Preparation method of tearable quick-drying water-based nail polish

By mixing water-based acrylic emulsion, film-forming agent and other materials in specific proportions, nail polish that is easy to peel and dry is prepared, which solves the problems of difficult cleaning and long drying time of existing nail polish, and achieves quick drying and easy drying. Peel-off properties improve ease of use and application efficiency.

CN118806643APending Publication Date: 2024-10-22JINHUA KEWEISI COSMETICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410857126.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing nail polish is difficult to clean when changing, affects nail health, takes a long time to dry, and is inconvenient to use.

Method used

A method for preparing tearable and quick-drying water-based nail polish is adopted, by mixing water-based acrylic emulsion, film-forming agent, film-forming aid, defoaming agent, matting agent, thickener and pigment in a specific proportion to form an easy-to-tear nail polish. The stretched film shortens the drying time.

Benefits of technology

It realizes the quick drying and easy-to-remove characteristics of nail polish, making it more convenient to use, more convenient to replace, and more efficient in application.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of cosmetics, and discloses a preparation method of tearable quick-drying water-based nail polish which comprises a water-based acrylic emulsion, a film-forming agent, a film-forming aid, a defoaming agent, a delustering agent, a thickening agent and a pigment. The film-forming agent is a final product, namely the film-forming agent, which is obtained by grafting polyurethane with 4-vinylbenzoic acid, then carrying out amidation reaction with chitosan, generating hydrogen bonds from hydroxyl and acrylamide, carrying out addition on double bonds of acrylamide and polyvinyl alcohol, and carrying out ring-opening reaction on polyvinyl alcohol and gamma-(2, 3-epoxypropoxy) propyltrimethoxysilane. Polyurethane, chitosan and polyvinyl alcohol are good film-forming substances, can form a film on the surface of a nail, are easy to tear, and are more convenient to use. And the film-forming auxiliary agent can help the film-forming agent to accelerate film forming, so that the thorough drying time of the nail polish is greatly prolonged. The easy-to-tear adhesive tape has the advantages of better easy-to-tear characteristic, more convenience in use, more convenience in replacement, shorter thorough drying time and higher smearing efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cosmetics, in particular to a method for preparing tearable quick-drying water-based nail polish. Background Art

[0002] Nail polish is a kind of cosmetics used for the application of fingernails and toenails. Nail polish is a must-have cosmetics for contemporary women. Good-looking nail polish can effectively improve the appearance of the hands and has a certain effect on improving the temperament of the whole person. There are various brands of nail polish on the market, black, white, red and various colors, flat and three-dimensional styles, and the nail art industry has gradually become popular. In order to be able to remain on the nails more firmly, many nail polishes have abandoned the feature of being easy to clean. Therefore, when it is necessary to replace the nail polish, a shovel must be used to clean the old nail polish, which is very inconvenient, and nail polish left on the nails for a long time may affect the health of the nails. For some people, nail polish that is easy to clean and tear is more suitable for them and will be widely used in the market. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a tearable quick-drying water-based nail polish.

[0005] (II) Technical solution

[0006] A method for preparing a tearable quick-drying water-based nail polish is as follows:

[0007] Mix 30-70 parts of aqueous acrylic emulsion, 10-30 parts of film former, 3-8 parts of film-forming aid, and 10-30 parts of water, stir evenly, add 0.1-3 parts of defoamer, 0.1-3 parts of matting agent, and 2-5 parts of thickener, stir continuously, add 3-15 parts of pigment under stirring, stir evenly to obtain nail polish;

[0008] The preparation method of the film-forming agent is as follows:

[0009] (1) Mix polyether diol and toluene diisocyanate, stir evenly, heat to 80-95° C., and keep warm for 2-6 hours; cool to 60-70° C., add dimethylolpropionic acid, diethylene glycol, and hydroxypropyl methacrylate, and keep warm for 2-6 hours; cool to below 40° C., add acetone and triethylamine, and disperse in water under vigorous stirring to obtain a polyurethane seed emulsion; add 4-vinylbenzoic acid and initiator potassium persulfate dropwise at 60-80° C., and keep warm for 2-6 hours at 80-90° C. to obtain intermediate 1;

