):
[0014] 1.1≤Mw / Mn≤3.0 (1)
[0015] Wherein, Mn is the number average molecular weight, Mw is the weight average molecular weight,
[0016] The curing agent is a crystalline compound, and the glass transition temperature of a cured product of the stretchable resin composition is 60° C. or lower. DETAILED DESCRIPTION
[0017] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these descriptions.
[0018] In the present embodiment, "elasticity" means that it can be elastically deformed and has stretchability, and more specifically, it means that the elongation before breaking is 10% or more. The cured product of the elastic resin composition of the present embodiment preferably has an elasticity of 10% or more and 500% or less, and more preferably has an elasticity of 30% or more and 300% or less. When the elasticity shows an elongation of 10% or more, it has the advantages of high followability when deformed into any shape and being difficult to be destroyed. The upper limit of the elasticity is not particularly limited, but when the elasticity is 500%, there is no problem in practical use.
[0019] The “cured product” in the present embodiment refers to a state in which the curing reaction is completed through a process in which sufficient energy such as heat or light is applied to the resin composition to cure it.
[0020] The stretchable resin composition according to the present embodiment is a stretchable resin composition containing at least an epoxy resin and a curing agent, wherein the weight average molecular weight of the epoxy resin is greater than or equal to 50,000 and less than or equal to 3,000,000, and the polydispersity of the average molecular weight of the epoxy resin, i.e., Mw / Mn, satisfies the following formula (1).
[0021] 1.1≤Mw / Mn≤3.0 (1)
[0022] Wherein, Mn is the number average molecular weight and Mw is the weight average molecular weight.
[0023] Furthermore, the curing agent is a crystalline compound, and the glass transition temperature of a cured product of the stretchable resin composition is 60° C. or lower.
[0024] With the above-mentioned configuration, a stretchable resin composition having flexibility, heat resistance, and high tear strength can be provided.
[0025] The stretchable resin composition according to the present embodiment has advantages of excellent heat resistance and adhesiveness due to the epoxy resin and the curing agent.
[0026] By setting the weight average molecular weight of the epoxy resin of this embodiment to be 50,000 or more and 3,000,000 or less, a resin composition having excellent elasticity can be obtained. Furthermore, by setting the polydispersity (Mw / Mn) of the average molecular weight to be 1.1≤Mw / Mn≤3.0, a resin composition having high tear strength can be obtained.
[0027] The curing agent involved in this embodiment is a crystalline compound. In addition, it is believed that by making the stretchable resin composition include a hard segment and a soft segment, a density difference of the molecular chain is generated in the resin composition, and the stress is dispersed, so that tear propagation is difficult to occur. As a result, a resin composition having stretchability and high tear strength can be obtained.
[0028] In addition, by setting the glass transition temperature (Tg) of the cured product of the stretchable resin composition according to the present embodiment to 60° C. or less, sufficient flexibility and stretchability can be ensured. The glass transition temperature is more preferably 40° C. or less. There is no need to set a lower limit, but from the viewpoint of the stickiness of the film surface at room temperature when the resin film is formed, the glass transition temperature is preferably 20° C. or more.
[0029] In addition, since the resin composition of the present invention has the above-mentioned characteristics, it can be applied not only to IoT and flexible display devices, but also to various technical fields such as the optical field, the electronic field, the bonding field, and the medical field, and is therefore very advantageous in industrial utilization.
[0030] Hereinafter, the stretchable resin composition according to the present embodiment will be described in detail.
[0031] (Epoxy resin)
[0032] The stretchable resin composition according to the present embodiment has advantages of excellent heat resistance and adhesiveness due to the epoxy resin contained therein.
[0033] As described above, the epoxy resin used in this embodiment can be used without particular limitation as long as it has a weight average molecular weight of 50,000 to 3,000,000 and has a polydispersity of average molecular weight, that is, Mw / Mn, that satisfies the following formula (1).
[0034] 1.1≤Mw / Mn≤3.0 (1)
[0035] Wherein, Mn is the number average molecular weight and Mw is the weight average molecular weight.
[0036] The more preferred lower limit of the weight average molecular weight is more than 100,000, more preferably more than 200,000. On the other hand, the more preferred upper limit is less than 2,000,000, more preferably less than 1,000,000. If the weight average molecular weight is less than 50,000, the elasticity and tear strength are poor, so it is not preferred. If the weight average molecular weight exceeds 3,000,000, the reactivity is poor, and curing requires a long time of processing, so it is not preferred. In addition, because the viscosity of the resin composition is too high and filmization is difficult, it is not preferred. It is believed that: if the weight average molecular weight is within this range, a composition with excellent elasticity and tear strength can be obtained.
[0037] The upper limit of the polydispersity of the average molecular weight (Mw / Mn) is more preferably 2.5, and further preferably 2.2. If the polydispersity of the average molecular weight exceeds 3.0, the tear strength deteriorates, which is not preferred.
[0038] The epoxy resin in the present embodiment can be used without particular limitation as long as the weight average molecular weight and the polydispersity of the average molecular weight are within the above ranges.
[0039] Specific examples of the epoxy resin that can be used in the present embodiment include epoxy resins containing polymerized units (A) of (meth)acrylate having an epoxy group, polymerized units (B) of (meth)acrylate having a cyano group, and polymerized units (C) of (meth)acrylate having an isobornyl group.
[0040] The epoxy resin of this embodiment preferably does not have unsaturated bonds such as double bonds and triple bonds between carbon atoms. That is, the carbon atoms of the epoxy resin are preferably bonded by saturated bonds (single bonds). It is believed that by not having unsaturated bonds between carbon atoms, it will not be oxidized over time and can better maintain elasticity.
