Method for evaluating optical film

By arranging a substrate with a straight portion on the outer periphery of the optical film, and performing optical axis measurement and correction based on the straight portion of the substrate, the problem of inaccurate optical axis measurement of the optical film is solved and accurate evaluation of the optical axis of the optical film is achieved.

CN118805077APending Publication Date: 2024-10-18NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027745.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-09
Filing Date
2023-03-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

It is difficult to accurately grasp the optical axis of the optical film in the existing technology, especially when the shapes are different, resulting in inaccurate measurement of the optical axis.

Method used

The optical film is disposed on a substrate with a linear portion on the outer periphery, and the optical axis of the optical film is measured based on the linear portion of the substrate, and correction is performed based on the positional relationship between the substrate and the optical film.

Benefits of technology

This method can significantly improve the evaluation accuracy of the optical axis of the optical film and ensure the accuracy of the optical axis measurement results of the optical film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118805077A_ABST
    Figure CN118805077A_ABST
Patent Text Reader

Abstract

The present invention accurately evaluates the optical axis of an optical film. An evaluation method according to an embodiment of the present invention is an evaluation method for an optical film. The method includes: disposing the optical film on a substrate having a linear portion on an outer periphery thereof; measuring the optical axis of the optical film on the basis of the linear portion of the substrate; and correcting the measurement result on the basis of the positional relationship between the substrate and the optical film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for evaluating an optical film. Background Art

[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming popular. In image display devices, optical components such as phase difference components and polarization components are generally used to realize image display and improve image display performance (e.g., refer to Patent Document 1).

[0003] In recent years, new uses of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. With the expansion of the use of image display devices, it is desirable for the optical film including the above-mentioned optical member to have a shape corresponding to the use.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-103286 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, depending on the shape, it may be difficult to accurately grasp the optical axis of the optical film.

[0009] In view of the above circumstances, a main object of the present invention is to accurately evaluate the optical axis of an optical film.

[0010] Solutions to the problem

[0011] 1. An evaluation method according to an embodiment of the present invention is an evaluation method for an optical film, the method comprising: disposing the optical film on a substrate having a straight portion on the periphery; measuring the optical axis of the optical film with reference to the straight portion of the substrate; and correcting the measurement result based on the positional relationship between the substrate and the optical film.

[0012] 2. In the evaluation method described in 1 above, a first straight line portion along the first direction and a second straight line portion along the second direction may be formed on the periphery of the substrate, and the substrate may have a corner where the first straight line portion and the second straight line portion intersect.

[0013] 3. In the evaluation method described in 1 or 2 above, the substrate may be optically isotropic.

[0014] 4. In any one of the evaluation methods described in 1 to 3 above, the total light transmittance of the substrate may be 85% or more.

[0015] 5. In any one of the evaluation methods 1 to 4 above, the haze of the substrate may be 5% or less.

[0016] 6. In the evaluation method according to any one of 1 to 5 above, the optical film may not have a linear portion on the periphery.

[0017] 7. In the evaluation method according to any one of 1 to 6 above, the optical film may have a positioning portion for the substrate.

[0018] 8. Another embodiment of the measuring device of the present invention is a measuring device for measuring the optical axis of an optical film, and the measuring device comprises: a substrate on which the above-mentioned optical film is configured, and the substrate has a straight portion at the periphery; a sample holding portion, which has a loading surface for loading the above-mentioned substrate, and a limiting surface upright relative to the above-mentioned loading surface; and a measuring portion, which measures the optical axis of the above-mentioned optical film, wherein the above-mentioned measurement is performed in a state where the above-mentioned straight portion of the above-mentioned substrate is in contact with the above-mentioned limiting surface.

[0019] 9. A substrate according to still another embodiment of the present invention is used for measuring an optical axis of an optical film, wherein the optical film is disposed on the substrate, and the substrate has a straight portion on its outer periphery.

[0020] Effects of the Invention

[0021] According to the evaluation method of the embodiment of the present invention, the optical axis of the optical film can be accurately evaluated. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a diagram showing a measurement substrate according to one embodiment of the present invention as viewed from above.

[0023] Figure 2A Observe from above Figure 1 The diagram shows an example of a state in which a measurement substrate is placed on a jig of a measurement device.

