Composition
By using a combination of curable hydrocarbon resin and antioxidants in electrical insulation materials, the problems of material durability and dielectric properties in high temperature environments are solved, and long-term stability of electrical insulation materials with low dielectric constant and low dielectric loss is achieved. sex.
Patent Information
- Application Number
- CN202380024919.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-18
AI Technical Summary
It is difficult for the existing technology to maintain the durability of electrical insulation materials with low dielectric constant and low dielectric loss in high temperature environments. Especially in electronic devices, the problem of material aging is difficult to solve.
Using a composition containing curable hydrocarbon resin, phenolic antioxidant, thioether antioxidant and phosphorus antioxidant, through specific composition ratio and structural design, an electrical insulation material with excellent dielectric properties and long-term durability is formed. .
It achieves long-term durability and excellent dielectric properties of the material in high-temperature environments, reduces the tangent value of the dielectric loss angle, and improves the stability and heat resistance of the material.
Smart Images

Figure BDA0005022262660000161 
Figure BDA0005022262660000171 
Figure BDA0005022262660000181
Abstract
Description
Technical Field
[0001] The present invention relates to compositions. Background Art
[0002] As communication frequencies develop towards high frequency bands above the gigahertz band, the demand for insulating materials with low dielectric properties also increases. This is because it is known that transmission loss is roughly equal to the sum of conductor loss and dielectric loss proportional to the dielectric loss tangent. Existing materials such as epoxy resins are difficult to reduce dielectric constants and dielectric losses, so new materials continue to be developed. For example, Patent Document 1 discloses an electrical insulating material formed by a graft or block copolymer containing olefin-based and styrene-based polymer segments.
[0003] In terms of the use of electrical insulating materials or materials also called LDM (Low Dielectric Macromonomers) for electronic devices, most of them are continuously exposed to relatively high temperatures, or are required to last for a long time when they cannot be easily replaced. Despite this, there is a trend of requiring lower dielectric constants and dielectric losses than before. In the field of polymer materials, various additives that are generally claimed to inhibit material aging are already on the market, but due to the influence on dielectric constants and dielectric losses, it is not easy to use additives in LDM products.
[0004] For example, Patent Document 2 discloses a solar cell module using a so-called cross-linked copolymer as a sealant and also exemplifies various additives. However, at that time, the level of dielectric constant and dielectric loss required for current LDM products was not considered.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 11-060645
[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-127544 Summary of the invention
[0009] Problems to be solved by the invention
[0010] There is a new problem of achieving the dielectric constant and dielectric loss at the level required for current LDM products, which cannot be achieved by the prior art, and at the same time achieving long-term durability (particularly durability under high temperature exposure).
[0011] Means for solving problems
[0012] In order to solve the above-mentioned problems, the present invention can provide the following aspects.
[0013] Method 1.
[0014] A composition comprising
[0015] (A) a curable hydrocarbon resin;
[0016] (B) phenolic antioxidants;
[0017] (C) a thioether antioxidant; and
[0018] (D) phosphorus antioxidants,
[0019] The total amount of the components (B), (C) and (D) is in the range of 2 to 10 mmol based on 100 g of the component (A) in the composition.
[0020] Method 2.
[0021] The composition according to embodiment 1, wherein, based on 100 g of the mass of the component (A) in the composition, the amount of the component (B) as calculated as the phenol part thereof is in the range of 0.5 to 4 mmol, the amount of the component (C) as calculated as the thioether part thereof is in the range of 0.5 to 4 mmol, and the amount of the component (D) as calculated as the phosphite part thereof is in the range of 0.5 to 4 mmol.
[0022] Method 3.
[0023] The composition according to embodiment 1 or 2, wherein the component (A) comprises an olefin-aromatic vinyl compound-aromatic polyene copolymer.
[0024] Method 4.
[0025] The composition according to Embodiment 3, wherein the component (A) satisfies all of the following conditions (1) to (4).
[0026] (1) The number average molecular weight of the copolymer is 500 to 100,000.
[0027] (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 70% by mass.
[0028] (3) The aromatic polyene monomer unit is one or more selected from polyenes having a carbon number of 5 to 20 and having a plurality of vinyl and / or vinylidene groups in the molecule, and the content of the vinyl and / or vinylidene groups derived from the aromatic polyene monomer unit is 1.5 to less than 20 in terms of number average molecular weight.
[0029] (4) The olefin monomer units are one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units and the aromatic polyene monomer units is 100% by mass.
[0030] Method 5.
[0031] The composition according to any one of embodiments 1 to 4, wherein the dielectric loss tangent value of the cured product of the composition under the condition of a measurement frequency range of 40 GHz obtained by a resonator method is defined as X1, and the dielectric loss tangent value of the cured product of the composition under the condition of a measurement frequency range of 40 GHz obtained by a resonator method after heating the cured product of the composition at 175° C. for 24 hours is defined as X2,
[0032] The value of (X1 / X2) is 2 or less.
[0033] Method 6.
[0034] The composition according to any one of aspects 1 to 5, wherein the component (B) has two or more aromatic rings in one molecule.
[0035] Method 7.
[0036] The composition according to any one of Embodiments 1 to 6, wherein the component (C) has a non-cyclic structure.
[0037] Method 8.
[0038] The composition according to any one of Embodiments 1 to 7, wherein the component (D) has an aromatic ring in the molecule.
[0039] Method 9.