[0041] The epoxy resin of this embodiment is preferably not an epoxy resin obtained by polymerizing only the polymerized unit (A), only the polymerized unit (B), or only the polymerized unit (C), but a resin obtained by randomly polymerizing the polymerized unit (A), the polymerized unit (B), and the polymerized unit (C). The form of polymerization is not particularly limited, and may be a block copolymer, an alternating copolymer, a random copolymer, a graft copolymer, etc.
[0042] Polymerized units of (meth)acrylate having an epoxy group (A)
[0043] The polymerized units (A) provide crosslinking points to the epoxy resin of the present embodiment, allowing it to be cured. In addition, it is believed that the presence of the polymerized units (A) improves the heat resistance of the cured product after heat curing due to the presence of epoxy groups.
[0044] The content of the polymerized unit (A) in the epoxy resin is not particularly limited, but preferably the epoxy equivalent of the polymerized unit (A) is greater than 500 g / eq and less than 15000 g / eq relative to the total amount of the epoxy resin. It is believed that by making the epoxy equivalent within this range, a resin composition having heat resistance and a moderate elastic modulus can be more reliably obtained. If the epoxy equivalent is less than 500 g / eq, the elastic modulus after curing becomes too high and may break during stretching. In addition, if the epoxy equivalent exceeds 15000 g / eq, the elastic modulus after curing at high temperature is reduced, for example, the film is deformed in the reflow process, which may lead to poor installation. The more preferred range of the epoxy equivalent is greater than 1000 g / eq and less than 5000 g / eq.
[0045] Specific examples of the (meth)acrylate monomer constituting the polymerized unit (A) having an epoxy group include glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, β-ethyl glycidyl (meth)acrylate, glycidyl vinyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, o-isopropenylbenzyl glycidyl ether, m-isopropenylbenzyl glycidyl ether, p-isopropenylbenzyl glycidyl ether, etc. These may be used alone or in combination of two or more.
[0046] ·Polymerized units of (meth)acrylate having a cyano group (B)
[0047] By containing a (meth)acrylate having a cyano group, hydrogen bonding occurs between the surface of the metal foil, and when the resin composition or resin film of the present embodiment is used in a metal foil-clad laminate, it has the advantage of excellent adhesion. In addition, it is believed that by having a polymerized unit (B), sufficient tear strength can be obtained and heat resistance is further improved.
[0048] The specific examples of the (meth)acrylate monomer constituting the polymerized unit (B) having a cyano group are not particularly limited, and specific examples thereof include acrylonitrile and methacrylonitrile.
[0049] The epoxy resin used in the present embodiment preferably contains more than 1 part by mass and less than 30 parts by mass of the polymerized unit (B) component relative to 100 parts by mass of the epoxy resin. It is believed that if the content is within this range, the above-mentioned effect can be obtained more reliably. If the content of the polymerized unit (B) component is lower than this range, the adhesion with the copper foil may deteriorate. In addition, if the content exceeds the above range, the elastic modulus becomes high and the elasticity may deteriorate, so it is not preferred. Relative to 100 parts by mass of the epoxy resin, the more preferred content of the polymerized unit (B) component is more than 10 parts by mass and less than 20 parts by mass.
[0050] Polymerized units of (meth)acrylate having an isobornyl group (C)
[0051] It is considered that by including the polymerized unit (C) component having an isobornyl group, it is possible to suppress the increase in shrinkage upon curing, and further, it is possible to suppress deformation such as warping when the resin composition or the resin film is cured.
[0052] Specific examples of the acrylic acid ester or (meth)acrylic acid ester monomer constituting the polymerized unit (C) having an isobornyl group are not particularly limited, and examples thereof include isobornyl (meth)acrylate.
[0053] The epoxy resin of the present embodiment preferably contains more than 1 part by mass and less than 50 parts by mass of the polymerized unit (C) component relative to 100 parts by mass of the epoxy resin. It is believed that if the content is within this range, the above-mentioned effect can be obtained more reliably. If the content of the polymerized unit (C) component is lower than this range, the dimensional stability is likely to deteriorate. In addition, if the content exceeds the above range, the reactivity of the polymerized unit (A) of the (meth) acrylate having an epoxy group is reduced, and the heat resistance of the resin composition after heat curing deteriorates, so it is not preferred. In addition, it is not preferred from the viewpoint that the viscosity of the resin composition becomes too large. The more preferred content of the polymerized unit (C) component is more than 10 parts by mass and less than 30 parts by mass relative to 100 parts by mass of the epoxy resin.
[0054] ・Polymer units other than those listed above
[0055] The epoxy resin of the present embodiment may contain other polymerized units in addition to the above-mentioned polymerized units (A), (B), and (C).
[0056] Specific examples of the other polymerized units include an acrylic monomer represented by the following formula (1) (hereinafter also referred to as a polymerized unit (D)).
[0057]
[0058] In the formula (1), R1 is hydrogen or a methyl group, and R2 is hydrogen or an alkyl group. In addition, X represents an integer.
[0059] In order to impart flexibility to the resin composition of the present embodiment, the acrylic monomer represented by the above formula (1) is preferably an acrylic monomer having a low glass transition temperature (Tg).
[0060] Specific examples of the acrylic monomer represented by the formula (1) include ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate.
[0061] As the epoxy resin of the present embodiment, a commercially available product can be used, for example, Teisan Resin PMS-14-67 (manufactured by Nagase ChemteX Corporation) or the like.