[0024] Figure 2B From a horizontal perspective Figure 1 The diagram shows an example of a state in which a measurement substrate is placed on a jig of a measurement device.

[0025] Figure 3 This is a schematic diagram showing a simplified configuration of an example of a display system for VR goggles.

[0026] Figure 4 This is a schematic cross-sectional view showing an example of the details of the optical film.

[0027] Explanation of symbols

[0028] 2 Optical film

[0029] 2a Positioning section

[0030] 4 substrate

[0031] 4a First straight line

[0032] 4b Second straight line

[0033] 4c Corner

[0034] 6. Determination of substrate

[0035] 8 Sample holding fixture

[0036] 8a Loading surface

[0037] 8b Restricted surface

[0038] 10 Display System

[0039] 12 Display components

[0040] 14 Reflective polarizing element

[0041] 16. First lens unit

[0042] 18 Half Mirror

[0043] 20 1st λ / 4 component

[0044] 22 2nd λ / 4 component

[0045] 24 Second lens unit DETAILED DESCRIPTION

[0046] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to these embodiments. In order to explain more clearly, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiments, but this is only an example and does not limit the interpretation of the present invention. In addition, with respect to the drawings, the same symbols are marked for the same or equivalent elements, and repeated descriptions are sometimes omitted.

[0047] (Definition of Terms and Symbols)

[0048] The definitions of terms and symbols in this specification are as follows.

[0049] (1) Refractive index (nx, ny, nz)

[0050] "nx" is the refractive index in the direction where the refractive index in the plane reaches the maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.

[0051] (2) In-plane phase difference (Re)

[0052] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Re(λ) can be calculated by the formula: Re(λ) = (nx-ny)×d.

[0053] (3) Retardation in the thickness direction (Rth)

[0054] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Rth(λ) can be calculated by the formula: Rth(λ) = (nx-nz)×d.

[0055] (4) Nz coefficient

[0056] The Nz coefficient can be calculated by Nz=Rth / Re.

[0057] (5) Angle

[0058] In this specification, when an angle is mentioned, the angle includes both clockwise and counterclockwise angles relative to a reference direction. Therefore, for example, "45°" means ±45°.

[0059] The evaluation method of the optical axis of an optical film according to an embodiment of the present invention comprises: preparing a measurement substrate by configuring an optical film on a substrate having a straight portion on the periphery; measuring the optical axis of the optical film based on the straight portion of the substrate; and correcting the measurement result based on the positional relationship between the substrate and the optical film.

[0060] The optical film as the evaluation object may have an optical axis. Specifically, the optical film includes at least a phase difference component, which may have a slow axis and a fast axis. The phase difference component may have any appropriate in-plane phase difference Re(550). The in-plane phase difference Re(550) of the phase difference component is, for example, 100nm~300nm. For example, in the case where the phase difference component can function as a so-called λ / 4 component, its in-plane phase difference Re(550) is, for example, 100nm~190nm, 110nm~180nm, 130nm~160nm, or 135nm~155nm.

[0061] Typically, the phase difference member may be a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound.

[0062] As the resin contained in the above-mentioned resin film, there can be mentioned: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination. As a method of combination, for example, blending and copolymerization can be mentioned. In the case where the phase difference component shows reverse dispersion wavelength characteristics, a resin film containing polycarbonate resin or polyester carbonate resin (hereinafter, sometimes referred to as polycarbonate resin) can be suitably used.

[0063] As the above-mentioned polycarbonate resin, any appropriate polycarbonate resin can be used. For example, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic dimethanols, di, tri or polyethylene glycols and alkylene glycols or spirodiols. Preferably, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, structural units derived from alicyclic dimethanols and / or structural units derived from di, tri or polyethylene glycols; more preferably, it contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from di, tri or polyethylene glycols. The polycarbonate resin may also contain structural units derived from other dihydroxy compounds as needed. It should be noted that the details of the polycarbonate resin that can be suitably used for the phase difference component and the method for forming the phase difference component are described in, for example, Japanese Patent Publication No. 2014-10291, Japanese Patent Publication No. 2014-26266, Japanese Patent Publication No. 2015-212816, Japanese Patent Publication No. 2015-212817, and Japanese Patent Publication No. 2015-212818, and the descriptions of these publications are incorporated into this specification as a reference.