[0040] A cured product, which is a cured product of the composition according to any one of Embodiments 1 to 8.
[0041] Method 10.
[0042] A laminate comprising a metal foil and a layer containing the composition according to any one of aspects 1 to 8.
[0043] Method 11.
[0044] A cured product, which is a cured product of the laminated product according to Embodiment 10.
[0045] Method 12.
[0046] A single-layer CCL, a multi-layer CCL, a single-layer FCCL or a multi-layer FCCL substrate, comprising the cured body described in embodiment 11.
[0047] Effects of the Invention
[0048] The composition according to the present invention can achieve the following effects: it has excellent dielectric properties and exhibits long-term durability even in a severe environment. DETAILED DESCRIPTION
[0049] In this specification, the concept of sheet also includes film. In addition, in this specification, even if it is recorded as film, it also includes the concept of sheet. In this specification, the so-called composition includes the concept of varnish. That is, the composition, especially the liquid composition in the composition, is recorded as varnish. The order of each process included in the method disclosed in this specification can also be freely changed in time series as long as it can exert its effect. Unless otherwise specified, the numerical range in this specification includes its lower limit and upper limit.
[0050] The composition of the present invention is characterized by comprising (A) a curable hydrocarbon resin (hereinafter sometimes referred to as "resin"), and predetermined amounts of (B) a phenolic antioxidant and (C) a thioether antioxidant relative to the (A) curable hydrocarbon resin.
[0051] (A) component can be any curable hydrocarbon resin, having a functional group that can be (heat) cured in the presence of heat or a free radical polymerization initiator. Through the presence of (A) component, the cured product of the present composition can meet the heat resistance required as an electrical insulating material. As a functional group, if it is a functional group that can be cured by heat or free radicals, it is not limited, preferably one or more of the group consisting of vinyl, vinylidene, and allyl. For example, as such a (A) component, it can be a multifunctional vinyl aromatic copolymer obtained by a cationic polymerization reaction described in International Publication No. 2018 / 181842 and International Publication No. 2017 / 115813, or a polyphenylene ether resin having a functional group, such as SA-9000 of SABIC, OPE-2St of Mitsubishi Gas Chemical, or a polyether (ketone) having a functional group, or a polymer or copolymer having a 1,2-polybutadiene structure, such as the trade name "Ricon" of CrayValley. In addition, materials such as olefin-aromatic vinyl compound-aromatic polyene copolymers obtained by single-site coordination polymerization can be cited. They can be one or a composition comprising multiple types. As component (A), it is most preferred to include a multifunctional vinyl aromatic copolymer or an olefin-aromatic vinyl compound-aromatic polyene copolymer whose constituents are substantially carbon atoms and hydrogen atoms.
[0052] As component (A), it is most preferred to include an olefin-aromatic vinyl compound-aromatic polyene copolymer (hereinafter, sometimes referred to as "copolymer"). Olefin-aromatic vinyl compound-aromatic polyene copolymer refers to a compound obtained by copolymerizing each monomer of olefin, aromatic vinyl compound, and aromatic polyene. Component (A) can be a monomer, an oligomer, or a mixture thereof. Component (A) preferably satisfies all of the following conditions (1) to (4).
[0053] (1) The number average molecular weight of the copolymer is 500 to 100,000.
[0054] (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 70% by mass.
[0055] (3) The aromatic polyene monomer unit is one or more selected from polyenes having a carbon number of 5 to 20 and having a plurality of vinyl and / or vinylidene groups in the molecule, and the content of the vinyl and / or vinylidene groups derived from the aromatic polyene monomer unit is 1.5 to less than 20 in terms of number average molecular weight.
[0056] (4) The olefin monomer units are one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is 100% by mass.
[0057] The so-called olefin monomer can be selected from one or more of alpha olefins with a carbon number of 2 or more and 20 or less and cyclic olefins with a carbon number of 5 or more and 20 or less, and refers to a compound substantially free of oxygen, nitrogen, and halogen and composed of carbon and hydrogen. As alpha olefins with a carbon number of 2 or more and 20 or less, for example, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, 3,5,5-trimethyl-1-hexene, etc. can be exemplified. As cyclic olefins with a carbon number of 5 or more and 20 or less, norbornene and cyclopentene can be exemplified. As olefins, a combination of alpha olefins other than ethylene and ethylene, cyclic olefins, or ethylene alone can be preferably used. The amount of alpha olefins other than ethylene added can be selected according to the target molecular weight.
[0058] From the viewpoint of improving the peel strength with copper foil and copper wiring, the olefin monomer is ethylene alone, or the mass ratio of the alpha olefin component / ethylene component contained in the copolymer is preferably 1 / 7 or less, and more preferably 1 / 10 or less. In this case, the content of the alpha olefin monomer component other than ethylene contained in the copolymer is more preferably 6% by mass or less, and most preferably 4% by mass or less, or the olefin is ethylene alone.
[0059] When the total of olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is set to 100% by mass, the content of olefin monomer units in this copolymer is preferably 20% by mass or more, more preferably 25% by mass or more, and most preferably 30% by mass or more. When the content of olefin monomer units is 20% by mass or more, the toughness (elongation) and impact resistance of the finally obtained solidified body are improved, and the rupture of the solidified body in the midway of curing and the rupture of the solidified body in the thermal cycle test are not easy to occur. In this copolymer, the content of olefin monomer units is preferably 90% by mass or less.
