Method for preparing high-performance carbon dioxide adsorbent from desulfurization waste residues and carbide slag

Pre-calcination and sol-gel method are used to prepare high-performance carbon dioxide adsorbent from carbide slag and desulfurization waste residue, which solves the problem of utilization of carbide slag and desulfurization waste residue, achieves efficient utilization of resources and improves the performance of the adsorbent.

CN118807682APending Publication Date: 2024-10-22SHAANXI COAL & CHEM TECH INST +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411123074.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing technology makes it difficult to effectively utilize carbide slag and desulfurization waste residue, resulting in environmental pollution and resource waste, and the quality of calcium-based products is affected by high alkalinity, impurity content and difficult decomposition characteristics.

Method used

Using the pre-calcination and sol-gel method, the mixed powder of carbide slag and desulfurization waste residue is mixed with acetic acid, citric acid and other substances under heating conditions to form a gel. After drying and calcination, a high-performance carbon dioxide adsorbent is prepared.

Benefits of technology

Efficient resource utilization of carbide slag and desulfurization waste residue is achieved, and a carbon dioxide adsorbent with excellent performance is prepared, which has good industrial application value and low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807682A_ABST
    Figure CN118807682A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-performance carbon dioxide adsorbent from desulfurization waste residues and carbide slag, which comprises the following steps: pre-calcining mixed powder of desulfurization waste residues and carbide slag, mixing the pre-calcined powder, water, an acetic acid solution, citric acid and a carbon-containing carrier, heating to form gel, and drying to obtain the high-performance carbon dioxide adsorbent. And drying and calcining to obtain the high-performance carbon dioxide adsorbent. The preparation process is simple, the required reagents are common reagents, the desulfurization waste residues and the carbide slag can be co-processed, efficient recycling of the carbide slag and the desulfurization waste residues is achieved, the performance is excellent, energy consumption is low, and good industrial application value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a high-performance carbon dioxide adsorbent by utilizing desulfurization waste residue and carbide slag, and belongs to the field of solid waste resource utilization. Background Art

[0002] A large amount of carbide slag is produced in the process of obtaining acetylene by hydrolysis of calcium carbide. Specifically, more than one ton of carbide slag is produced for each ton of carbide hydrolysis. If carbide slag is discharged at will without harmless treatment, the harmful substances it contains will cause serious pollution to the soil and groundwater, thereby affecting food safety and posing a threat to environmental safety. Effective treatment and recycling of carbide slag has significant social benefits, which can reduce environmental pollution, save resources, promote green development, reduce energy consumption and pollutant emissions, solve the shortage of high-quality limestone resources, and promote the recycling concept of waste treatment. Carbide slag is a high-quality calcium source with the advantages of small particle size and high reaction activity. It can be used as a raw material to produce cement, building blocks and other building materials or as a material for road construction. At the same time, carbide slag can be used to prepare chemical products such as calcium oxide and calcium carbonate. However, the high alkalinity, high impurity content, high difficulty in decomposition and separation characteristics of carbide slag significantly affect the resource utilization of carbide slag and the quality of calcium-based products prepared by it. Summary of the invention

[0003] In order to overcome the problem that the prior art cannot be applied in the preparation of calcium-based products, the purpose of the present invention is to provide a method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste slag and carbide slag. The method realizes the application of carbide slag in the preparation of high-performance carbon dioxide adsorbent, and the preparation process is simple and can efficiently realize the resource utilization of desulfurization waste slag and carbide slag.

[0004] To achieve this object, the present invention adopts the following technical solutions:

[0005] A method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag comprises the following steps:

[0006] The mixed powder of desulfurization waste residue and carbide slag is pre-calcined, and then the pre-calcined powder, water, acetic acid solution and citric acid are mixed, heated to form a gel, and then dried and calcined to obtain a high-performance carbon dioxide adsorbent.

[0007] Furthermore, the mass ratio of the desulfurization waste residue to the carbide slag is (1-5):10.