[0064] The thickness of the phase difference member composed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.

[0065] The orientation solidification layer of the above-mentioned liquid crystal compound is a layer in which the liquid crystal compound is oriented in a given direction within the layer and its orientation state is fixed. It should be noted that the "orientation solidification layer" is a concept including an orientation solidification layer obtained by solidifying the liquid crystal monomer as described later. In the phase difference component, representatively, the rod-shaped liquid crystal compound is oriented (parallel orientation (homogeneous alignment)) in a state of being arranged along the slow axis direction of the phase difference component. As rod-shaped liquid crystal compounds, for example, liquid crystal polymers and liquid crystal monomers can be cited. The liquid crystal compound is preferably capable of polymerization. If the liquid crystal compound is capable of polymerization, the orientation state of the liquid crystal compound can be fixed by polymerizing after orienting the liquid crystal compound.

[0066] The orientation solidification layer (liquid crystal orientation solidification layer) of the above-mentioned liquid crystal compound can be formed by the following method: an orientation treatment is applied to the surface of a given substrate, a coating liquid containing a liquid crystal compound is applied to the surface, and the liquid crystal compound is oriented along the direction corresponding to the above-mentioned orientation treatment to fix the orientation state. As an orientation treatment, any appropriate orientation treatment can be adopted. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be cited. As a specific example of mechanical orientation treatment, friction treatment and stretching treatment can be cited. As a specific example of physical orientation treatment, magnetic field orientation treatment and electric field orientation treatment can be cited. As a specific example of chemical orientation treatment, inclined evaporation method and optical orientation treatment can be cited. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.

[0067] The liquid crystal compound can be aligned by treating it at a temperature corresponding to the type of the liquid crystal compound at which it exhibits a liquid crystal phase. By such a temperature treatment, the liquid crystal compound is in a liquid crystal state and is aligned in the alignment treatment direction of the substrate surface.

[0068] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state can be fixed by subjecting the aligned liquid crystal compound to polymerization or crosslinking treatment as described above.

[0069] As the above-mentioned liquid crystal compound, any appropriate liquid crystal polymer and / or liquid crystal monomer can be used. Liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for making liquid crystal alignment solidification layers are described in, for example, Japanese Patent Publication No. 2006-163343, Japanese Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. The records of these publications are cited as references in this specification.

[0070] The thickness of the phase difference member composed of the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.

[0071] Figure 1 This is a diagram of a measurement substrate of an embodiment of the present invention observed from above. The measurement substrate 6 has a substrate 4 and an optical film 2 arranged on the substrate 4. The substrate 4 has a given thickness (for example, 0.5 mm to 10 mm), and the two main surfaces facing each other are horizontal. The substrate 4 has a top view straight line portion on the periphery. The substrate 4 has a first straight line portion 4a extending along the first direction and a second straight line portion 4b extending along the second direction on the periphery. In addition, the substrate 4 has a corner 4c where the first straight line portion 4a and the second straight line portion 4b intersect. The first direction of the substrate 4 is approximately orthogonal to the second direction, and its top view shape is set to be approximately rectangular, but the top view shape of the substrate is not particularly limited as long as a straight line portion is formed on at least a portion of the periphery. For example, it means that the ratio of the length of the longest straight line portion to the total length of the periphery exceeds 0.1.

[0072] The substrate used for the above-mentioned measurement substrate is preferably optically isotropic. By using an optically isotropic substrate, the influence on the evaluation of the optical axis of the optical film can be suppressed. In this specification, "optically isotropic" means that the in-plane phase difference Re(590) is 0nm~10nm. The in-plane phase difference Re(590) of the substrate used for the above-mentioned measurement substrate is more preferably less than 1nm, further preferably less than 0.1nm, particularly preferably less than 0.05nm, and most preferably less than 0.01nm. The phase difference Rth(590) in the thickness direction of the substrate used for the above-mentioned measurement substrate is preferably -10nm~+10nm.