[0010] (2) adding chitosan to a 5-12% by mass acetic acid solution and stirring to prepare a chitosan solution; mixing intermediate 1 and the chitosan solution, stirring to prepare a chitosan solution; adding a catalyst, a strong acid cation exchange resin, heating to reflux, and reacting for 8-16 hours to obtain intermediate 2; adding acrylamide to water and stirring to dissolve; heating intermediate 2 to 50-60° C., adding an acrylamide aqueous solution and an initiator, potassium persulfate, heating to 80-90° C. and reacting for 2-6 hours; cooling to room temperature after the reaction to obtain intermediate 3;

[0011] (3) adding polyvinyl alcohol to water, heating to boiling, stirring to dissolve, adding intermediate 3 to polyvinyl alcohol solution, heating to reflux, reacting for 1-3 hours, cooling to room temperature after the reaction, and obtaining intermediate 4; adding γ-(2,3-epoxypropoxy)propyltrimethoxysilane to isopropanol, stirring to dissolve, and then adding it to intermediate 4, stirring and reacting at 50-65° C. for 3-8 hours, distilling off the solvent under reduced pressure, cooling to room temperature, and sealing to obtain a film-forming agent;

[0012] The preparation method of the film-forming aid is as follows:

[0013] Mix phenol and catalyst, pass nitrogen, add propylene oxide, heat to 40-50°C, start stirring, continue heating to 90-130°C, react for 3-8h, cool to room temperature, discharge, distill, collect 242-244°C fraction to obtain film-forming aid.

[0014] Preferably, in step (1) of the method for preparing the film-forming agent, the mass ratio of the polyurethane seed emulsion to 4-vinylbenzoic acid is 1:0.8-2.

[0015] Preferably, in step (2) of the method for preparing the film-forming agent, the mass ratio of the intermediate 1 to chitosan is 1:0.4-1; the mass ratio of the intermediate 2 to acrylamide is 1:0.3-0.8.

[0016] Preferably, in step (3) of the method for preparing the film-forming agent, the mass ratio of the intermediate 3 to polyvinyl alcohol is 1:0.2-0.8; the mass ratio of the intermediate 4 to γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 1:0.2-0.6.

[0017] Preferably, in the preparation method of the film-forming aid, the molar ratio of phenol to propylene oxide is 1:1-1.25.

[0018] Preferably, the defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0019] Preferably, the matting agent is fumed silica or aqueous wax slurry.

[0020] Preferably, the thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0021] Preferably, the pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0022] (III) Beneficial technical effects

[0023] The tearable quick-drying water-based nail polish comprises a water-based acrylic emulsion, a film-forming agent, a film-forming aid, a defoaming agent, a matting agent, a thickener and a pigment.

[0024] The film-forming agent is polyurethane grafted with 4-vinylbenzoic acid, which is then amidated with chitosan, in which the hydroxyl group generates hydrogen bonds with acrylamide, the double bonds of acrylamide and polyvinyl alcohol are added, and polyvinyl alcohol and γ-(2,3-epoxypropoxy)propyltrimethoxysilane undergo a ring-opening reaction to obtain the final product, the film-forming agent. Polyurethane, chitosan, and polyvinyl alcohol are all good film-forming substances that can form a thin film on the surface of the nails, and these materials are easier to tear and more convenient to use. Film-forming aids can help the film-forming agent accelerate film formation and greatly increase the drying time of nail polish.

[0025] The invention has good tearing characteristics, is more convenient to use, is more convenient to replace, has a faster drying time, and has a higher application efficiency. DETAILED DESCRIPTION

[0026] Example 1

[0027] Mix 30 parts of aqueous acrylic emulsion, 10 parts of film former, 3 parts of film-forming aid and 10 parts of water, stir evenly, add 0.1 parts of defoamer, 0.1 parts of matting agent and 2 parts of thickener, stir continuously, add 3 parts of pigment while stirring, stir evenly to obtain nail polish.

[0028] The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0029] The matting agent is fumed silica or aqueous wax slurry.

[0030] The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0031] The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0032] The preparation method of the film-forming agent is as follows:

[0033] (1) 80 mL of polyether diol and 60 mL of toluene diisocyanate were mixed, stirred evenly, heated to 80°C, and kept warm for 2 h; cooled to 60°C, 20 mL of dihydroxymethylpropionic acid, 20 mL of diethylene glycol, and 30 mL of hydroxypropyl methacrylate were added, and the mixture was kept warm for 2 h; cooled to below 40°C, 40 mL of acetone and 30 mL of triethylamine were added, and water was added and dispersed under vigorous stirring to obtain a polyurethane seed emulsion; 200 mL of 4-vinylbenzoic acid and 1 g of initiator potassium persulfate were added dropwise at 60°C, and the mixture was kept warm for 2 h at 80°C to obtain intermediate 1.