[0008] Furthermore, the pre-calcination is carried out in an air atmosphere, the pre-calcination temperature is 1000-1100°C, and the time is 1-4h; the pre-calcination heating rate is 5-10°C / min; and the SO2 gas generated during the pre-calcination process is collected for the preparation of sulfuric acid.

[0009] Furthermore, it also includes a carbon-containing carrier.

[0010] Furthermore, the carbon-containing carrier is one or both of activated carbon and blue charcoal.

[0011] Furthermore, the acetic acid solution is a solution obtained by diluting acetic acid and water in a volume ratio of 1:4 to 1:6; and the mass ratio of the acetic acid solution to the pre-calcined powder is 1.5:1 to 1.8:1.

[0012] Furthermore, the mass ratio of the water to the pre-calcined powder is 7:1 to 9:1; the mass ratio of the carbon-containing carrier to the pre-calcined powder is 1:10 to 1:4.

[0013] Furthermore, the mass ratio of the citric acid to the pre-calcined powder is 0.5:1 to 0.6:1.

[0014] Furthermore, the heating temperature is 80-90° C., and the time is 5-7 hours; the stirring rate is 400 r / min-600 r / min; the drying temperature is 105-130° C., and the drying time is 24 hours-48 hours.

[0015] Furthermore, the calcination is carried out in an air or nitrogen atmosphere; the calcination temperature is 800-900°C, the time is 2-4hh; and the calcination heating rate is 5-10°C / min.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The method described in the present invention uses carbide slag and desulfurization waste residue as raw materials, first pre-calcines them, and then uses a sol-gel method to obtain a carbon dioxide adsorbent, thereby achieving efficient resource utilization of carbide slag and desulfurization waste residue. The method described in the present invention has a simple process, and the required reagents are all common reagents, which can synergistically treat desulfurization waste residue and carbide slag, and has excellent performance, low energy consumption, and good industrial application value.

[0018] Furthermore, the present invention obtains the adsorbent by calcining in air or nitrogen atmosphere, enriching the pores therein and making the various substances evenly distributed, making full use of inert substances such as Al, Si and alkali metal elements such as Fe in carbide slag and desulfurization waste slag to improve the adsorbent's anti-sintering ability and capture performance.

[0019] Furthermore, the acetic acid solution and citric acid are used together to play a dispersing role, thereby improving the dispersion of the active component.

[0020] Furthermore, pre-calcination at 1000-1100°C is performed to remove calcium carbonate produced by long-term storage of carbide slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a flow chart of the preparation method of the present invention;

[0022] Figure 2 is a SEM image of the carbon dioxide adsorbent provided in Example 2 of the present invention;

[0023] Figure 3 is a SEM image of the carbon dioxide adsorbent provided in Example 6 of the present invention;

[0024] Figure 4 It is a SEM picture of the carbon dioxide adsorbent provided in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0025] In order to explain the present invention more clearly and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0026] The following are typical but non-limiting embodiments of the present invention:

[0027] Desulfurization waste residue refers to the solid waste generated by removing sulfur from fuel through desulfurization facilities when burning sulfur-containing fuel. These waste residues usually contain high concentrations of sulfur compounds, such as calcium sulfate and magnesium sulfate, among which calcium and magnesium have high mass fractions, which makes desulfurization waste residue have the potential to be used as a raw material for preparing carbon dioxide adsorbents. Therefore, the comprehensive utilization of carbide slag and desulfurization waste residue, and the research and development of technology for preparing high-performance carbon dioxide adsorbents using desulfurization waste residue and carbide slag, not only opens up a resource utilization path for desulfurization waste residue and carbide slag, but also has important reference significance for the preparation and production of high-performance carbon dioxide adsorbents.

