Efficient phosphorus removal adsorbent for sewage and preparation method of efficient phosphorus removal adsorbent

By mixing bentonite with slag and modifying it, combined with the catalysis of calcium ions and magnesium ions, an efficient phosphorus removal adsorbent is formed, which solves the problems of poor phosphorus removal effect and high cost in the existing technology, and achieves high efficiency and environmental protection. The phosphorus removal effect of water bodies.

CN118807683AInactive Publication Date: 2024-10-22BEIJING UNIV OF CIVIL ENG & ARCHITECTURE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411219568.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Among existing water phosphorus removal technologies, biological methods have harsh conditions, chemical methods produce secondary pollution, physical methods consume large amounts of energy and are costly, and existing phosphorus removal adsorbents have high preparation costs and limited adsorption effects.

Method used

Using bentonite and slag as raw materials, through mixing and modification, iron oxide is used to improve the phosphorus adsorption capacity, and the catalytic premix of calcium ions and magnesium ions is used to increase the interlayer spacing of the adsorbent to form an efficient phosphorus removal adsorbent.

Benefits of technology

It significantly improves the phosphorus adsorption effect, reduces production costs and environmental impact, and provides an efficient and environmentally friendly phosphorus removal solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807683A_ABST
    Figure CN118807683A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of phosphorus removal agents, in particular to an efficient phosphorus removal adsorbent for sewage and a preparation method of the efficient phosphorus removal adsorbent. The invention relates to a high-efficiency and high-strength concrete additive which comprises the following components in parts by weight: 4-5 parts of a powdery premix, 0.1-0.2 part of a modified premix and 80-100 parts of a catalytic premix, the weight ratio of the catalytic premix to the powdery premix is 20: 1, the powdery premix comprises bentonite and slag, the weight ratio of the bentonite to the slag is 10: (1.5-2.5), and the content of montmorillonite in the bentonite is 60%-70%. According to the phosphorus removal adsorbent disclosed by the invention, the bentonite and the furnace slag are used as raw materials, the furnace slag contains more iron oxide, the surface of the iron oxide has good phosphorus adsorption capacity, the phosphorus adsorption capacity of the bentonite can be remarkably improved, the furnace slag and the bentonite are mixed for utilization, by-products can be effectively utilized, and the phosphorus removal effect is improved. The dependence on fresh raw materials is reduced, and the production cost and the environmental influence are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phosphorus removal agent preparation, and in particular to a high-efficiency phosphorus removal adsorbent for sewage and a preparation method thereof. Background Art

[0002] The eutrophication of oceans, rivers, lakes and other water bodies has always attracted much attention. Eutrophication will have a series of adverse effects on aquatic life, shipping safety and water landscape. Excessive phosphorus is the key factor causing eutrophication of water bodies. Studies have shown that when phosphorus in water exceeds 0.02 mg / L, eutrophication will occur. Therefore, when managing water bodies such as rivers and lakes, phosphorus control is an extremely important link. The sources of phosphorus are relatively wide. The production wastewater of phosphorus-containing pesticides, fertilizers, detergents, and domestic wastewater will lead to phosphorus discharge.

[0003] Existing water phosphorus removal technologies include biological, chemical and physical methods. Biological phosphorus removal does not require the addition of chemicals and is environmentally friendly, but it has the disadvantages of harsh operating conditions, complex process flow, and high construction and operation costs. Chemical phosphorus removal requires the addition of a large amount of chemical agents, produces a large amount of chemical sludge, and may cause secondary pollution to the environment. Physical phosphorus removal, such as reverse osmosis technology and electrodialysis technology, consumes a lot of energy, has expensive equipment and high operating costs. Compared with the above technologies, adsorption technology has the characteristics of high phosphorus removal rate and simple operation.

[0004] The phosphorus removal adsorbents in the prior art are mostly made of natural bentonite, which has a relatively limited adsorption effect and needs to be combined with additional additives, resulting in a high preparation cost. Summary of the invention

[0005] In view of the problems existing in the background technology, a highly efficient phosphorus removal adsorbent for sewage and a preparation method thereof are proposed. The present invention uses bentonite and slag as raw materials. The slag contains a large amount of iron oxides, and the surface of the iron oxides has a good phosphorus adsorption capacity, which can significantly improve the phosphorus adsorption capacity of bentonite. Mixing the slag and bentonite for use can not only effectively utilize these by-products, but also help reduce dependence on fresh raw materials, reduce production costs and environmental impacts.