[0034] (2) Add 150 g of chitosan to 500 mL of 5% glacial acetic acid solution and stir to prepare a chitosan solution; mix the intermediate 1 and the chitosan solution, stir to prepare a chitosan solution; add a strong acid cation exchange resin as a catalyst, heat to reflux, and react for 8 h to obtain an intermediate 2; add 150 g of acrylamide to 300 mL of water and stir to dissolve; heat the intermediate 2 to 50°C, add an acrylamide aqueous solution and 10 g of an initiator potassium persulfate, heat to 80°C and react for 1 h; after the reaction is completed, cool to room temperature to obtain an intermediate 3.

[0035] (3) Add 200 g of polyvinyl alcohol to 500 mL of water, heat to boiling, stir to dissolve, add intermediate 3 to the polyvinyl alcohol solution, heat to reflux, react for 1 hour, cool to room temperature after the reaction, and obtain intermediate 4; add 200 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to 500 mL of isopropanol, stir to dissolve, and then add it to intermediate 4, stir and react at 50° C. for 3 hours, remove the solvent by vacuum distillation, cool to room temperature, and seal to obtain a film-forming agent.

[0036] The preparation method of the film-forming aid is as follows:

[0037] Mix 100g of phenol and 0.2g of catalyst sodium hydroxide, pass nitrogen, add 120mL of propylene oxide, heat to 40°C, start stirring, continue heating to 90°C, react for 3h, cool to room temperature, discharge, distill, collect 242-244°C fraction, and obtain a film-forming aid.

[0038] Example 2

[0039] Mix 70 parts of aqueous acrylic emulsion, 30 parts of film former, 8 parts of film-forming aid and 30 parts of water, stir evenly, add 3 parts of defoamer, 3 parts of matting agent and 5 parts of thickener, stir continuously, add 15 parts of pigment while stirring, stir evenly to obtain nail polish.

[0040] The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0041] The matting agent is fumed silica or aqueous wax slurry.

[0042] The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0043] The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0044] The preparation method of the film-forming agent is as follows:

[0045] (1) 300 mL of polyether diol and 180 mL of toluene diisocyanate were mixed, stirred evenly, heated to 95° C., and kept warm for 6 h; cooled to 70° C., 60 mL of dimethylolpropionic acid, 40 mL of diethylene glycol, and 60 mL of hydroxypropyl methacrylate were added, and the mixture was kept warm for 6 h; cooled to below 40° C., 80 mL of acetone and 60 mL of triethylamine were added, and water was added and dispersed under vigorous stirring to obtain a polyurethane seed emulsion; 1200 mL of 4-vinylbenzoic acid and 5 g of initiator potassium persulfate were added dropwise at 80° C., and the mixture was kept warm for 6 h at 90° C. to obtain intermediate 1.

[0046] (2) Add 2000 g of chitosan to 5000 mL of 12% glacial acetic acid solution and stir well to prepare a chitosan solution; mix the intermediate 1 and the chitosan solution, stir well, add a catalyst strong acid cation exchange resin, heat to reflux, and react for 16 hours to obtain the intermediate 2; add 3000 g of acrylamide to 8000 mL of water and stir to dissolve, heat the intermediate 2 to 60°C, add the acrylamide aqueous solution and 30 g of initiator potassium persulfate, heat to 90°C to react for 6 hours, and cool to room temperature after the reaction to obtain the intermediate 3.

[0047] (3) Add 5000g of polyvinyl alcohol to 10000mL of water, heat to boiling, stir to dissolve, add intermediate 3 to the polyvinyl alcohol solution, heat to reflux, react for 3h, cool to room temperature after the reaction, and obtain intermediate 4; add 5000g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to 10000mL of isopropanol, stir to dissolve, then add it to intermediate 4, stir and react at 65°C for 8h, remove the solvent by vacuum distillation, cool to room temperature and seal to obtain a film-forming agent.