[0028] The present invention provides a method for preparing a high-performance carbon dioxide adsorbent by using desulfurization waste residue and carbide slag, comprising the following steps:

[0029] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder; wherein the mass ratio of the desulfurization waste residue to the carbide slag is (1-5):10;

[0030] (2) pre-calcining the mixed powder of carbide desulfurization slag obtained in step (1) at a temperature of 1000-1100° C. to obtain the pre-calcined mixed powder of carbide desulfurization slag, and collecting the SO2 gas generated during the pre-calcination process for preparing sulfuric acid; the purpose of the pre-calcination is to remove the calcium carbonate generated by the long-term storage of the carbide slag.

[0031] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and activated carbon (and / or blue charcoal), stirred under heating conditions in a water bath to form a gel, and then dried and calcined at a temperature of 800 to 900° C. to obtain the high-performance carbon dioxide adsorbent; wherein the acetic acid solution and citric acid are used in combination to play a dispersing role, thereby improving the dispersion of the active components.

[0032] Wherein, the pre-calcination in step (2) is carried out in an air atmosphere.

[0033] Wherein, the pre-calcination time in step (2) is 1 to 4 hours.

[0034] Wherein, the heating rate of the pre-calcination in step (2) is 5 to 10°C / min.

[0035] Wherein, the acetic acid solution in step (3) is a solution obtained by diluting pure acetic acid and water in a volume ratio of 1:4 to 1:6.

[0036] Wherein, the mass ratio of the water in step (3) to the mixed powder of pre-calcined calcium carbide desulfurization slag is 7:1 to 9:1.

[0037] Wherein, the mass ratio of the acetic acid solution in step (3) to the mixed powder of pre-calcined calcium carbide desulfurization slag is 1.5:1 to 1.8:1.

[0038] Wherein, the mass ratio of the citric acid and the pre-calcined calcium carbide desulfurization slag mixed powder in step (3) is 0.5:1 to 0.6:1.

[0039] Wherein, the mass ratio of the activated carbon and the pre-calcined calcium carbide desulfurization slag mixed powder in step (3) is 1:10 to 1:4.

[0040] Wherein, the heating temperature in step (3) is 80-90° C. and the heating time is 5-7 h;

[0041] Wherein, the stirring rate in step (3) is 400 r / min to 600 r / min.

[0042] Wherein, the drying temperature in step (3) is 105-130° C., and the drying time is 24 h to 48 h.

[0043] Wherein, the calcination in step (3) is carried out in an air or nitrogen atmosphere; the purpose of calcination is to convert the pre-calcined calcium carbide desulfurization slag mixed powder into an effective component that can adsorb CO2.

[0044] Wherein, the calcination time in step (3) is 2 to 4 hours;

[0045] Wherein, the heating rate of the calcination in step (3) is 5 to 10°C / min.

[0046] The preparation process of the invention is simple, the required reagents are common reagents, the desulfurization waste residue and carbide slag can be synergistically disposed, and the efficient resource utilization of carbide slag and desulfurization waste residue is achieved, and the invention has excellent performance, low energy consumption, and good industrial application value.

[0047] Example 1

[0048] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0049] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0050] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0051] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution and citric acid, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, and the citric acid is 2.7g. The heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then it is dried and calcined, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 adsorbent.

[0052] Example 2

[0053] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0054] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0055] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0056] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and activated carbon, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, citric acid is 2.7g, and activated carbon is 0.25g. The heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then it is dried and calcined, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 adsorbent.

[0057] See also Figure 2 It can be seen that the adsorbent particles have more pores and the particles are connected to each other to form a relatively strong structure. There are also long strips of particles, which play a certain supporting role.

[0058] Example 3

[0059] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0060] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0061] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0062] (3) Mix the pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) with water, acetic acid solution, citric acid and blue carbon, and stir under heating conditions to form a gel, wherein the mass of the pre-calcined calcium carbide desulfurization slag mixed powder is 5g, the water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, the citric acid is 2.7g, the blue carbon is 0.25g, the heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then dry and calcine, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 additive.

[0063] Example 4

[0064] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0065] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0066] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0067] (3) Mix the pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) with water, acetic acid solution, citric acid and activated carbon, and stir under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, citric acid is 2.7g, and activated carbon is 1.0g. The heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then dry and calcine, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 adsorbent.