[0006] The invention provides a high-efficiency phosphorus removal adsorbent for sewage, comprising the following components in parts by weight: 4-5 parts of powdered premix, 0.1-0.2 parts of modified premix and 80-100 parts of catalytic premix, and in a weight ratio of catalytic premix: powdered premix = 20:1.

[0007] Preferably, the powdery premix comprises bentonite and slag, in a weight ratio of bentonite:slag=10:1.5-2.5, and the content of montmorillonite in the bentonite is 60%-70%.

[0008] Preferably, the modified premix liquid comprises hexadecyltrimethylammonium bromide and sodium alkyl ether sulfate, and the weight ratio of hexadecyltrimethylammonium bromide to sodium alkyl ether sulfate is 3:1.

[0009] Preferably, the catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 80-120 mmol / L, the concentration of magnesium ions is 40-60 mmol / L, and the molar ratio of calcium ions to magnesium ions is 2:1.

[0010] The present invention also provides a method for preparing a high-efficiency phosphorus removal adsorbent for sewage, which is applied to prepare the high-efficiency phosphorus removal adsorbent for sewage mentioned above, comprising the following steps:

[0011] S1. Weigh a certain amount of industrial bentonite and slag, grind and mix them, and pass them through a 100-mesh sieve to obtain a powdery premix;

[0012] S2, cetyl trimethyl ammonium bromide and alkyl ether sodium sulfate are mixed uniformly in a certain proportion to form a modified premixed liquid, which is then poured into the powdered premix, and the two are stirred for 2-4 hours using a temperature-controlled stirrer to maintain a constant temperature and a constant speed to form a mixture;

[0013] S3, weighing a certain amount of calcium chloride and magnesium chloride and mixing them with water to form a catalytic premixed liquid, injecting the mixture into the catalytic premixed liquid, stirring at room temperature with a magnetic stirrer for 3-5 hours, filtering and washing the solid-liquid mixture to obtain a solid product;

[0014] S4, drying the solid product, and then calcining it at high temperature using a calcination device to obtain a dephosphorization adsorbent.

[0015] Preferably, the drying method in step S4 can be air drying, air drying and oven drying, wherein the drying temperature needs to be less than 90°C, and the calcination temperature needs to be controlled at 600°C-800°C.

[0016] Through the above technical scheme, that is, the phosphorus removal adsorbent disclosed in the present invention, bentonite and slag are used as raw materials. The slag contains more iron oxides, and the surface of the iron oxides has good phosphorus adsorption capacity, which can significantly improve the adsorption capacity of bentonite for phosphorus. Mixing the slag with bentonite can not only effectively utilize these by-products, but also help reduce dependence on fresh raw materials, reduce production costs and environmental impacts; and a catalytic premix is ​​provided, which exchanges sodium ions in the raw materials with calcium ions and magnesium ions, thereby increasing the interlayer spacing of the adsorbent, expanding its adsorption area, and further improving its adsorption capacity.

[0017] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention is a flowchart of a method for preparing a highly efficient phosphorus removal adsorbent for sewage. DETAILED DESCRIPTION

[0019] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0020] Embodiment 1

[0021] The invention provides a high-efficiency phosphorus removal adsorbent for sewage, comprising the following components by weight: 4 parts of powdered premix, 0.1 parts of modified premix and 80 parts of catalytic premix, and by weight ratio, the catalytic premix: powdered premix = 20:1.

[0022] Furthermore, the powdery premix includes bentonite and slag, the content of montmorillonite in the bentonite is 60%-70%, and the weight ratio of bentonite: slag is 10:1.

[0023] Furthermore, the modified premix liquid includes hexadecyltrimethylammonium bromide and sodium alkyl ether sulfate, and the weight ratio of hexadecyltrimethylammonium bromide to sodium alkyl ether sulfate is 3:1.

[0024] Furthermore, the catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 80 mmol / L, the concentration of magnesium ions is 40 mmol / L, and the molar ratio of calcium ions: magnesium ions is 2:1.