[0048] The preparation method of the film-forming aid is as follows:

[0049] Mix 500g of phenol and 7g of catalyst sodium hydroxide, pass nitrogen, add 600mL of propylene oxide, heat to 50°C, start stirring, continue heating to 130°C, react for 8h, cool to room temperature, discharge, distill, collect 242-244°C fraction, and obtain a film-forming aid.

[0050] Example 3

[0051] Mix 40 parts of aqueous acrylic emulsion, 15 parts of film former, 4 parts of film-forming aid and 12 parts of water, stir evenly, add 1 part of defoamer, 1 part of matting agent and 3 parts of thickener, stir continuously, add 5 parts of pigment while stirring, stir evenly to obtain nail polish.

[0052] The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0053] The matting agent is fumed silica or aqueous wax slurry.

[0054] The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0055] The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0056] The preparation method of the film-forming agent is as follows:

[0057] (1) 100 mL of polyether diol and 100 mL of toluene diisocyanate were mixed, stirred evenly, heated to 85° C., and kept warm for 3 h; cooled to 62° C., 30 mL of dihydroxymethylpropionic acid, 30 mL of diethylene glycol, and 40 mL of hydroxypropyl methacrylate were added, and the mixture was kept warm for 5 h; cooled to below 40° C., 50 mL of acetone and 40 mL of triethylamine were added, and water was added and dispersed under vigorous stirring to obtain a polyurethane seed emulsion; 500 mL of 4-vinylbenzoic acid and 2 g of initiator potassium persulfate were added dropwise at 65° C., and the mixture was kept warm for 3 h at 82° C. to obtain intermediate 1.

[0058] (2) Add 500 g of chitosan to 1500 mL of 6% glacial acetic acid solution and stir to prepare a chitosan solution; mix the intermediate 1 and the chitosan solution, stir to prepare a chitosan solution; add a catalyst, a strong acid cation exchange resin, heat to reflux, and react for 10 h to obtain an intermediate 2; add 500 g of acrylamide to 2000 mL of water and stir to dissolve; heat the intermediate 2 to 55°C, add an acrylamide aqueous solution and 20 g of an initiator, potassium persulfate, and heat to 85°C to react for 3 h. After the reaction is completed, cool to room temperature to obtain an intermediate 3.

[0059] (3) Add 1000 g of polyvinyl alcohol to 3000 mL of water, heat to boiling, stir to dissolve, add intermediate 3 to the polyvinyl alcohol solution, heat to reflux, react for 2 h, and cool to room temperature after the reaction to obtain intermediate 4; add 1000 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to 5000 mL of isopropanol, stir to dissolve, and then add it to intermediate 4, stir and react at 52° C. for 5 h, remove the solvent by vacuum distillation, cool to room temperature, and seal to obtain a film-forming agent.

[0060] The preparation method of the film-forming aid is as follows:

[0061] Mix 200g of phenol and 2g of catalyst sodium hydroxide, pass nitrogen, add 300mL of propylene oxide, heat to 42°C, start stirring, continue heating to 100°C, react for 5h, cool to room temperature, discharge, distill, collect 242-244°C fraction, and obtain a film-forming aid.

[0062] Example 4

[0063] Mix 50 parts of aqueous acrylic emulsion, 20 parts of film former, 5 parts of film-forming aid and 20 parts of water, stir evenly, add 2 parts of defoamer, 2 parts of matting agent and 4 parts of thickener, stir continuously, add 8 parts of pigment while stirring, stir evenly to obtain nail polish.

[0064] The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0065] The matting agent is fumed silica or aqueous wax slurry.

[0066] The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0067] The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0068] The preparation method of the film-forming agent is as follows:

[0069] (1) 200 mL of polyether diol and 150 mL of toluene diisocyanate were mixed, stirred evenly, heated to 90°C, and kept warm for 5 h; cooled to 65°C, 40 mL of dihydroxymethylpropionic acid, 28 mL of diethylene glycol, and 50 mL of hydroxypropyl methacrylate were added, and the mixture was kept warm for 4 h; cooled to below 40°C, 60 mL of acetone and 50 mL of triethylamine were added, and water was added and dispersed under vigorous stirring to obtain a polyurethane seed emulsion; 800 mL of 4-vinylbenzoic acid and 2 g of initiator potassium persulfate were added dropwise at 72°C, and the mixture was kept warm for 4 h at 85°C to obtain intermediate 1.