[0060] The aromatic vinyl compound monomer may be an aromatic vinyl compound having 8 to 20 carbon atoms, and examples thereof include styrene, p-methylstyrene, p-isobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.
[0061] The content of the aromatic vinyl compound monomer unit included in this copolymer can be 0 mass % or more and 70 mass % or less, preferably 10 mass % or more and 60 mass % or less. When the content of the aromatic vinyl compound monomer unit is 70 mass % or less, the glass transition temperature of the cured product of the resin composition finally obtained is lower than near room temperature, and the toughness and elongation at low temperatures can be improved, so it is preferred. When the content of the aromatic vinyl compound monomer unit is 10 mass % or more, the following effects can be obtained: the aromaticity of this copolymer is improved, the affinity with flame retardants and fillers becomes good, the exudation of flame retardants can be avoided, and the filling property of fillers can be improved. In addition, when the content of the aromatic vinyl compound monomer unit is 10 mass % or more, a cured product with a high peel strength from copper foil and copper wiring can also be obtained.
[0062] As an aromatic polyene monomer, it can be a polyene with a carbon number of 5 or more and 20 or less having multiple vinyl and / or vinylidene groups in its molecule, preferably various divinylbenzenes at ortho, meta, and para positions or mixtures thereof, divinylnaphthalene, divinylanthracene, p-2-propylene styrene, p-3-butylene styrene, etc. having an aromatic vinyl structure and substantially free of oxygen, nitrogen, and halogen and composed of carbon and hydrogen. In addition, bifunctional aromatic vinyl compounds such as 1,2-bis(vinylphenyl)ethane (abbreviated as: BVPE) described in Japanese Patent Publication No. 2004-087639 can also be used. Among them, various divinylbenzenes at ortho, meta, and para positions, or mixtures thereof are preferably used, and a mixture of meta and para divinylbenzenes can be used most preferably. In this specification, these divinylbenzenes are sometimes collectively described as divinylbenzenes. When divinylbenzenes are used as aromatic polyenes, the curing efficiency is high and the curing is easy during the curing treatment, so it is preferred.
[0063] As each monomer of the above olefin, aromatic vinyl compound, aromatic polyene, it is also possible to include in addition: olefin containing polar groups such as oxygen atoms, nitrogen atoms, etc.; aromatic vinyl compounds containing oxygen atoms, nitrogen atoms, etc.; or aromatic polyene containing oxygen atoms, nitrogen atoms, etc. The total mass of these monomers containing polar groups is preferably less than 10% by mass of the total mass of this composition, more preferably less than 3% by mass, most preferably without the monomer containing polar groups. By making the ratio of the total mass of the monomer containing polar groups less than 10% by mass, the dielectric properties (low dielectric constant, low dielectric loss) of the cured body obtained by curing this composition can be improved.
[0064] Examples of the copolymer not containing an aromatic vinyl compound monomer unit (olefin-aromatic polyene copolymer) include ethylene-divinylbenzene copolymer, ethylene-propylene-divinylbenzene copolymer, ethylene-1-butene-divinylbenzene copolymer, ethylene-1-hexene-divinylbenzene copolymer, ethylene-1-octene-divinylbenzene copolymer, and the like.
[0065] Examples of the copolymer containing an aromatic vinyl compound monomer unit (olefin-aromatic vinyl compound-aromatic polyene copolymer) include ethylene-styrene-divinylbenzene copolymer, ethylene-propylene-styrene-divinylbenzene copolymer, ethylene-1-hexene-styrene-divinylbenzene copolymer, ethylene-1-octene-styrene-divinylbenzene copolymer, and the like.
[0066] The number average molecular weight (Mn) of the copolymer may be 500 to 100,000, preferably 500 to 50,000, more preferably 500 to 20,000, and more preferably 500 to 10,000. When Mn is 100,000 or less, a suitable viscosity for a varnish can be obtained, and the effect of improving the workability when using the composition can be obtained.
[0067] The weight average molecular weight (Mw) of the copolymer may preferably be 10,000 to 200,000, more preferably 20,000 to 200,000, and more preferably 20,000 to 150,000. Preferably, the value Mw / Mn obtained by dividing the weight average molecular weight by the number average molecular weight may be in the range of 2.0≤Mw / Mn≤13.0, more preferably 2.0≤Mw / Mn≤12.0, and more preferably 2.0≤Mw / Mn≤10.0.
[0068] The number average molecular weight and weight average molecular weight in this specification refer to values measured as molecular weights converted to standard polystyrene by gel permeation chromatography (GPC). The measurement conditions of the GPC method in this specification are as follows.