[0073] The total light transmittance of the substrate is preferably 85% or more, more preferably 88% or more, and further preferably 90% or more. The haze of the substrate is preferably 5% or less, more preferably 3% or less, and further preferably 1% or less. By using such a substrate, the influence caused by the evaluation of the optical axis of the optical film can be suppressed. As the substrate, for example, a glass substrate can be preferably used.

[0074] The optical film 2 has no straight line portion on the periphery. In this specification, "no straight line portion on the periphery" means that the ratio of the length of the longest straight line portion to the total length of the periphery is less than 0.1. In the example shown in the figure, the optical film is set to be roughly elliptical, but it is not limited to this and can also be, for example, roughly circular.

[0075] Although not shown, the optical film 2 may be disposed on the substrate 4 via any appropriate layer. For example, the optical film 2 is preferably adhered to the substrate 4 via an adhesive layer such as an adhesive layer or a pressure-sensitive adhesive layer.

[0076] The optical axis of the optical film is measured using the above-mentioned measurement substrate. Any appropriate device can be used as a measuring device for the optical axis. Examples of the measuring device for the optical axis include KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd.

[0077] Typically, when measuring the optical axis, the measurement substrate is placed on a jig of a measurement device. Figure 2A Observe from above Figure 1 FIG. 1 is a diagram showing an example of a state in which a measurement substrate is placed on a fixture of a measurement device, Figure 2B From a horizontal perspective Figure 1 FIG. 1 is a diagram showing an example of a state in which a measurement substrate is placed on a fixture of a measurement device. The sample holding fixture 8 of the measurement device has a placing surface 8a formed by a horizontal plane, and a limiting surface 8b upright relative to the placing surface 8a. The measurement substrate 6 (substrate 4) is placed on the placing surface 8a in a state in which the first straight portion 4a is butted against the limiting surface 8b of the sample holding fixture 8. The substrate 4 has an end surface 41 including the first straight portion 4a, and the end surface 41 is butted against the limiting surface 8b. By using the substrate 4 to evaluate the optical axis of the optical film 2, the evaluation accuracy can be significantly improved compared to the case in which the substrate 4 is not used. By butting the first straight portion 4a forming the corner 4c against the limiting surface 8b, the evaluation accuracy can be further improved. It should be noted that, although not shown in the figure, in addition to the limiting surface 8b, a reference portion for mounting the sample holding fixture 8 on the measurement device can also be provided on the sample holding fixture 8.

[0078] The measurement result of the optical axis of the optical film using the measurement substrate is corrected based on the positional relationship between the substrate and the optical film. The positional relationship between the substrate and the optical film can be coordinated (digitized) using, for example, an image measuring machine. As an image measuring machine, for example, the NEXIV series manufactured by Nikon Corporation can be cited.

[0079] The positional relationship between the substrate and the optical film can be determined, for example, by the straight portion of the substrate, the distance from any location of the optical film, or the line connecting any two points, and the angle. The optical film 2 has positioning portions 2a, 2a for positioning the position of the optical film 2 relative to the first straight portion 4a of the substrate 4. In the example shown in the figure, the positioning portion 2a is provided as a cutout portion formed by partially cutting out the periphery when viewed from above, but is not limited thereto. The positioning portion may also be, for example, a protrusion that protrudes partially from the periphery when viewed from above, or a mark provided in the surface of the optical film.

[0080] In addition to the phase difference component, the optical film may also include other components. As specific examples of other components, optical components such as polarization components can be cited. The optical film can be used in any appropriate image display device. The optical film can be used, for example, in VR goggles.

[0081] Figure 3 1 is a schematic diagram showing a simplified structure of an example of a display system of VR goggles, schematically showing the arrangement and shape of each component of the display system. The display system 10 includes a display element 12, a reflective polarization member 14, a first lens portion 16, a half mirror 18, a first λ / 4 member 20, a second λ / 4 member 22, and a second lens portion 24. The reflective polarization member 14 is arranged on the display surface 12a side of the display element 12, i.e., in front, and can reflect light emitted from the display element 12. The first lens portion 16 is arranged on the optical path between the display element 12 and the reflective polarization member 14, and the half mirror 18 is arranged between the display element 12 and the first lens portion 16. The first λ / 4 member 20 is arranged on the optical path between the display element 12 and the half mirror 18, and the second λ / 4 member 22 is arranged on the optical path between the half mirror 18 and the reflective polarization member 14.