[0070] (2) Add 800 g of chitosan to 2000 mL of 10% glacial acetic acid solution and stir to prepare chitosan solution; mix intermediate 1 and chitosan solution, stir to prepare, add catalyst strong acid cation exchange resin, heat to reflux, react for 15 h, and obtain intermediate 2; add 1800 g of acrylamide to 5000 mL of water and stir to dissolve, heat intermediate 2 to 58°C, add acrylamide aqueous solution and 25 g of initiator potassium persulfate, heat to 85°C and react for 3 h, and cool to room temperature after the reaction to obtain intermediate 3.

[0071] (3) Add 4000 g of polyvinyl alcohol to 8000 mL of water, heat to boiling, stir to dissolve, add intermediate 3 to the polyvinyl alcohol solution, heat to reflux, react for 1 hour, cool to room temperature after the reaction, and obtain intermediate 4; add 3000 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to 6000 mL of isopropanol, stir to dissolve, and then add it to intermediate 4, stir and react at 60° C. for 6 hours, remove the solvent by vacuum distillation, cool to room temperature, and seal to obtain a film-forming agent.

[0072] The preparation method of the film-forming aid is as follows:

[0073] Mix 300g of phenol and 5g of catalyst sodium hydroxide, pass nitrogen, add 300mL of propylene oxide, heat to 45°C, start stirring, continue heating to 110°C, react for 5h, cool to room temperature, discharge, distill, collect 242-244°C fraction, and obtain a film-forming aid.

[0074] Example 5

[0075] Mix 60 parts of aqueous acrylic emulsion, 25 parts of film former, 6 parts of film-forming aid and 25 parts of water, stir evenly, add 2.5 parts of defoamer, 2.5 parts of matting agent and 4 parts of thickener, stir continuously, add 12 parts of pigment while stirring, stir evenly to obtain nail polish.

[0076] The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

[0077] The matting agent is fumed silica or aqueous wax slurry.

[0078] The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

[0079] The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.

[0080] The preparation method of the film-forming agent is as follows:

[0081] (1) 250 mL of polyether diol and 160 mL of toluene diisocyanate were mixed, stirred evenly, heated to 92° C., and kept warm for 3 h; cooled to 68° C., 50 mL of dihydroxymethylpropionic acid, 35 mL of diethylene glycol, and 50 mL of hydroxypropyl methacrylate were added, and the mixture was kept warm for 5 h; cooled to below 40° C., 70 mL of acetone and 50 mL of triethylamine were added, and water was added and dispersed under vigorous stirring to obtain a polyurethane seed emulsion; 1000 mL of 4-vinylbenzoic acid and 4 g of initiator potassium persulfate were added dropwise at 75° C., and the mixture was kept warm for 5 h at 88° C. to obtain intermediate 1.

[0082] (2) Add 1800 g of chitosan to 4500 mL of 10% glacial acetic acid solution and stir to prepare chitosan solution; mix intermediate 1 and chitosan solution, stir to prepare, add catalyst strong acid cation exchange resin, heat to reflux, react for 15 h, and obtain intermediate 2; add 2000 g of acrylamide to 6000 mL of water and stir to dissolve, heat intermediate 2 to 60°C, add acrylamide aqueous solution and 25 g of initiator potassium persulfate, heat to 90°C and react for 5 h, and cool to room temperature after the reaction to obtain intermediate 3.

[0083] (3) Add 4000 g of polyvinyl alcohol to 9000 mL of water, heat to boiling, stir to dissolve, add intermediate 3 to the polyvinyl alcohol solution, heat to reflux, react for 3 hours, cool to room temperature after the reaction, and obtain intermediate 4; add 4000 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to 8000 mL of isopropanol, stir to dissolve, then add it to intermediate 4, stir and react at 62° C. for 5 hours, remove the solvent by vacuum distillation, cool to room temperature, and seal to obtain a film-forming agent.

[0084] The preparation method of the film-forming aid is as follows:

[0085] Mix 450g of phenol and 6g of catalyst sodium hydroxide, pass nitrogen, add 500mL of propylene oxide, heat to 48°C, start stirring, continue heating to 120°C, react for 6h, cool to room temperature, discharge, distill, collect 242-244°C fraction, and obtain a film-forming aid.

[0086] Comparative Example 1: Commercially available nail polish.

[0087] Test Example: The nail polishes of Examples 1-5 and Comparative Example 1 were applied on nails to test the drying time and ease of tearing of the nail polishes.