[0069] Measurement device: Viscotek GPCMax
[0070] Chromatographic column: TSK-GEL MultiporeHXL-M, x 300mm 3 pieces
[0071] Column temperature: 40°C
[0072] Detector: RI
[0073] Solvent: THF
[0074] Liquid delivery flow: 1.0ml / min
[0075] Sample concentration: 0.2wt / Vol%
[0076] Sample injection volume: 200 μL
[0077] In the present copolymer, the content of vinyl and / or vinylidene groups (preferably vinyl groups) derived from aromatic polyene units can be 1.5 or more and less than 20, preferably 2 or more and less than 7, in terms of number average molecular weight. When the content of the vinyl and / or vinylidene groups is 1.5 or more, the crosslinking efficiency is high, and a cured product with a sufficient crosslinking density can be obtained. The vinyl content derived from aromatic polyene units (divinylbenzene units) in the copolymer in terms of number average molecular weight can be obtained by dividing the number average molecular weight (Mn) calculated by the GPC (gel permeation chromatography) method known to those skilled in the art by the standard polystyrene conversion and the crosslinking density by the number average molecular weight (Mn) calculated by the GPC (gel permeation chromatography) method known to those skilled in the art by the crosslinking density (Mn). 1 The vinyl content derived from the aromatic polyene unit obtained by H-NMR measurement is compared. 1 Comparison of the intensity of each peak area obtained by H-NMR measurement shows that the vinyl content derived from the aromatic polyene unit (divinylbenzene unit) in the copolymer is 0.6% by mass, and the number average molecular weight based on standard polystyrene conversion measured by GPC is 49,000. The molecular weight of the vinyl derived from the aromatic polyene unit in the number average molecular weight is the product of these, i.e., 299, which is divided by the formula weight of the vinyl, 130, to obtain 2.3. That is, the vinyl content derived from the aromatic polyene unit in the copolymer in terms of number average molecular weight is 2.3. 1 The attribution of the peaks obtained by H-NMR measurement is known from the literature. 1 A method for determining the composition of a copolymer by comparing the peak areas obtained by H-NMR measurement is also known. 1 Based on the H-NMR method, the quantitative model was used to determine 13The peak area and ratio of the C-NMR spectrum are used to improve the accuracy of the composition. In addition, in this specification, the content of divinylbenzene units in the copolymer is determined based on the peak intensity of the vinyl group derived from the divinylbenzene unit (based on 1 That is, based on the content of vinyl groups derived from divinylbenzene units, one vinyl group is regarded as one divinylbenzene unit derived from the copolymer, and the content of divinylbenzene units is determined.
[0078] The phenolic antioxidant as the component (B) included in the present composition is a component that exerts a synergistic effect of imparting excellent durability to the present composition by combining with the components (C) and (D) described later and using them in a prescribed amount. The present invention is characterized in that if different types of antioxidants are simply combined without considering the amount, a significant effect cannot be exerted in a composition with a specific component (A) as a main component.
[0079] In a preferred embodiment, the dielectric loss tangent value of the solidified body of the present composition under the condition of a measurement frequency range of 40 GHz obtained by a resonator method is set to X1, and the dielectric loss tangent value of the solidified body of the present composition under the condition of a measurement frequency range of 40 GHz obtained by a resonator method after heating the solidified body of the present composition at 175°C for 24 hours is set to X2, and the value of (X1 / X2) can be 2 or less, more preferably 1.5 or less, and further preferably 1.2 or less. That is, the present composition can present an effect that the dielectric loss tangent is not easily damaged even when heated (or, natural degradation caused by long-term placement equivalent to being heated).
[0080] More preferably, as a synergistic effect of the components (B), (C) and (D), an effect that the storage elastic modulus does not deteriorate compared to before the addition of the antioxidant can be obtained.
[0081] Regarding the amount of component (B), based on 100 g of component (A), the amount (molar equivalent) of component (B) based on the phenolic moiety is in the range of 0.5 to 4 mmol, more preferably in the range of 0.5 to 3 mmol, and even more preferably in the range of 0.5 to 2.5 mmol.
[0082] Component (B) refers to a compound having a phenolic skeleton (site) and having the function of terminating a free radical chain reaction. Component (B) may include a monophenolic antioxidant, a polyphenolic antioxidant (bisphenolic antioxidant, triphenolic antioxidant, etc.), or a mixture thereof. Component (B) preferably includes a hindered phenolic antioxidant (a compound having a substituent such as a tert-butyl group on the aromatic ring of the phenolic site that becomes a bulky steric hindrance). From the viewpoint of improving thermal durability, component (B) may have two or more aromatic rings in one molecule.
[0083] Examples of the monophenol antioxidant include octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, butylated hydroxyanisole, 2,6-di-tert-butyl-4-ethylphenol, stearyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl (meth)acrylate, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl (meth)acrylate, and 6-tert-butyl-4-[3-[(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphin-6-yl)oxy]propyl]-2-methylphenol. These are available, for example, under the trade names of Sumilizer GS, Sumilizer GM, and Sumilizer GP (manufactured by Sumitomo Chemical Co., Ltd.).
[0084] Examples of polyphenol antioxidants include 2,2-methylene-bis(4-methyl-6-tert-butylphenol), N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane (4,4',4"-(1-Methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol)), 6,6'-di-tert-butyl-4,4'-butylene di-m-cresol, 3,9-bis{2 -[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoic acid] 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl ester, 2,2'-methylenebis(6-tert-butyl-p-cresol), 4,4'-thiobis(6-tert-butyl-m-cresol). These can be obtained, for example, under the trade name Sumilizer GA-80, Sumilizer MDP-S, Sumilizer WX-R (manufactured by Sumitomo Chemical Co., Ltd.), etc. These may be used alone or in combination of two or more.
[0085] The thioether antioxidant as the component (C) contained in the present composition refers to a compound having a thioether skeleton (site) and having the function of terminating a free radical chain reaction. The amount of the component (C) is such that, based on 100 g of the mass of the component (A), the amount (molar equivalent) of the component (C) based on the thioether site is in the range of 0.5 to 4 mmol, more preferably in the range of 0.5 to 3 mmol, and even more preferably in the range of 0.5 to 2.5 mmol.