[0062] The blending ratio of the epoxy resin in the resin composition of the present embodiment is not particularly limited as long as it is within a range that can obtain the effects of the present invention such as flexibility and adhesion, and is preferably about 50 to 99% by mass based on the entire resin composition.
[0063] The resin composition of the present embodiment may contain resins other than the epoxy resins described above, and may further contain polyurethane resins, acrylic resins, fluororesins, silicone resins, or epoxy resins other than the above resins, etc., depending on the purpose.
[0064] (Curing agent)
[0065] The resin composition of the present embodiment further contains a curing agent. The curing agent that can be used in the present embodiment is not particularly limited as long as it is a crystalline compound and acts as a curing agent for the epoxy resin. Based on the cohesive force of the crystalline compound, a resin composition with high tear strength can be obtained.
[0066] In the present embodiment, the crystalline compound can include a compound having a relatively low molecular weight (polymerization average molecular weight of 300 or less), and exhibiting crystallinity. In this specification, "exhibiting crystallinity" refers to a state in which molecules are oriented based on the regularity of the resin composition or the π-π interaction. In particular, in the present embodiment, since the curing agent is dissolved in an organic solvent and mixed with other constituent materials, it is preferred that the curing agent has an attraction based on interaction, and the preferred resin has a π bond.
[0067] As preferred examples of specific crystalline compounds, molecules having a planar structure in the main chain such as phenyl, biphenyl, diphenol or naphthalene, and compounds having low molecular weight and showing crystallinity can be cited. The crystalline compound of this embodiment is generally solid at room temperature. The crystalline compound can be used alone or in combination of two or more depending on the situation.
[0068] The crystalline compound used as the curing agent of this embodiment can be a commercially available product, for example, PP-BIOC-F, BIOC-E, BIP-BZ, BIP-PHBZ, 3PC, B126X-PC, BIR-PC, TEP-DF, TEP-TPA, TEP-BOCP, BIP-ANT and PAPS-PN2 (all of which are manufactured by Asahi Organic Materials Co., Ltd.) can be used.
[0069] In the resin composition of the present embodiment, the addition amount of the curing agent can be appropriately set according to the epoxy equivalent. Specifically, for example, preferably relative to the total solid content of the resin composition of the present embodiment, the crystalline compound is preferably 1.0 mass % or more and 20 mass % or less. More preferably, 5 mass % or more and 10 mass % or less.
[0070] (Curing accelerator)
[0071] The resin composition of the present embodiment may further contain a curing accelerator. The curing accelerator is not particularly limited, and for example, metal soaps such as imidazoles and derivatives thereof, organophosphorus compounds, zinc octoate, secondary amines, tertiary amines, and quaternary ammonium salts may be used. These may be used alone or in combination of two or more, depending on the circumstances.
[0072] (Conductive powder)
[0073] The stretchable resin composition of this embodiment can be used as a stretchable resin composition having conductivity by further containing conductive powder. Thus, a stretchable resin composition can be provided that can form a conductive resin sheet or film for a stretchable substrate having good shape recovery during stretching and small resistance change before and after stretching.
[0074] The metal powder in the present embodiment is not particularly limited as long as it is a powder with conductivity, and elements such as silver, gold, platinum, palladium, copper, nickel, aluminum, magnesium, tungsten, cobalt, zinc, brass, molybdenum, tantalum, niobium, iron, tin, chromium, lead, titanium, manganese, stainless steel and nickel-chromium alloy can be used, as well as oxides, nitrides, carbides, alloys, etc. containing these elements. In addition, materials in which a part or all of the surface of these metal powders or polymer material powders is covered with the above-mentioned elements with conductivity or oxides, nitrides, carbides, alloys, etc. containing these elements can also be used. Among them, from the viewpoint of conductivity and cost, it is preferred to use silver or copper, etc. These can be used alone, or two or more can be used in combination.
[0075] The shape of the metal powder in the present embodiment is not particularly limited, but from the viewpoint of conductivity, a flat shape is preferred. For example, the aspect ratio of thickness to in-plane length direction is preferably 10 or more. If the aspect ratio is 10 or more, the surface area of the metal powder becomes larger, and conductivity is easily ensured. If the aspect ratio is 1000 or less, from the viewpoint of ensuring better conductivity and printability, it is preferably 10 or more and 1000 or less, and more preferably 20 or more and 500 or less. As an example of a conductive filler having this aspect ratio, a tap density of 6.0 g / cmm as measured by a tapping method can be cited. 3 In addition, if the tap density is 2.0 g / cm 3 Below, the aspect ratio is larger and thus more preferred.
[0076] The particle size of the metal powder in the embodiment is not particularly limited. For example, from the perspective of printability during screen printing, the average particle size measured by a laser light scattering method (particle size when the volume accumulation is 50%; D50) is preferably greater than 0.1 μm and less than 30.0 μm, and more preferably greater than 1.0 μm and less than 10 μm.
[0077] The surface of the metal powder in the embodiment may also be subjected to coupling treatment. Alternatively, the resin composition of the present embodiment contains a coupling agent. Thus, there is an advantage that the adhesion between the binder resin and the conductive filler is further improved. As a coupling agent added to the resin composition or used for coupling treatment of the conductive filler, as long as it is a coupling agent that can be adsorbed on the filler surface or react with the filler surface, it can be used without particular restrictions. Specifically, silane coupling agents, titanate coupling agents, aluminum coupling agents, etc. can be cited. In the case of using a coupling agent in the present embodiment, the amount added is preferably about 1% to 20% by mass relative to the overall stretch resin composition.