[0088] Table 1 Test results

[0089] Group Drying time (min) Tearing Example 1 3 Easy to tear Example 2 2.5 Easy to tear Example 3 2.5 Easy to tear Example 4 2 Easy to tear Example 5 2.4 Easy to tear Comparative Example 1 4 Hard to tear

[0090] It can be seen from Table 1 that the nail polishes of Examples 1-5 take shorter time to dry than the nail polishes of Comparative Example 1, are easier to tear off after drying, and are more convenient to use.

[0091] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a tearable quick-drying water-based nail polish, characterized in that: The preparation method of the nail polish is as follows: Mix 30-70 parts of aqueous acrylic emulsion, 10-30 parts of film former, 3-8 parts of film-forming aid, and 10-30 parts of water, stir evenly, add 0.1-3 parts of defoamer, 0.1-3 parts of matting agent, and 2-5 parts of thickener, stir continuously, add 3-15 parts of pigment under stirring, stir evenly to obtain nail polish; The preparation method of the film-forming agent is as follows: (1) Mix polyether diol and toluene diisocyanate, stir evenly, heat to 80-95° C., and keep warm for 2-6 hours; cool to 60-70° C., add dimethylolpropionic acid, diethylene glycol, and hydroxypropyl methacrylate, and keep warm for 2-6 hours; cool to below 40° C., add acetone and triethylamine, and disperse in water under vigorous stirring to obtain a polyurethane seed emulsion; add 4-vinylbenzoic acid and initiator potassium persulfate dropwise at 60-80° C., and keep warm for 2-6 hours at 80-90° C. to obtain intermediate 1; (2) adding chitosan to a 5-12% by mass acetic acid solution and stirring to prepare a chitosan solution; mixing intermediate 1 and the chitosan solution, stirring to prepare a chitosan solution; adding a catalyst, a strong acid cation exchange resin, heating to reflux, and reacting for 8-16 hours to obtain intermediate 2; adding acrylamide to water and stirring to dissolve; heating intermediate 2 to 50-60° C., adding an acrylamide aqueous solution and an initiator, potassium persulfate, heating to 80-90° C. and reacting for 2-6 hours; cooling to room temperature after the reaction to obtain intermediate 3; (3) adding polyvinyl alcohol to water, heating to boiling, stirring to dissolve, adding intermediate 3 to polyvinyl alcohol solution, heating to reflux, reacting for 1-3 hours, cooling to room temperature after the reaction, and obtaining intermediate 4; adding γ-(2,3-epoxypropoxy)propyltrimethoxysilane to isopropanol, stirring to dissolve, and then adding it to intermediate 4, stirring and reacting at 50-65° C. for 3-8 hours, distilling off the solvent under reduced pressure, cooling to room temperature, and sealing to obtain a film-forming agent; The preparation method of the film-forming aid is as follows: Mix phenol and catalyst, pass nitrogen, add propylene oxide, heat to 40-50°C, start stirring, continue heating to 90-130°C, react for 3-8h, cool to room temperature, discharge, distill, collect 242-244°C fraction to obtain film-forming aid.

2. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: In the step (1) of the method for preparing the film-forming agent, the mass ratio of the polyurethane seed emulsion to 4-vinylbenzoic acid is 1:0.8-2.

3. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: In the step (2) of the film-forming agent preparation method, the mass ratio of the intermediate 1 to chitosan is 1:0.4-1; the mass ratio of the intermediate 2 to acrylamide is 1:0.3-0.

8.

4. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: In step (3) of the film-forming agent preparation method, the mass ratio of the intermediate 3 to polyvinyl alcohol is 1:0.2-0.8; the mass ratio of the intermediate 4 to γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 1:0.2-0.

6.

5. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: In the preparation method of the film-forming aid, the molar ratio of phenol to propylene oxide is 1:1-1.

25.

6. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: The defoaming agent is DSA-5, BYK028, TWIN4100 or CK-470.

7. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: The matting agent is fumed silica or aqueous wax slurry.

8. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: The thickener is sodium carboxymethyl cellulose, sodium alginate, sodium polyacrylate or polyvinyl pyrrolidone.

9. The method for preparing a tearable quick-drying water-based nail polish according to claim 1, characterized in that: The pigment is titanium white, iron yellow, chromium oxide green, cobalt blue, titanium cobalt green, carbon black or cadmium yellow.