[0086] In addition, based on 100 g of the mass of component (A) in the present composition, the total amount of component (B) and the amount of component (C) may be in the range of 1 to 10 mmol or in the range of 2 to 10 mmol, more preferably in the range of 2 to 8 mmol, and even more preferably in the range of 2 to 7 mmol.
[0087] Examples of the component (C) include dialkyl thiodipropionate, (ditridecyl 3,3'-thiodipropionate, dilauryl thiodipropionate, dimyristyl thiodipropionate, distearyl thiodipropionate, etc.), pentaerythritol tetra(β-alkylthiopropionate), and bis[3-(dodecylthio)propionic acid] 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl ester. These may be used alone or in combination of two or more.
[0088] From the viewpoint of enhancing the synergistic effect with the component (B), the component (C) preferably has a non-cyclic structure.
[0089] In a preferred embodiment, the present composition may further include a phosphorus antioxidant (D). With respect to the amount of the component (D), based on the mass of the component (A) in the composition of 100 g, the amount of the component (D) in terms of the phosphite ester site is preferably in the range of 0.5 to 4 mmol, more preferably in the range of 0.5 to 3 mmol, and further preferably in the range of 0.5 to 2.5 mmol. In addition, based on the mass of the component (A) in the composition of 100 g, the total amount of the components (B), (C) and (D) is preferably in the range of 2 to 10 mmol, more preferably in the range of 2 to 8 mmol, and further preferably in the range of 2 to 7 mmol.
[0090] By combining the three antioxidants in a predetermined amount, a synergistic effect is further exerted to obtain extremely excellent dielectric properties. In particular, even a slight difference in the dielectric loss tangent (a difference of the order of 0.0001) has a great impact, so even a slight reduction can be considered a significant effect.
[0091] Examples of the component (D) include 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,2'-methylenebis(4,6-di-tert-butylphenyl)2-ethylhexyl phosphite, tris(nonylphenyl)phosphite, distearyl pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)phosphite, and the like. diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)octylphosphite, tetrakis(tridecyl)-4,4'-butylenebis(3-methyl-6-tert-butylphenyl)diphosphite, 2,2'-ethylenebis(4,6-di-tert-butylphenyl)fluorophosphite, bis(2,4,6-tri-tert-butylphenyl)pentaerythritol diphosphite.
[0092] From the viewpoint of enhancing the synergistic effect of the three antioxidants, the component (D) preferably has an aromatic ring in the molecule.
[0093] The present composition may further contain any additional components exemplified below unless the effects thereof are impaired.
[0094] <Curing agent>
[0095] As the curing agent that can be used in the present composition, known curing agents that can be used in the polymerization or curing of aromatic polyenes and aromatic vinyl compounds can be used. Examples of such curing agents include free radical polymerization initiators, cationic polymerization initiators, and anionic polymerization initiators, and free radical polymerization initiators can be used preferably. Organic peroxide-based (peroxide) and azo-based polymerization initiators are preferred, and can be freely selected according to the application and conditions. The product catalog that records organic peroxides can be found on the homepage of NOF Corporation, for example https: / / ww w.nof.co.jp / business / chemical / chemical-product01 Download. In addition, organic peroxides are also listed in the product catalogs of Fujifilm Wako Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. Curing agents can be obtained from these companies. In addition, known photopolymerization initiators using light, ultraviolet rays, and radiation can also be used as curing agents. As curing agents using photopolymerization initiators, photoradical polymerization initiators, photocationic polymerization initiators, or photoanionic polymerization initiators can be cited. Such photopolymerization initiators can be obtained, for example, from Tokyo Chemical Industry Co., Ltd. In addition, curing can also be performed using radiation or electron beams themselves. In addition, crosslinking and curing can also be performed by thermal polymerization of the raw materials contained without containing a curing agent.
[0096] The amount of the curing agent used is not particularly limited, and is generally preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the composition. The composition preferably does not include a curing agent or a solvent. When using a curing agent such as a peroxide (peroxide) or an azo polymerization initiator, the curing treatment is performed at an appropriate temperature and time in consideration of its half-life. The conditions in this case are optional depending on the curing agent, and generally, a temperature range of about 50°C to 200°C is suitable.
[0097] <Solvent (solvent)>
[0098] For this composition, an appropriate solvent can be added as needed. The solvent is used to adjust the viscosity and fluidity of the composition. As a solvent, a volatile solvent is preferred, for example, cyclohexane, toluene, ethylbenzene, acetone, isopropanol, etc. can be used. In addition, as far as its usage is concerned, from the perspective of the molding processability and operation of the composition before curing as a thermoplastic resin, it is preferably 10 parts by mass or less relative to 100 parts by mass of the copolymer. In addition, from the perspective of removal during and after curing, it is more preferred that no solvent is substantially used. Substantially no use means preferably 5 parts by mass or less, more preferably 1 part by mass or less, and most preferably 0 parts by mass. In addition, when used as a varnish, it is preferred to add an appropriate solvent to this composition. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As a solvent, when the boiling point at atmospheric pressure is high, that is, when the volatility is low, the thickness of the film obtained by coating becomes uniform, so it is preferred to have a solvent with a boiling point above a certain degree. The preferred boiling point is about 100°C or more at atmospheric pressure, preferably 130°C or more and 300°C or less. As a solvent suitable for such a varnish, toluene, xylene, mesitylene, ethylbenzene, limonene, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, etc. can be used. In addition, the amount used is preferably in the range of 10 to 2000 parts by mass relative to 100 parts by mass of the present composition.