[0078] When the stretchable resin composition of the present embodiment contains conductive powder, the proportion of the metal powder is not particularly limited as long as it is within the range that can obtain conductivity, and for example, it is preferably 60 to 90% by mass relative to 100% by mass of the total amount of the epoxy resin and the curing agent. It is believed that if the content of the metal powder is within the above range, the resistance value will not become too large, and the stretchability of the composition after curing will be more excellent. A more preferred content is 75.0 to 85.0% by mass.
[0079] In addition to the metal powder, in order to further improve the conductivity, a conductive or semiconductive conductive auxiliary agent may be added to the stretchable resin composition of the embodiment. As the conductive or semiconductive auxiliary agent, conductive polymers, ionic liquids, carbon black, acetylene black, inorganic compounds used in carbon nanotubes or antistatic agents may be used, and one or more of these may be used at the same time. In addition, instead of using metal powder, conductive polymers, ionic liquids, carbon black, acetylene black, inorganic compounds used in carbon nanotubes or antistatic agents may be used to impart conductivity.
[0080] (Other ingredients)
[0081] In addition, within the scope of not impairing the effects of the present invention, the resin composition involved in this embodiment may also contain other additives as needed, such as surfactants, flame retardants, flame retardant aids, leveling agents, colorants, fragrances, plasticizers, pH adjusters, viscosity adjusters, ultraviolet absorbers, infrared absorbers, antioxidants, preservatives, lubricants, conductive aids and inorganic particles.
[0082] In the case of adding metal powder to the stretchable resin composition of the present embodiment, in order to improve the dispersion stability of the metal powder and the resin, it is preferred to further add a dispersant. As long as it has the effect of a dispersant, any dispersant can be used without particular limitation, for example, copolymers containing acid groups, block copolymers with affinity for pigments, phosphate compounds, polyether phosphate compounds, fatty acid ester compounds, alkylene oxide copolymers, modified polyether polymers, fatty acid derivatives and carbamate polymers can be cited. As commercially available dispersants, the DISPERBYK series manufactured by BYK Chemicals; the SOLSPERSE series manufactured by Lubrizol Japan; the Sokalan, Tamol, Efka series manufactured by BASF; the Nuosperse series manufactured by Hemmings; the DISPARLON series manufactured by Kusumoto Chemicals; the FLOWLEN series manufactured by Kyoeisha Chemicals; and the AJISPER series manufactured by Ajinomoto Fine-Techno, etc. These can be used alone or in combination according to the situation. The content used is preferably 0.01 to 10% by mass based on the metal powder contained in the stretchable resin composition.
[0083] (Cured product of stretchable resin composition)
[0084] Storage modulus at 250°C
[0085] In a preferred embodiment, the storage modulus of the cured product of the resin composition of the present embodiment is 0.1 MPa or more. It is believed that by making the storage modulus within the range, the cured product of the resin composition can have heat resistance. In the present embodiment, "storage modulus" refers to the storage modulus at 250°C, which is a value measured by the method described in the embodiments described later. From the viewpoint of exerting better heat resistance, the storage modulus is preferably 0.5 MPa or more, more preferably 1.0 MPa or more. If it is less than 0.1 MPa, the crosslinking density is too low, and the recovery after elongation may be poor, so it is not preferred. The upper limit is not particularly limited, and there is no problem if it is about 10.0 MPa or less. As described above, the cured product of the resin composition of the present embodiment has excellent heat resistance and has the advantage that a reflow process can be used in the mounting process of electronic components. The storage modulus at 250°C can be obtained by the method shown in the embodiments described later.
[0086] Tensile modulus
[0087] In a preferred embodiment, the tensile modulus of the cured product of the resin composition of the present embodiment is more than 0.1MPa and less than 0.5GPa. It is believed that: thus, a cured product with sufficient flexibility can be obtained. If less than 0.1MPa, there is a tendency to become too soft and difficult to operate. If it exceeds 0.5GPa, flexibility may deteriorate. The more preferred range of tensile modulus is more than 1MPa and less than 0.1GPa. The tensile modulus can be obtained by the method shown in the embodiments described later.
[0088] (Preparation of resin composition and resin film)
[0089] The preparation method of the resin composition involved in the present embodiment is not particularly limited, for example, the epoxy resin, curing agent and solvent are uniformly mixed. The solvent used is not particularly limited, and for example, toluene, xylene, methyl ethyl ketone and acetone can be used. These solvents can be used alone or in combination of two or more. In addition, at this, organic solvents and various additives for adjusting viscosity can also be mixed as needed.
[0090] In addition, when the stretchable resin composition contains conductive (metal) powder, the metal powder is preferably added to the mixture obtained by the above method. For example, the metal powder, the curing agent, dispersant, etc. added as needed, and the solvent can be uniformly mixed and stirred in the above-mentioned resin composition to obtain a resin composition with conductivity. The mixing and stirring method is not particularly limited, and a high shear dispersion device such as a rotation-revolution stirrer and a three-roll grinder is preferably used. In addition, vacuum defoaming can also be performed.
[0091] Then, the resin film of the present embodiment can be obtained by heating and drying the resin composition obtained as described above to evaporate the solvent. That is, the present embodiment also includes a resin film formed using the resin composition as described above.
[0092] The method, apparatus and conditions for heating and drying the resin composition may be the same as in the past or improved. The specific heating temperature and time may be appropriately set according to the curing agent and solvent used, for example, the resin composition may be heated and dried at 130 to 200° C. for about 60 to 180 minutes to form a resin film.