[0068] Example 5

[0069] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0070] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0071] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0072] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and blue carbon, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, citric acid is 2.7g, blue carbon is 1.0g, heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then it is dried and calcined, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 adsorbent.

[0073] Example 6

[0074] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0075] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:5;

[0076] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 1 h, and the heating rate is 10° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0077] (3) Mix the pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) with water, acetic acid solution and citric acid, stir under heating conditions to form a gel, wherein the mass of the pre-calcined calcium carbide desulfurization slag mixed powder is 5g, the water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, the citric acid is 12g, the heating and stirring is 90°C water bath heating, the stirring rate is 500r / min, and the time is 5h. Then dry and calcine, the drying temperature is 110°C, the time is 48h, the calcination atmosphere is air atmosphere, the calcination temperature is 800°C, the holding time is 2h, and the heating rate is 10°C / min, to obtain the CO2 adsorbent.

[0078] See also Figure 3 , it can be seen that there are abundant pores on the adsorbent particles, and the particles are connected to each other to form a relatively strong structure.

[0079] Example 7

[0080] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0081] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:2;

[0082] (2) pre-calcining the mixed powder of calcium carbide desulfurization slag obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1100° C., the holding time is 4 hours, and the heating rate is 5° C. / min, to obtain the pre-calcined mixed powder of calcium carbide desulfurization slag;

[0083] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and activated carbon, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 35mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, citric acid is 2.5g, and activated carbon is 1.25g. The heating and stirring is 80°C water bath heating, the stirring rate is 400r / min, and the time is 7h. Then it is dried and calcined, the drying temperature is 105°C, the time is 48h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 900°C, the holding time is 2h, and the heating rate is 5°C / min, to obtain the CO2 adsorbent.

[0084] Example 8

[0085] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0086] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 1:10;

[0087] (2) pre-calcining the carbide desulfurization slag mixed powder obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 2 h, and the heating rate is 6° C. / min, to obtain the pre-calcined carbide desulfurization slag mixed powder;

[0088] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid, activated carbon and blue charcoal, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 45mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:6, citric acid is 3g, activated carbon is 0.25g, blue charcoal is 1g, heating and stirring are 85°C water bath heating, the stirring rate is 600r / min, and the time is 6h. Then it is dried and calcined, the drying temperature is 115°C, the time is 40h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 800°C, the holding time is 3h, and the heating rate is 6°C / min, to obtain the CO2 adsorbent.

[0089] Example 9

[0090] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0091] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 3:10;

[0092] (2) pre-calcining the mixed powder of calcium carbide desulfurization slag obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1000° C., the holding time is 3 hours, and the heating rate is 9° C. / min, to obtain the pre-calcined mixed powder of calcium carbide desulfurization slag;

[0093] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and activated carbon, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 40mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:5, citric acid is 2.8g, and activated carbon is 1.0g. The heating and stirring is 85°C water bath heating, the stirring rate is 450r / min, and the time is 6.5h. Then it is dried and calcined, the drying temperature is 120°C, the time is 30h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 840°C, the holding time is 4h, and the heating rate is 7°C / min, to obtain the CO2 adsorbent.

[0094] Example 10

[0095] This embodiment provides a method for preparing a high-performance CO2 adsorbent using desulfurization waste residue and carbide slag, the preparation method comprising the following steps:

[0096] (1) mixing and stirring desulfurization waste residue and carbide slag, grinding them into powder, and obtaining carbide desulfurization slag mixed powder, wherein the mass ratio of the desulfurization waste residue to the carbide slag is 2:5;

[0097] (2) pre-calcining the mixed powder of calcium carbide desulfurization slag obtained in step (1), wherein the pre-calcination atmosphere is an air atmosphere, the temperature is 1100° C., the holding time is 3 hours, and the heating rate is 8° C. / min, to obtain the pre-calcined mixed powder of calcium carbide desulfurization slag;