[0099] The present composition can also be made into a viscous liquid varnish according to its composition and mixing ratio. For example, by using a sufficient amount of solvent and / or by using a proper amount of liquid monomer, it can be made into a varnish. When used as a varnish, it is preferred to add a suitable solvent to the present composition. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As a solvent, when the boiling point at atmospheric pressure is high, that is, when the volatility is low, it has the advantage that the thickness of the film obtained by coating becomes uniform, so it is preferred to use a solvent with a boiling point of a certain degree or more. The preferred boiling point is about 100°C or more at atmospheric pressure, preferably 110°C or more and 300°C or less. As a solvent suitable for such a varnish, xylene, mesitylene, ethylbenzene, limonene, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, etc. can be used. In addition, its usage amount is preferably in the range of 10 to 2000 parts by mass relative to 100 parts by mass of the present composition. The varnish-like composition can also be made using a polymerization liquid containing the present copolymer obtained by polymerization. For example, the polymerization solution may be concentrated or the residual monomers may be removed. Alternatively, a solvent, other resin components, various additives, etc. may be added as necessary to adjust the component concentrations, solution viscosity, etc. for production.
[0100] The varnish can be applied or impregnated on a substrate, for example, and the solvent can be removed by drying, etc., thereby forming an uncured or semi-cured molded body. Usually, the molded body has a sheet, film, or tape form.
[0101] <Curing>
[0102] The curing of the present composition can be carried out by referring to the curing conditions (temperature, time, pressure) of the included curing agent and by known methods. When the curing agent used is a peroxide, the curing conditions can be determined by referring to the half-life temperature disclosed for each peroxide.
[0103] In the present invention, a laminate comprising a layer containing the above-mentioned composition and a metal foil can also be provided. That is, the present composition can be used as various insulating materials for wiring (preferably for wiring of high-frequency signals), such as a cover layer, a solder resist, a buildup material, an interlayer insulating agent, a bonding sheet, an interlayer adhesive, and a bump sheet for a flip chip bonding machine. In addition, it can also be used as an electrical insulating layer and an adhesive layer of a substrate substrate such as a single-layer or multi-layer printed substrate, a flexible printed substrate, a CCL (copper-clad laminate), and a FCCL (flexible copper-clad laminate) substrate.
[0104] <Viscosity>
[0105] In this specification, the viscosity of the composition is obtained in accordance with JIS Z 8803:2011 when it is prepared as a 50 mass % toluene solution. The viscosity of the composition at 25°C is determined at a shear rate of 1 s-1 Under the condition of , it can be 100000 cP or less, preferably 10000 cP or less or 9000 cP or less, further preferably 8000 cP or less, more preferably 5000 cP or less. The lower limit of the viscosity is not particularly limited, for example, it can be 500 cP or more, preferably 1000 cP or more. By making the viscosity within such a range, the effect of improving the operability of the varnish can be obtained.
[0106] <Manufacturing method>
[0107] The composition containing the copolymer can be obtained by mixing the olefin monomer, the aromatic vinyl compound monomer and the aromatic polyene monomer in a suitable solvent to prepare a raw material solution, and subjecting the raw material solution to a single-site coordination polymerization reaction. In another embodiment, a step of polymerizing in a liquid monomer without using a solvent can be used instead. In another embodiment, the vinyl aromatic copolymer can be obtained by a cationic polymerization reaction.
[0108] As the solvent that can be used, there can be mentioned saturated aliphatic or aromatic hydrocarbons such as pentane, hexane, heptane, cyclohexane, methylcyclohexane, benzene, toluene, ethylbenzene, xylene, mesitylene, limonene, chlorine-substituted benzene, chlorine-substituted toluene, dichloromethane, chloroform, or a single halogenated hydrocarbon or a mixed solvent. Preferably, a mixed alkane solvent, cyclohexane, toluene, ethylbenzene, etc. can be used as the solvent.
[0109] It should be noted that the copolymer can be produced even without using a chain transfer agent, but a chain transfer agent may be used to reduce the molecular weight. As such a chain transfer agent, a known chain transfer agent used together with a so-called single-site coordination polymerization catalyst may be used, for example, hydrogen, alkyl aluminums such as triisobutyl aluminum, 9-BBN described in Chung TC: Macromolecules, 26, 3467 (1993), etc.
[0110] The equipment capable of producing the present composition may be, for example, a single or multiple connected tank-type polymerization tank, a linear or annular single or multiple connected pipeline polymerization equipment, etc. The pipeline-shaped polymerization tank may have various known mixers such as a dynamic or static mixer, a static mixer with heat removal function, and various known coolers such as a cooler with a heat removal capillary. In addition, it may also have a batch prepolymerization tank. In addition, a gas phase polymerization process may also be adopted.
[0111] The polymerization temperature is preferably 0 to 200° C. When it is 0° C. or higher, the polymerization rate is fast, which is industrially advantageous. When it is 200° C. or lower, the effect of not decomposing the transition metal compound can be obtained. In addition, it is industrially preferably 30 to 160° C., and particularly preferably 50 to 160° C. The pressure during the polymerization is usually preferably 1 to 100 atmospheres, more preferably 1 to 30 atmospheres, and most preferably 1 to 10 atmospheres industrially.