[0082] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying an image. Light emitted from the display surface 12a passes through a polarizing element that may be included in the display element 12, for example, and then emitted as first linearly polarized light.

[0083] The first λ / 4 member 20 can convert the first linearly polarized light incident on the first λ / 4 member 20 into the first circularly polarized light. The first λ / 4 member 20 can be provided integrally with the display element 12.

[0084] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarization member 14 toward the reflective polarization member 14. The half mirror 18 is integrally provided with the first lens portion 16.

[0085] The second λ / 4 member 22 can allow the light reflected by the reflective polarization member 14 and the half mirror 18 to pass through the reflective polarization member 14. The second λ / 4 member 22 can be provided integrally with the first lens portion 16.

[0086] The first circularly polarized light emitted from the first λ / 4 member 20 passes through the half mirror 18 and the first lens portion 16, and is converted into the second linearly polarized light by the second λ / 4 member 22. The second linearly polarized light emitted from the second λ / 4 member 22 does not pass through the reflective polarization member 14, but is reflected toward the half mirror 18. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarization member 14 is the same direction as the reflection axis of the reflective polarization member 14. Therefore, the second linearly polarized light incident on the reflective polarization member 14 is reflected by the reflective polarization member 14.

[0087] The second linear polarized light reflected by the reflective polarization member 14 is converted into the second circular polarized light by the second λ / 4 member 22, and the second circular polarized light emitted from the second λ / 4 member 22 is reflected by the half mirror 18 after passing through the first lens portion 16. The second circular polarized light reflected by the half mirror 18 passes through the first lens portion 16, and is converted into the third linear polarized light by the second λ / 4 member 22. The third linear polarized light is transmitted through the reflective polarization member 14. At this time, the polarization direction of the third linear polarized light incident on the reflective polarization member 14 is the same direction as the transmission axis of the reflective polarization member 14. Therefore, the third linear polarized light incident on the reflective polarization member 14 is transmitted through the reflective polarization member 14.

[0088] The light transmitted through the reflective polarization element 14 passes through the second lens portion 24 and enters the eye 26 of the user.

[0089] The absorption axis of the polarization component included in the display element 12 and the reflection axis of the reflective polarization component 14 may be arranged substantially parallel to each other, or substantially orthogonal to each other. The angle formed by the absorption axis of the polarization component included in the display element 12 and the slow axis of the first λ / 4 component 20 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The angle formed by the absorption axis of the polarization component included in the display element 12 and the slow axis of the second λ / 4 component 22 is, for example, 40° to 50°, 42° to 48°, or approximately 45°.

[0090] The in-plane phase difference Re(550) of the first λ / 4 member 20 is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 member 20 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) of the first λ / 4 member 20 is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.

[0091] The in-plane phase difference Re(550) of the second λ / 4 component 22 is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 component 22 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) of the second λ / 4 component 22 is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.

[0092] Although not shown, the display system 10 may include an absorptive polarization element disposed in front of the reflective polarization element 14. The reflection axis of the reflective polarization element and the absorption axis of the absorptive polarization element may be disposed substantially parallel to each other.

[0093] The above-mentioned optical film may, for example, include components provided in the above-mentioned display system. Specifically, the optical film may include phase difference components such as a λ / 4 component. In addition, the optical film may include polarization components such as a reflective polarization component and an absorptive polarization component. In addition, the optical film may include other components such as a protective component and an adhesive layer for integrating adjacent components. The thickness of the optical film varies, for example, depending on the type and number of components included, and is, for example, 50μm to 400μm. The optical film applied to the above-mentioned display system may have a shape corresponding to the shape of the first lens portion or the second lens portion. For example, it may be designed to be a shape that does not have a straight line portion on the periphery, such as a roughly circular shape or a roughly elliptical shape. In this case, the optical film may be integrally provided on the first lens portion or the second lens portion.

[0094] Figure 4 The optical film 2 includes a second λ / 4 member 22 which may correspond to the above-mentioned phase difference member, another phase difference member 28 disposed on one side of the second λ / 4 member 22 , and a protective member 30 disposed on the other side of the second λ / 4 member 22 .