[0093] It should be noted that the resin film of the present embodiment can be formed only by the above-mentioned resin composition or its semi-cured product, but it is also possible to adopt a structure of a film with resin having a resin layer and a support (support film) comprising the resin composition or its semi-cured product. That is, the present embodiment also includes a resin sheet material having the resin film and a support overlapping with the resin film. As the support, electrical insulating films such as polyimide film, PET (polyethylene terephthalate) film, polyester film, polyparaben film, polyetheretherketone film, polyphenylene sulfide film, aramid film, polycarbonate film and polyarylate film can be listed.
[0094] The resin sheet material of this embodiment may be a resin sheet material comprising: the resin composition before curing (uncured) (the resin composition in stage A); and a support, or a resin sheet material comprising: a semi-cured product of the resin composition (the resin composition in stage B); and a support.
[0095] As a method for manufacturing the resin sheet material, for example, after coating the resin varnish-like resin composition as described above on the surface of a film supporting substrate, the solvent is evaporated from the varnish to reduce or remove the solvent, thereby obtaining a resin sheet material before curing (stage A) or in a semi-cured state (stage B).
[0096] It should be noted that, in the resin sheet material of the present embodiment, the resin composition or its semi-cured product as described above may be a product obtained by drying or heating the resin composition.
[0097] In the present embodiment, "semi-cured material" refers to the material of the state that the resin combination is cured to the extent that it can be further cured midway. That is, the semi-cured material is the material of the state (B-stage) that makes the resin combination semi-cured. For example, if the resin combination is heated, the initial viscosity is slowly reduced, and then begins to solidify, and the viscosity slowly rises. In this case, "semi-cured" refers to the state during the period from when the viscosity begins to rise to before fully solidified.
[0098] The resin sheet material of the present embodiment also includes a cured resin sheet material obtained by curing the resin-attached film in the pre-curing state (A stage) or semi-cured state (B stage) as described above.
[0099] (Application of resin film and resin sheet material)
[0100] The resin film and resin sheet material of this embodiment can be used as materials and substrates for various electronic components in various applications. In particular, since they are excellent in flexibility and strength and have both adhesion, resin fluidity and dimensional stability, they are very suitable for use as materials in, for example, foldable electronic paper, organic EL displays, solar cells, RFID, pressure sensors, wearable devices, skin patch-type devices, etc.
[0101] (Metal foil with resin, metal foil-clad laminate, and wiring board)
[0102] Next, a resin-coated metal foil, a metal foil-clad laminate, a wiring board, and the like using the resin composition and / or the resin film according to the present embodiment will be described.
[0103] The metal foil with resin of the present embodiment has: a resin layer including the above-mentioned resin film; and a metal foil overlapping the resin layer. That is, it has a structure in which the metal foil is laminated on at least one side of the resin layer. The metal foil may also be present on both sides of the resin layer. The metal foil with resin of the present embodiment may be a metal foil with resin including: a resin layer including the resin composition before curing (the resin composition in the A stage); and a metal foil, or may be a metal foil with resin including: a resin layer including a semi-cured product of the resin composition (the resin composition in the B stage); and a metal foil.
[0104] As a method for manufacturing the metal foil with resin, for example, the following method can be cited: a method in which the resin composition in the form of a resin varnish as described above is applied to the surface of a metal foil such as a copper foil and then dried. As the coating method, a bar coater, a comma coater, a die coater, a roll coater, a gravure coater, etc. can be cited.
[0105] As the metal foil, any metal foil used for metal foil-clad laminates, wiring boards, etc. can be used without limitation, and examples thereof include copper foil and aluminum foil.
[0106] The thickness and the like of the metal foil and the film supporting substrate can be appropriately set depending on the intended purpose.
[0107] There are no particular limitations on the drying or heat-drying conditions in the method for manufacturing a metal foil with a resin. After a resin composition in the form of a resin varnish is applied to the above-mentioned metal foil, it is heat-dried under the same conditions as the above-mentioned resin film to evaporate the solvent from the varnish and reduce or remove the solvent, thereby obtaining a metal foil with a resin and a film with a resin before curing (stage A) or in a semi-cured state (stage B).
[0108] The metal foil with resin and the above-mentioned resin sheet material (film with resin) can be provided with covering film etc. as required. By providing covering film, the mixing of foreign matter etc. can be prevented. As covering film, there is no particular limitation as long as it can be peeled off without damaging the form of resin composition, and for example, polyolefin film, polyester film, TPX film, film formed by arranging release agent layer on these films, and paper obtained by laminating these films on paper substrate etc. can be used.
[0109] The metal foil-clad laminate of the present embodiment includes: an insulating layer comprising a cured product of the resin composition; and a metal foil overlapping the insulating layer. It should be noted that the metal foil used in the metal foil-clad laminate may be the same as the metal foil described above.
[0110] In addition, the metal foil-clad laminate of the present embodiment can be made by, for example, taking a piece of the resin film or overlapping a plurality of the resin films, and overlapping a metal foil such as copper foil on the upper and lower surfaces or one side surface thereof, and heating and pressing the same to form a laminated body, thereby making a laminate with metal foil on both sides or one side. The heating and pressing conditions can be appropriately set according to the thickness of the laminate to be manufactured, the type of the resin composition, etc., for example, the temperature can be set to 150 to 220° C., the pressure can be set to 1.5 to 5.0 MPa, and the time can be set to 60 to 180 minutes.