[0112] When the copolymer is recovered from the reaction system after the polymerization is completed, any process can be used, and preferably, the steam stripping method and the crumb forming method, which are so-called methods for recovering raw rubber, can be used. In the laboratory, the method of precipitating the copolymer in a large amount of methanol, the so-called methanol precipitation method, is convenient. In addition, the copolymer can be removed from the polymerization solution by an evaporation method based on a rotary evaporator, a thin film evaporator, etc. without recovering the copolymer, and the solvent and the residual monomers can be removed in whole or in part, and diluted with a solvent, and can also be used as a varnish.
[0113] Example
[0114] With reference to the manufacturing method of International Publication No. 00 / 37517, Japanese Patent Publication No. 2009-161743, Japanese Patent Publication No. 2010-280771, the amount of monomer, ratio, polymerization pressure, polymerization temperature are appropriately changed to obtain the copolymers shown in Table 1. The total of olefin monomer units, aromatic vinyl compound monomer units and aromatic polyene monomer units is set to 100 mass%. Table 1 also shows the number average molecular weight of the copolymer. The determination of molecular weight is carried out as described above.
[0115] <Vinyl unit content>
[0116] The content of vinyl units derived from ethylene, styrene and divinylbenzene in the copolymer is determined by 1 H-NMR was determined based on the intensity of the peak area assigned to each sample. The sample was dissolved in deuterated 1,1,2,2-tetrachloroethane and the measurement was performed at 23°C.
[0117] Each of Examples and Comparative Examples was prepared using copolymers P-1 to P-3 according to the composition shown in Table 2. The amount of the antioxidant is indicated by the amount of substance (mmol equivalent) calculated as each functional group site when 100 parts by mass of the copolymer is assumed to be 100 g.
[0118] [Table 1]
[0119]
[0120] [Table 2]
[0121]
[0122] [Table 3]
[0123]
[0124] The main raw materials are as follows. Divinylbenzene was divinylbenzene (meta- and para-mixed product, divinylbenzene purity 81%) manufactured by NIPPON STEEL Chemical & Material Co., Ltd. As a curing agent, Perhexyne 25B (2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyne) manufactured by NOF Corporation was used. As a solvent, toluene (commercially available product) was used.
[0125] The (B) component used is as follows.
[0126] 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane ("ADK STAB AO-80" manufactured by ADEKA Corporation, molecular weight 741)
[0127] The component (C) used is as follows.
[0128] 2,2-bis{[3-(dodecylthio)-1-oxopropoxy]methyl}propane-1,3-diyl bis[3-(dodecylthio)propanoate ("ADK STAB AO-412S" manufactured by ADEKA Corporation, molecular weight 1162)
[0129] 3,3'-Ditridecyl thiodipropionate ("ADK STAB AO-503" manufactured by ADEKA Corporation, molecular weight 543)
[0130] The component (D) used is as follows.
[0131] 3,9-Bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane ("ADK STAB PEP-36" manufactured by ADEKA Corporation, molecular weight 633)
[0132] <Production of varnish and cured sheet>
[0133] Using a container with a heating and cooling jacket and a stirring blade, P-1 (ethylene-styrene-divinylbenzene copolymer) obtained in the synthesis example and a solvent (toluene) are heated to about 60°C and stirred to dissolve the copolymer. Further, the prescribed weight parts of antioxidants and curing agents shown in Tables 2 to 3 are added to 100 weight parts of the resin component and dissolved, and stirred and mixed to obtain a varnish-like composition. It should be noted that the amount of the antioxidant shown in the table is the value when the mass of the copolymer is set to 100g. The obtained composition is poured into a silicon mold frame (frame part length 7cm, width 7cm, thickness 0.5mm, 1.0mm, or 2.0mm) on a Teflon (registered trademark) sheet set on a glass plate, and after air drying, it is further dried at 60°C in a vacuum dryer for more than 3 hours to obtain an uncured sheet. Furthermore, a Teflon sheet and a SUS mold frame were set under a load of 5 MPa using a pressing machine, and were heated at 120°C for 30 minutes, at 150°C for 30 minutes, and then at 200°C for 120 minutes. The Teflon sheet and the SUS mold frame were removed to obtain a cured sheet.
[0134] <Measurement of dielectric loss (dielectric loss tangent)>
[0135] As for the dielectric loss tangent, the cavity perturbation method (8722ES network analyzer manufactured by Agilent Technology, split cylindrical resonator 40GHz manufactured by Keysight Technologies) was used to measure the value at 23°C and 40GHz using a 0.2mm×25mm×30mm sample cut from a sheet. In order to confirm the high temperature resistance to thermal oxidation degradation of the material, the sheet was placed at 175°C in an air atmosphere for 24 hours, and then the dielectric loss tangent was measured. The ratio of the dielectric loss tangent value (X1) before heating to the dielectric loss tangent value (X2) after heating, i.e., the value of the rate of change X1 / X2 (the "rate of change of dielectric loss tangent before and after heating" in the table) was judged to be no degradation when it was less than 1.2, and the degradation was judged to be within the allowable range when it was greater than 1.2 and less than 2.0, and it was judged to be degradation when it was greater than 2.0.