[0095] The refractive index characteristics of the second λ / 4 component 22 preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, in a range that does not impair the effect of the present invention, ny<nz may be possible. The Nz coefficient of the second λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0096] Another phase difference component 28 can use, for example, a component whose refractive index characteristics can show the relationship of nz>nx=ny (so-called positive C plate). The phase difference Rth(550) in the thickness direction of the positive C plate is preferably -50nm~-300nm, more preferably -70nm~-250nm, further preferably -90nm~-200nm, and particularly preferably -100nm~-180nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the positive C plate is, for example, less than 10nm.

[0097] The positive C plate can be formed of any appropriate material, but the positive C plate is preferably composed of a film containing a liquid crystal material solidified in a homeotropic orientation. The liquid crystal material (liquid crystal compound) capable of homeotropic orientation can be a liquid crystal monomer or a liquid crystal polymer. As a specific example of such a liquid crystal compound and a method for forming a positive C plate, there can be cited the liquid crystal compound and the method for forming the phase difference layer described in

[0020] to

[0028] of Japanese Patent Gazette No. 2002-333642. In this case, the thickness of the positive C plate is preferably 0.5 μm to 5 μm.

[0098] Typically, the protective member 30 includes a substrate. The substrate may be composed of any appropriate film. As the material that is the main component of the film constituting the substrate, for example, cellulose resins such as triacetyl cellulose (TAC), polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, cycloolefins such as polynorbornene, polyolefins, (meth) acrylic acid, acetate resins, etc. can be cited. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 15 μm to 35 μm.

[0099] The protective member 30 preferably may have a surface treatment layer formed on the substrate in addition to the substrate. The protective member having the surface treatment layer may be arranged in such a manner that the substrate is located on the second λ / 4 member 22 side. The surface treatment layer may have any appropriate function. The surface treatment layer preferably has, for example, an anti-reflection function. The thickness of the surface treatment layer is preferably 1 μm to 20 μm, more preferably 2 μm to 15 μm, and further preferably 3 μm to 10 μm.

[0100] Although not shown, the components included in the optical film 2 are preferably integrated via an adhesive layer. In addition, the optical film 2 can be integrally provided on the first lens portion of the above-mentioned display system through an adhesive layer (for example, an adhesive layer) not shown. Specifically, an adhesive layer can be provided on the surface of another phase difference component 28, and the optical film 2 can be attached to the first lens portion through the adhesive layer. The adhesive layer can be formed by an adhesive or an adhesive. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm, preferably 3 μm to 20 μm, and more preferably 5 μm to 15 μm.

[0101] Example

[0102] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. It should be noted that the thickness, phase difference value, transmittance and haze are values ​​measured by the following measurement methods.

[0103] <Thickness>

[0104] The thickness of 1 μm or less was measured using a scanning electron microscope (manufactured by JEOL Ltd., product name “JSM-7100F”). The thickness exceeding 1 μm was measured using a digital micrometer (manufactured by Anritsu Co., Ltd., product name “KC-351C”).

[0105] <Phase difference value>

[0106] The measurement was performed using KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd. The measurement wavelengths were 450 nm, 550 nm, and 590 nm, and the measurement temperature was 23°C.

[0107] <Total light transmittance>

[0108] The measurement was performed using MDH-4000 manufactured by Nippon Denshoku Co., Ltd. in accordance with JIS K 7361.

[0109] <Haze>

[0110] The measurement was performed in accordance with JIS 7136 using a haze meter (manufactured by Murakami Color Science Laboratory Co., Ltd., product name: "HN-150").

[0111] [Example 1]

[0112] A glass substrate having a thickness of 1.3 mm and a size of 65 mm×165 mm was prepared, and the in-plane retardation Re (590) of the glass substrate was 0 nm, the total light transmittance was 92.26%, and the haze was 0.16%.