[0111] Furthermore, the wiring board of the present embodiment comprises: an insulating layer comprising the above-mentioned resin film or a cured product of the above-mentioned resin composition; and wirings provided on at least one selected from the surface and the inside of the insulating layer.
[0112] The resin composition and resin film of the present embodiment are suitable for use as materials for the insulating layer of a wiring board. As a method for manufacturing a wiring board, for example, the metal foil on the surface of the metal foil-clad laminate obtained above is etched to form a circuit (wiring), thereby obtaining a wiring board having a conductor pattern (wiring) as a circuit on the surface of the laminate. As a method for forming a circuit, in addition to the method described above, for example, a method for forming a circuit by a semi-additive process (SAP: Semi Additive Process) or a modified semi-additive process (MSAP: Modified Semi Additive Process) can be cited.
[0113] Since the resin-coated metal foil, metal foil-clad laminate, and wiring board obtained using the resin composition and resin film of the present embodiment are excellent in flexibility, heat resistance, and strength (tensile strength), they are very useful in industrial applications.
[0114] As described above, this specification discloses the techniques of various embodiments, and the main techniques are summarized as follows.
[0115] The stretchable resin composition according to the first aspect of the present invention is a stretchable resin composition comprising an epoxy resin and a curing agent, wherein:
[0116] The weight average molecular weight of the epoxy resin is 50,000 to 3,000,000.
[0117] The polydispersity of the average molecular weight of the epoxy resin, i.e., Mw / Mn, satisfies the following formula (1):
[0118] 1.1≤Mw / Mn≤3.0(1)
[0119] Wherein, Mn is the number average molecular weight, Mw is the weight average molecular weight,
[0120] The curing agent is a crystalline compound,
[0121] The glass transition temperature of a cured product of the stretchable resin composition is 60° C. or lower.
[0122] The stretchable resin composition according to a second aspect of the present invention is the stretchable resin composition according to the first aspect, wherein the epoxy resin has an epoxy equivalent of 500 g / eq or more and 15000 g / eq or less.
[0123] The stretchable resin composition according to the third aspect of the present invention is the stretchable resin composition according to the first or second aspect, wherein the epoxy resin comprises polymerized units (A) of (meth)acrylate having an epoxy group, polymerized units (B) of (meth)acrylate having a cyano group, and polymerized units (C) of (meth)acrylate having an isobornyl group.
[0124] The stretchable resin composition according to a fourth aspect of the present invention is the stretchable resin composition according to any one of the first to third aspects, wherein the epoxy resin contains 1 to 30 parts by mass of the polymerized unit component (B) based on 100 parts by mass of the epoxy resin.
[0125] The stretchable resin composition according to a fifth aspect of the present invention is the stretchable resin composition according to any one of the first to fourth aspects, wherein the epoxy resin contains 1 part by mass or more and 50 parts by mass or less of the polymerized units (C) component based on 100 parts by mass of the epoxy resin.
[0126] A sixth aspect of the present invention is the stretchable resin composition according to any one of the first to fifth aspects, wherein a tensile modulus of a cured product of the stretchable resin composition is 0.1 MPa to 0.5 GPa.
[0127] A seventh aspect of the present invention is the stretchable resin composition according to any one of the first to sixth aspects, wherein a cured product of the stretchable resin composition has a storage modulus of 0.1 MPa or more at 250°C.
[0128] The stretchable resin composition according to an eighth aspect of the present invention is the stretchable resin composition according to any one of the first to seventh aspects, wherein the crystalline compound accounts for 1.0 mass % to 20 mass % of the solid content of the stretchable resin composition.
[0129] A resin sheet material according to a ninth aspect of the present invention comprises the stretchable resin composition according to any one of the first to eighth aspects; and a support overlapping the stretchable resin composition.
[0130] A resin-coated metal foil according to a tenth aspect of the present invention comprises a stretchable resin layer containing the stretchable resin composition according to any one of the first to eighth aspects; and a metal foil overlapping the stretchable resin layer.
[0131] The metal foil-clad laminate according to the eleventh aspect of the present invention comprises an insulating layer formed of a cured product of the stretchable resin composition according to any one of the first to eighth aspects; and a metal foil overlapping the insulating layer.
[0132] A wiring board according to a twelfth aspect of the present invention comprises an insulating layer comprising a cured product of the stretchable resin composition according to any one of the first to eighth aspects; and wiring provided on at least one selected from the surface and the inside of the insulating layer.
[0133] A thirteenth aspect of the present invention is the stretchable resin composition according to any one of the first to eighth aspects, wherein the stretchable resin composition further contains a conductive powder.
[0134] Example
[0135] First, various materials used in this example are as follows.
[0136] <Method for preparing epoxy resin 1>
[0137] Acrylonitrile as a polymerized unit (B), isobornyl acrylate as a polymerized unit (C), and a polymerized unit (D) represented by the following formula (1) were mixed in the ratios (overlapping %) listed in Table 1, and glycidyl methacrylate as a polymerized unit (A) was added in such a manner that the epoxy equivalent relative to the total amount of the epoxy resin reached the value listed in Table 1. Then, the mixture was subjected to a polymerization reaction to obtain an epoxy resin 1 (manufactured by Nagase ChemteX Co., Ltd., "PMS-14-67") containing methyl ethyl ketone (MEK) as a solvent. The solid content ratio was 40% by weight, the weight average molecular weight Mw was 290,000, and the polydispersity (Mw / Mn) of the average molecular weight was 2.1.