[0098] (3) The pre-calcined calcium carbide desulfurization slag mixed powder obtained in step (2) is mixed with water, acetic acid solution, citric acid and activated carbon, and stirred under heating conditions to form a gel, wherein the pre-calcined calcium carbide desulfurization slag mixed powder has a mass of 5g, water is 42mL, the acetic acid solution is 8mL of acetic acid diluted with water in a volume ratio of 1:4, citric acid is 2.6g, and active blue carbon is 0.75g. The heating and stirring is 85°C water bath heating, the stirring rate is 550r / min, and the time is 6h. Then it is dried and calcined, the drying temperature is 130°C, the time is 24h, the calcination atmosphere is a nitrogen atmosphere, the calcination temperature is 870°C, the holding time is 3h, and the heating rate is 8°C / min, to obtain the CO2 adsorbent.

[0099] Comparative Example 1

[0100] This comparative example provides a method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag, the only difference being that step (3) is not performed.

[0101] See also Figure 4 It can be seen that the image of carbide slag under the electron microscope is blocky and mostly agglomerated together. The particles are large, there are fewer pores on the surface of the particles, and the specific surface area is small.

[0102] The carbon dioxide adsorbents prepared in Examples 1-6 and Comparative Example 1 were used for high-temperature carbon dioxide capture to evaluate the capture performance of the adsorbents. The reaction process and conditions during the application were as follows: (1) Heating stage: nitrogen atmosphere, heating from room temperature to 750-900°C, with a heating rate of 10°C / min; (2) Activation stage: nitrogen atmosphere, maintaining at 750-900°C for 20-40 min, then cooling from 750-900°C to 500-650°C, with a cooling rate of 10°C / min; (3) Carbon dioxide capture stage: 15% CO2, nitrogen as the balance gas, and a reaction time of 40 min at 500-650°C.

[0103] The temperature in the activation stage in Examples 1-6 and Comparative Example 1 was 600° C., and the temperature in the carbon dioxide capture stage was 600° C. This process was carried out, and the test results obtained are shown in Table 1.

[0104] Table 1 Adsorption performance test results

[0105]

[0106]

[0107] As shown in Table 1, when the above adsorbents are used for CO2 capture, the adsorbents in Examples 1-6 have higher CO2 capture amounts than Comparative Example 1, and the carbonation conversion rates of Examples 2 and 6 can reach more than 97%. It can be seen that when the adsorbent is prepared, the calcium carbonate and magnesium carbonate are decomposed and the amorphous carbon is burned by heating, mixing, stirring and calcining to release a large amount of gas and heat, thereby obtaining smaller adsorbent particles and a looser porous structure, thereby enhancing the carbon dioxide capture capacity of the adsorbent.

[0108] The carbon dioxide adsorbent prepared in Examples 2-6 was used for high-temperature carbon dioxide capture and desorption to evaluate the regeneration performance of the adsorbent: the reaction process and conditions during the application were: (1) Heating stage: nitrogen atmosphere, heating from room temperature to 750-900°C, heating rate 10°C / min; (2) Activation stage: nitrogen atmosphere, maintaining at 750-900°C for 20-40 min, then cooling from 750-900°C to 500-650°C, cooling rate 10°C / min; (3) Carbon dioxide capture stage: 15% CO2, nitrogen as balance gas, reaction time at 500-650°C for 40 min; (4) Carbon dioxide desorption stage: nitrogen atmosphere, heating from 500-650°C to 650-750°C, heating rate 10°C / min, and maintaining at 650-750°C for 50-70 min.

[0109] In Example 2-6, the temperature of the activation stage was 600° C., the temperature of the carbon dioxide capture stage was 600° C., and the temperature of the carbon dioxide desorption stage was 650° C. After the process was performed once, steps (3) to (4) were repeated 15 times, and the results are shown in Table 2.