[0113] (Fabrication of λ / 4 member)

[0114] The polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10-6 parts by mass of calcium acetate monohydrate as a catalyst were added. -2 Mass parts (6.78×10 -5mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. The internal temperature reached 220°C 40 minutes after the start of the temperature rise, and the pressure was reduced while controlling to maintain the temperature, so that it reached 13.3kPa after 90 minutes after reaching 220°C. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux condenser, so that a certain amount of monomer components contained in the phenol vapor was returned to the reactor, and the uncondensed phenol vapor was introduced into a 45°C condenser for recovery. After nitrogen was introduced into the first reactor to temporarily restore it to atmospheric pressure, the reaction liquid after oligomerization in the first reactor was transferred to the second reactor. Next, the temperature rise and pressure reduction in the second reactor were started, so that it reached an internal temperature of 240°C and a pressure of 0.2kPa after 50 minutes. Then, the polymerization was carried out until the given stirring power was reached. When the predetermined power was reached, nitrogen gas was introduced into the reactor to restore the pressure, and the produced polyester carbonate resin was extruded into water, and the strands were cut to obtain pellets.

[0115] After the obtained polyester carbonate resin (pellets) was vacuum dried at 80°C for 5 hours, a long strip of resin film with a thickness of 135 μm was produced using a film-making device equipped with a single screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chilled roll (setting temperature: 120~130°C) and a winder. The obtained long strip of resin film was stretched in the width direction at a stretching temperature of 143°C and a stretching ratio of 2.8 times to obtain a stretched film with a thickness of 47 μm. The Re (590) of the obtained stretched film was 145 nm, the Re (450) / Re (550) was 0.86, and the Nz coefficient was 1.12. In addition, the total light transmittance of the stretched film was 96.81% and the haze was 0.48%.

[0116] (Formation of positive C plate)

[0117] A liquid crystal coating liquid was prepared by dissolving 20 parts by weight of a side chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula represent the molar % of the monomer unit, and for convenience, the block polymer is represented: the weight average molecular weight is 5000), 80 parts by weight of a polymerizable liquid crystal showing a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Chiba Specialty Chemicals: trade name IRGACURE 907) in 200 parts by weight of cyclopentanone. Then, the coating liquid was applied to a PET substrate subjected to a vertical alignment treatment using a wire bar coater, and then heated and dried at 80°C for 4 minutes to align the liquid crystal. The liquid crystal layer was irradiated with ultraviolet rays to cure the liquid crystal layer, thereby forming a positive C plate with a thickness of 4 μm and an Rth (550) of -100 nm on the substrate.

[0118] [Chemical formula 1]

[0119]

[0120] (Production of protective components)

[0121] The antireflection layer forming material shown below was applied to an acrylic film having a lactone ring structure, heated at 80°C for 1 minute, and irradiated the heated coating layer with a high pressure mercury lamp at a cumulative light intensity of 300 mJ / cm 2 The coating layer was cured by ultraviolet rays to obtain an acrylic film (thickness 44 μm) having an antireflection layer with a thickness of 0.1 μm.

[0122] (Anti-reflection layer forming material)

[0123] 100 parts by weight of a multifunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name “Viscoat #300”, solid content 100% by weight), 150 parts by weight of hollow nano-silica particles (manufactured by JGC Catalysts & Chemicals Co., Ltd., trade name “THRULYA 5320”, solid content 20% by weight, weight average particle size 75 nm), 50 parts by weight of solid nano-silica particles (manufactured by Nissan Chemical Industries, Ltd., trade name “MEK-2140Z-AC”, solid content 30% by weight, weight average particle size 10 nm), 12 parts by weight of an additive containing a fluorine element (manufactured by Shin-Etsu Chemical Co., Ltd., trade name “KY-1203”, solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name “OMNIRAD 907”, solid content 100% by weight) were mixed. A mixed solvent of TBA (tert-butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 was added to the mixture as a diluent so that the overall solid content reached 4 weight %, and the mixture was stirred to prepare a coating liquid for forming an antireflection layer.

[0124] (Optical Film)

[0125] The positive C plate was bonded to the λ / 4 member (stretched film) via an ultraviolet curable adhesive (1 μm thickness after curing). Next, the protective member was bonded to the λ / 4 member via the 5 μm thick adhesive layer to obtain a laminate.