[0138]
[0139] In the formula, R1 is hydrogen or a methyl group, and R2 is hydrogen or an alkyl group. In addition, X represents an integer.
[0140] <Preparation of Epoxy Resins 2 to 9>
[0141] Epoxy resins 2 to 9 were prepared in the same manner as epoxy resin 1, except that the mixing ratio of the polymerized units (B) to (D) was changed to the values shown in Table 1 and the amount of the polymerized unit (A) added was changed to the values shown in Table 1 so that the epoxy equivalent in each epoxy resin became the values shown in Table 1. In epoxy resins 2 to 9, the solid content ratio was 40% by weight.
[0142] In addition, the number average molecular weight (Mn), weight average molecular weight (Mw), and polydispersity (Mw / Mn) of epoxy resins 1 to 9 are summarized in Table 1 below.
[0143] In addition, each molecular weight and polydispersity were calculated|required as follows.
[0144] First, the dried product of the resin combination obtained in the above-mentioned is immersed in THF and fully stirred, and insoluble components are removed by suction filtration using a PTFE membrane filter, and the dissolved product of the resin combination is obtained. The number average molecular weight Mn and weight average molecular weight Mw of the dissolved product obtained are calculated using the molecular weight calibration curve made by monodisperse polystyrene standard samples. In addition, polydispersity Mw / Mn is calculated based on these. Each molecular weight of each epoxy resin is measured using a gel permeation chromatography device (manufactured by Shimadzu Corporation, Nexera GPC system).
[0145]
[0146] (Curing agent)
[0147] Crystalline compound 1 ("BIOC-E" manufactured by Asahi Organic Materials Co., Ltd., a crystalline phenol derivative)
[0148] Crystalline compound 2 (“PAPS-PN2” manufactured by Asahi Organic Materials Co., Ltd., a crystalline phenol derivative)
[0149] Amine curing agent (non-crystalline) (Mitsui Chemicals Fine Co., Ltd. "D2000", polyetheramine)
[0150] Phenolic curing agent (non-crystalline) (manufactured by Gunei Chemical Industry Co., Ltd., "ELPC75", acid equivalent 211 g / eq.)
[0151] · Carboxylic acid curing agent (non-crystalline) (manufactured by NOF Corporation, "TN-1", acid equivalent 260 g / eq.)
[0152] (Curing accelerator)
[0153] Imidazole curing accelerator (Shikoku Chemical's "2E4MZ", 2-ethyl-4-methylimidazole)
[0154] <Preparation of Resin Films 1 to 13>
[0155] The resin composition of the formulation composition (parts by mass) shown in Table 2 was added to a solvent (methyl ethyl ketone) so that the solid content of the composition reached about 43% by mass, thereby preparing resin varnishes 1 to 13. After standing to defoam, the resin varnishes 1 to 13 were respectively coated on a PET film (manufactured by Mitsui Chemicals Tocell Co., Ltd., SP-PET O1) using a doctor blade. Then, an oven was used to heat at 80°C for 60 minutes and further heated at 160°C for 5 minutes, thereby obtaining semi-cured resin films 1 to 13. Resin films 1 to 6 correspond to the resin films (embodiments) of the present invention, and resin films 7 to 13 are comparative examples.
[0156]
[0157] <Method for producing cured resin films 1 to 13>
[0158] The semi-cured resin films 1 to 13 obtained above were further heated at 180° C. for 1 hour, respectively, to obtain cured resin films 1 to 13 .
[0159] [Evaluation test]
[0160] <Method for measuring glass transition temperature (Tg) and storage modulus at 250°C>
[0161] Each cured resin film (cured resin films 1 to 13) was cut into 10 mm × 30 mm and mounted on a dynamic viscoelasticity measuring device (DMS6100 manufactured by Seiko Instruments Inc.). The test was conducted with a strain amplitude of 10 μm, a frequency of 10 Hz (sine wave), and a heating rate of 5°C / min, and the calculated peak temperature of tanδ was used as the glass transition temperature. In addition, the storage modulus (Mpa) at 250°C was also measured in the same manner using the measuring device.
[0162] In this test, a Tg of 60° C. or higher was evaluated as acceptable, and a storage modulus of 0.1 MPa or higher at 250° C. was evaluated as acceptable.
[0163] <Measurement Method of Tensile Modulus and Elongation at Break>
[0164] Each cured resin film (cured resin films 1 to 13) was cut into a dumbbell shape No. 6 (JIS K 6251, 2017) and mounted on a universal testing machine (AGS-X manufactured by Shimadzu Corporation). The test was conducted at a tensile speed of 25 mm / min, and the slope of r-σ was obtained from all stress (σ) data corresponding to strains (r) of 0 to 0.05 using the least squares method, and the initial tensile modulus (Mpa) was calculated.
[0165] Strain (r) = x / x0 (x is the distance the fixture moves, x0 is the initial distance between fixtures)
[0166] Stress (σ)=F / (d·1) (F is the test force, d is the film thickness, and l is the test piece width). In addition, the elongation (%) of each cured resin film when it was broken was measured using the tester.
[0167] In this test, an initial tensile modulus of 0.1 MPa or more was evaluated as acceptable, and a breaking elongation at 250° C. of 50% or more was evaluated as acceptable.
[0168] <Measurement Method of Tear Strength>
[0169] Each cured resin film (cured resin films 1 to 13) was cut into a specified shape (JIS K 7128-3) and mounted on a universal testing machine (AGS-X manufactured by Shimadzu Corporation). The test was conducted at a tensile speed of 500 mm / min, and the stress (N / mm) at break was measured. In this test, the stress of 30 N / mm or more was evaluated as acceptable.