[0136] <Measurement of storage modulus>
[0137] The dynamic viscoelasticity measuring device (RSA-G2 from Rheometrics) was used to measure the storage modulus at a frequency of 1 Hz and a temperature range of 20°C to +300°C. The storage modulus was determined by cutting out a sample (3 mm x 40 mm) from a film having a thickness of about 0.2 mm. The main measurement parameters related to the measurement are as follows.
[0138] Measuring frequency 1Hz
[0139] Heating rate: 3℃ / min
[0140] Sample measurement length 13mm
[0141] Test Type = Dynamic Temperature Ramp (DTempRamp)
[0142] Initial Static Force: 5.0g
[0143] Auto Tension SensitiVity: 1.0g
[0144] Max Auto Tension Rate: 0.033mm / s
[0145] Maximum applied strain: 1.5%
[0146] Minimum allowable torque (Min Allowed Force) 1.0g
[0147] Strain 0.1%
[0148] In the storage modulus value at 25°C, whether the storage modulus deteriorates due to the addition of the antioxidant was evaluated based on the following criteria ("Deterioration of 25°C DMA storage modulus" in the table). When the storage modulus value of the sample without adding an antioxidant (before heating) was set to 1, if the storage modulus value of the sample with added antioxidant was 0.8 or more, the deterioration was recorded as "no", and if it was less than 0.8, the deterioration was recorded as "yes".
[0149] <Appearance Evaluation>
[0150] In order to confirm the high-temperature resistance to thermal oxidative degradation of the material, the sheet was left to stand in an air atmosphere at 175° C. for 24 hours, and then the color change of the sheet was visually evaluated (“discoloration after heating” in the table).
[0151] The above evaluation results are also shown in Tables 2 to 3. In any of the Examples, the storage modulus did not deteriorate, the color did not change after heating, and the dielectric loss tangent did not deteriorate after heating.
[0152] On the other hand, in Comparative Example 1 in which no antioxidant was added, the color was changed by heating and the product was severely damaged, so it was not suitable for practical use.
[0153] In Comparative Example 2 in which no antioxidant was added, the color was changed by heating, and the dielectric loss tangent was greatly deteriorated.
[0154] In Comparative Examples 3 to 5 in which only the component (B) was used as the antioxidant, all of them changed color due to heating.
[0155] In Comparative Example 6 in which only the component (D) was used as the antioxidant, the dielectric loss tangent was significantly deteriorated by heating.
[0156] In Comparative Example 7 in which only the component (C) was used as the antioxidant, the dielectric loss tangent was significantly deteriorated by heating.
[0157] In Comparative Example 8, in which the antioxidant (B) and (C) components were used but the total amount of substances was small, the dielectric loss tangent was significantly deteriorated by heating.
[0158] In Comparative Example 9 in which the antioxidant (B), (C), and (D) components were used but the total amount of substances was small, the dielectric loss tangent was significantly deteriorated by heating.
[0159] In Comparative Example 10 in which the antioxidant (B) and (C) components were used but the total amount of substances was too large, the dielectric loss tangent was too high both before and after heating.
Claims
1. A composition comprising: (A) a curable hydrocarbon resin; (B) phenolic antioxidants; (C) a thioether antioxidant; and (D) phosphorus antioxidants, The total amount of the components (B), (C) and (D) is in the range of 2 to 10 mmol based on 100 g of the component (A) in the composition.
2. The composition according to claim 1, wherein Based on 100 g of the mass of the component (A) in the composition, the amount of the component (B) calculated as the phenol part is in the range of 0.5 to 4 mmol, the amount of the component (C) calculated as the thioether part is in the range of 0.5 to 4 mmol, and the amount of the component (D) calculated as the phosphite part is in the range of 0.5 to 4 mmol.
3. The composition according to claim 1 or 2, wherein The component (A) contains an olefin-aromatic vinyl compound-aromatic polyene copolymer.
4. The composition according to claim 3, wherein (A) The component satisfies all of the following conditions (1) to (4), (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less; (2) the aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 70% by mass; (3) the aromatic polyene monomer unit is one or more selected from polyenes having a plurality of vinyl and / or vinylidene groups in the molecule and having a carbon number of 5 to 20, and the content of vinyl and / or vinylidene groups derived from the aromatic polyene monomer unit is 1.5 to less than 20 in terms of number average molecular weight; (4) The olefin monomer units are one or more selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units and the aromatic polyene monomer units is 100% by mass.
5. The composition according to any one of claims 1 to 4, wherein When the dielectric loss tangent value of the cured product of the composition in the measurement frequency range of 40 GHz obtained by the resonator method is set as X1, and the dielectric loss tangent value of the cured product of the composition in the measurement frequency range of 40 GHz obtained by the resonator method after heating the cured product of the composition at 175° C. for 24 hours is set as X2, The value of (X1 / X2) is 2 or less.
6. The composition according to any one of claims 1 to 5, wherein The component (B) has two or more aromatic rings in one molecule.
7. The composition according to any one of claims 1 to 6, wherein The component (C) has a non-cyclic structure.
8. The composition according to any one of claims 1 to 7, wherein The component (D) has an aromatic ring in the molecule.
9. A cured product, which is a cured product of the composition according to any one of claims 1 to 8. 10 . A laminate comprising a metal foil and a layer containing the composition according to claim 1 .
11. A cured product, which is a cured product of the laminated product according to claim 10.
12. A single-layer CCL, a multi-layer CCL, a single-layer FCCL or a multi-layer FCCL substrate, comprising the cured body according to claim 11.