[0126] 32 sheets of the laminated body were punched out. Figure 1 The elliptical optical film shown is punched out so that the slow axis direction of the λ / 4 member determined in advance is in a direction of 45° with respect to the short side direction of the obtained optical film.

[0127] (Measurement of shaft angle)

[0128] The obtained optical film was placed on the above-mentioned glass substrate to obtain a measurement substrate. Specifically, the optical film was bonded to the glass substrate via a 12 μm-thick pressure-sensitive adhesive layer to obtain a measurement substrate.

[0129] The obtained measurement substrate was placed on the sample holding fixture of the phase difference measuring device (manufactured by Oji Instruments Co., Ltd., product name "KOBRA-WPR"). Specifically, as shown in FIG2 , the straight portion of the measurement substrate was brought into contact with the limiting surface of the sample holding fixture. Then, under the conditions of a measurement wavelength of 590 nm, a measurement temperature of 23°C ± 2°C, and a measurement humidity of 60% ± 2%, the slow axis direction of the optical film was measured. Specifically, the axial angle formed by the slow axis direction of the optical film relative to the limiting surface of the sample holding fixture was measured.

[0130] (Correction)

[0131] The axis angle obtained by the above measurement was corrected, and the slow axis of the optical film was evaluated. Specifically, the position of the optical film in the measurement substrate relative to the upper side of the glass substrate was coordinateized, the offset of the bonding was calculated, and the axis angle obtained by the above measurement was corrected using the calculated offset. The coordinateization of the glass substrate and the optical film position was performed using an image measuring machine (Nikon Corporation, "NEXIV VMZ-R6555").

[0132] [Comparative Example 1]

[0133] The slow axis of the optical film was evaluated in the same manner as in Example 1 except for the following points.

[0134] In the measurement of the axis angle, the optical film was directly placed on the sample holding jig without using a glass substrate. Specifically, the elliptical optical film was butted so that the short side direction of the film was perpendicular to the limiting surface of the sample holding jig.

[0135] ·Axis angle correction is not performed.

[0136] The standard deviation (degree of deviation) of the evaluation results of Example 1 and the measurement results of Comparative Example 1 are shown below. In Comparative Example 1, it is believed that the optical film is easily offset when placed on the fixture, resulting in deviation in the measured value. On the other hand, in Example 1, the above-mentioned offset is not easy to occur by using a glass substrate, and since correction is performed, the deviation of the evaluation value is very low.

[0137]

[0138] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the above-described embodiments may be replaced with substantially the same configuration, a configuration that exhibits the same effects, or a configuration that achieves the same purpose.

[0139] Industrial Applicability

[0140] The evaluation method according to the embodiment of the present invention can be suitably used for evaluating the optical axis of an optical film.

Claims

1. A method for evaluating an optical film, the method comprising: Arranging the optical film on a substrate having a linear portion on the outer periphery; measuring the optical axis of the optical film with reference to the straight portion of the substrate; as well as The measurement result is corrected based on the positional relationship between the substrate and the optical film.

2. The evaluation method according to claim 1, wherein: A first straight line portion extending along a first direction and a second straight line portion extending along a second direction are formed on an outer periphery of the substrate, and the substrate has a corner portion where the first straight line portion and the second straight line portion intersect.

3. The evaluation method according to claim 1, wherein: The substrate is optically isotropic.

4. The evaluation method according to claim 1, wherein: The total light transmittance of the substrate is greater than 85%.

5. The evaluation method according to claim 1, wherein: The substrate has a haze of 5% or less.

6. The evaluation method according to claim 1, wherein: The optical film has no straight line portion on the outer periphery.

7. The evaluation method according to claim 1, wherein: The optical film has a positioning portion for the substrate.

8. A measuring device for measuring an optical axis of an optical film, The measuring device comprises: The substrate on which the optical film is disposed has a straight line portion on the periphery; a sample holding portion having a placement surface on which the substrate is placed and a restriction surface standing upright relative to the placement surface; and a measuring unit for measuring the optical axis of the optical film, in, The measurement is performed in a state where the straight portion of the substrate is brought into contact with the restriction surface.

9. A substrate for measuring an optical axis of an optical film, wherein the optical film is arranged on the substrate. in, The substrate has a straight portion on the outer periphery.