[0170] The results are summarized in Table 3.
[0171]
[0172] <Inspection>
[0173] The above results show that the resin films (resin films 1 to 6) using the resin composition of the present invention have excellent heat resistance when cured to form a cured film, and have moderate flexibility, will not break even if stretched greatly, and have excellent tear strength. In addition, according to the comparison of Example 4 with other examples, it can be seen that by making the epoxy equivalent of 500g / eq or more and the content of the crystalline compound of 20% by mass or less, it has mechanical strength that can also be applied to a variety of uses.
[0174] On the other hand, in Comparative Example 1 using an epoxy resin with large polydispersity, sufficient tear strength could not be obtained. In addition, in Comparative Example 2 using an epoxy resin with a small molecular weight, sufficient elongation at break could not be obtained, and in Comparative Example 3 using an epoxy resin with an excessively large molecular weight, the storage modulus was below the measurement limit, and sufficient heat resistance could not be obtained. In addition, the cured film of Comparative Example 4 could not obtain a sufficient Tg.
[0175] In Comparative Examples 5 to 7, since resin films containing no crystalline compound as a curing agent were used, the tear strength was extremely low.
[0176] <Production Example of Copper Foil with Semi-cured Resin and Copper Foil with Cured Resin>
[0177] Using the resin varnish 1, copper foil with semi-cured resin and copper foil with cured resin were manufactured.
[0178] First, the resin varnish 1 obtained above was applied to a copper foil (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., CF-T9DA-SV-18) using a doctor blade. Then, the copper foil was heated at 80° C. for 60 minutes and further heated at 180° C. for 5 minutes using an oven, thereby obtaining a copper foil 1 with semi-cured resin having each of the resin films 1 to 13 and the copper foil.
[0179] Then, the copper foil 1 with the semi-cured resin obtained above was further heated at 180° C. for 1 hour, thereby obtaining the copper foil 1 with the cured resin.
[0180] This application is based on Japanese patent application No. 2022-34432 filed on March 7, 2022, and the contents are included in this application.
[0181] In order to describe the present invention, the present invention has been appropriately and fully described above by referring to specific embodiments and drawings, but it should be recognized that those skilled in the art can easily change and / or improve the above-mentioned embodiments. Therefore, as long as the modified embodiments or improved embodiments implemented by those skilled in the art do not deviate from the protection scope of the claims recorded in the claims, the modified embodiments or improved embodiments can be interpreted as being included in the protection scope of the claims.
[0182] Industrial Applicability
[0183] The stretchable resin composition of the present invention has flexibility, heat resistance, and high tear strength, and is therefore useful in various technical fields such as the optical field, the electronic field, the adhesive field, and the medical field.
Claims
1. A stretchable resin composition, characterized in that it contains: Epoxy resin and curing agent, wherein The weight average molecular weight of the epoxy resin is 50,000 to 3,000,000. The polydispersity of the average molecular weight of the epoxy resin, i.e., Mw / Mn, satisfies the following formula (1): 1.1≤Mw / Mn≤3.0 (1) Wherein, Mn is the number average molecular weight, Mw is the weight average molecular weight, The curing agent is a crystalline compound, The glass transition temperature of a cured product of the stretchable resin composition is 60° C. or lower.
2. The stretchable resin composition according to claim 1, characterized in that The epoxy equivalent of the epoxy resin is 500 g / eq or more and 15000 g / eq or less.
3. The stretchable resin composition according to claim 1, characterized in that The epoxy resin includes polymerized units (A) of (meth)acrylate having an epoxy group, polymerized units (B) of (meth)acrylate having a cyano group, and polymerized units (C) of (meth)acrylate having an isobornyl group.
4. The stretchable resin composition according to claim 1, characterized in that The epoxy resin contains 1 part by mass or more and 30 parts by mass or less of the polymerized unit (B) component based on 100 parts by mass of the epoxy resin.
5. The stretchable resin composition according to claim 1, characterized in that The epoxy resin contains 1 part by mass or more and 50 parts by mass or less of the polymerized unit (C) component based on 100 parts by mass of the epoxy resin.
6. The stretchable resin composition according to claim 1, characterized in that The tensile modulus of a cured product of the stretchable resin composition is 0.1 MPa or more and 0.5 GPa or less.
7. The stretchable resin composition according to claim 1, wherein The storage modulus of a cured product of the stretchable resin composition at 250° C. is 0.1 MPa or more.
8. The stretchable resin composition according to claim 1, wherein The crystalline compound accounts for 1.0 mass % or more and 20 mass % or less of the solid content of the stretchable resin composition.
9. A resin sheet material, characterized in that include: The stretchable resin composition according to any one of claims 1 to 8; as well as A support body overlapped with the stretchable resin composition.
10. A metal foil with resin, characterized in that include: A stretchable resin layer comprising the stretchable resin composition according to any one of claims 1 to 8; as well as A metal foil overlapped with the stretchable resin layer.
11. A metal foil-clad laminate, characterized in that include: An insulating layer comprising a cured product of the resin composition according to any one of claims 1 to 8; as well as A metal foil overlaps the insulating layer.
12. A wiring board, characterized in that include: An insulating layer comprising a cured product of the resin composition according to any one of claims 1 to 8; as well as A wiring is provided on at least one selected from the surface and the inside of the insulating layer.
13. The stretchable resin composition according to any one of claims 1 to 8, characterized in that The stretchable resin composition further contains conductive powder.