[0110] Table 2 Repeated adsorption performance results

[0111]

[0112] As shown in Table 2, when the above carbon dioxide adsorbent is used for high-temperature carbon dioxide capture and desorption, the adsorbents in Examples 2-6 all have a significant decrease in adsorption performance in the first two cycles, but the adsorbents show good stability in subsequent cycles. Among them, the regeneration performance of the adsorbents in Example 2, Example 3, and Example 6 is good, which shows that the use of desulfurization waste residue and carbide slag to prepare carbon dioxide adsorbents makes full use of silicon oxide, aluminum oxide and other materials contained in desulfurization waste residue and carbide slag to support calcium oxide and magnesium oxide, plays a certain anti-sintering effect, and enhances the cycle stability of the adsorbent.

[0113] In summary, it can be seen that the method of the present invention uses carbide slag and desulfurization waste residue as raw materials, first pre-calcines them, and then uses the sol-gel method to obtain a carbon dioxide adsorbent, thereby realizing efficient resource utilization of carbide slag and desulfurization waste residue; the present invention obtains the adsorbent by calcining in an air or nitrogen atmosphere, enriches the pores therein, and at the same time makes the distribution of various substances uniform, and makes full use of inert substances such as Al, Si and alkali metal elements such as Fe in the carbide slag and desulfurization waste residue to improve the sintering resistance and capture performance of the adsorbent; the method is simple in process, and the required reagents are all common reagents, which can synergistically treat desulfurization waste residue and carbide slag, and has excellent performance, low energy consumption, and good industrial application value.

[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag, characterized in that: The following steps are involved: The mixed powder of desulfurization waste residue and carbide slag is pre-calcined, and then the pre-calcined powder, water, acetic acid solution and citric acid are mixed, heated to form a gel, and then dried and calcined to obtain a high-performance carbon dioxide adsorbent.

2. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The mass ratio of the desulfurization waste residue to the carbide slag is (1-5):

10.

3. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The pre-calcination is carried out in an air atmosphere, the pre-calcination temperature is 1000-1100°C, and the time is 1-4h; the pre-calcination heating rate is 5-10°C / min; SO2 gas generated during the pre-calcination process is collected and used to prepare sulfuric acid.

4. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: Carbonaceous supports are also included.

5. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 4, characterized in that: The carbon-containing carrier is one or both of activated carbon and blue charcoal.

6. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The acetic acid solution is a solution obtained by diluting acetic acid and water in a volume ratio of 1:4 to 1:6; the mass ratio of the acetic acid solution to the pre-calcined powder is 1.5:1 to 1.8:

1.

7. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 4, characterized in that: The mass ratio of the water to the pre-calcined powder is 7:1 to 9:1; the mass ratio of the carbon-containing carrier to the pre-calcined powder is 1:10 to 1:

4.

8. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The mass ratio of the citric acid to the pre-calcined powder is 0.5:1 to 0.6:

1.

9. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The heating temperature is 80-90° C., and the time is 5-7 hours; the stirring rate is 400 r / min-600 r / min; the drying temperature is 105-130° C., and the drying time is 24 hours-48 hours.

10. The method for preparing a high-performance carbon dioxide adsorbent using desulfurization waste residue and carbide slag according to claim 1, characterized in that: The calcination is carried out in air or nitrogen atmosphere; the calcination temperature is 800-900°C, the time is 2-4h; the calcination heating rate is 5-10°C / min.

Citation Information

Patent Citations

  • Method for preparing lithiumzirconate materials capable of rapidly absorbing CO2 at high temperature

    CN101774636A

  • Method for capturing carbon dioxide by virtue of acetylene sludge

    CN107285357A

  • Method for preparing porous calcium-based material from eggshell and application of porous calcium-based material in thermochemical energy storage

    CN113512409A

  • CO2 adsorbent based on multi-source solid waste modification and preparation method and application thereof

    CN114130350A

  • Method for desulfurization and carbon sequestration of coal-fired flue gas by using carbide slag slurry

    CN115006982A