[0025] Embodiment 2

[0026] The difference between this embodiment and embodiment 1 is that, in terms of weight ratio, the mineral mixed raw material includes bentonite and slag, and the ratio of bentonite to slag is 10:1.5.

[0027] Embodiment 3

[0028] The difference between this embodiment and embodiment 1 is that, in terms of weight ratio, the mineral mixed raw material includes bentonite and slag, and the ratio of bentonite to slag is 10:2.

[0029] Embodiment 4

[0030] The difference between this embodiment and embodiment 1 is that, in terms of weight ratio, the mineral mixed raw material includes bentonite and slag, and the ratio of bentonite to slag is 10:2.5.

[0031] Embodiment 5

[0032] The difference between this embodiment and embodiment 1 is that, in terms of weight ratio, the mineral mixed raw material includes bentonite and slag, and the ratio of bentonite to slag is 10:3.

[0033] Embodiment 6

[0034] The difference between this embodiment and embodiment 1 is that the high-efficiency phosphorus removal adsorbent includes the following components in parts by weight: 4 parts of powdered premix, 0.2 parts of modified premix and 80 parts of catalytic premix, and in weight ratio, catalytic premix: powdered premix = 20:1.

[0035] Embodiment 7

[0036] The difference between this embodiment and embodiment 1 is that the high-efficiency phosphorus removal adsorbent includes the following components by weight: 4 parts of powdered premix, 0.3 parts of modified premix and 80 parts of catalytic premix, and by weight ratio, catalytic premix: powdered premix = 20:1

[0037] Embodiment 8

[0038] The difference between this embodiment and embodiment 1 is that the catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 100 mmol / L, the concentration of magnesium ions is 50 mmol / L, and the molar ratio of calcium ions: magnesium ions is 2:1.

[0039] Embodiment 9

[0040] The difference between this embodiment and embodiment 1 is that the catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 120 mmol / L, the concentration of magnesium ions is 60 mmol / L, and the molar ratio of calcium ions: magnesium ions is 2:1.

[0041] Embodiment 10

[0042] The difference between this embodiment and embodiment 1 is that the catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 130 mmol / L, the concentration of magnesium ions is 65 mmol / L, and the molar ratio of calcium ions: magnesium ions is 2:1.

[0043] Embodiment 11

[0044] The present invention also proposes a method for preparing the above-mentioned high-efficiency phosphorus removal adsorbent for sewage, comprising the following steps:

[0045] S1. Weigh a certain amount of industrial bentonite and slag, grind and mix them, and pass them through a 100-mesh sieve to obtain a powdery premix;

[0046] S2, cetyl trimethyl ammonium bromide and alkyl ether sodium sulfate are mixed uniformly in a certain proportion to form a modified premixed liquid, which is then poured into the powdered premix, and the two are stirred for 2-4 hours using a temperature-controlled stirrer to maintain a constant temperature and a constant speed to form a mixture;

[0047] S3, weighing a certain amount of calcium chloride and magnesium chloride and mixing them with water to form a catalytic premixed liquid, injecting the mixture into the catalytic premixed liquid, stirring at room temperature with a magnetic stirrer for 3-5 hours, filtering and washing the solid-liquid mixture to obtain a solid product;

[0048] S4, drying the solid product, and then calcining it at high temperature using a calcination device to obtain a dephosphorization adsorbent.

[0049] In an optional embodiment, the drying method in step S4 can be air drying, air drying and oven drying, wherein the drying temperature needs to be less than 90°C, and the calcination temperature needs to be controlled at 600°C-800°C.

[0050] Experimental Example 1

[0051] The wastewater to be tested was divided into six groups, each containing 1L, and the initial phosphorus content was measured. Then, 1g of natural bentonite adsorbent and the phosphorus removal adsorbent prepared in Examples 1, 2, 3, 4 and 5 were added to the corresponding wastewater. After 24 hours, the phosphorus content was tested again and the removal rate was calculated. The results are shown in the following table:

[0052] Phosphorus removal adsorbent Initial concentration (mg / L) Concentration after removal (mg / L) Removal rate (100%) Natural bentonite 8.2 7.21 12.07 Embodiment 1 8.2 1.32 83.90 Embodiment 2 8.2 1.04 87.31 Embodiment 3 8.2 0.83 89.88 Embodiment 4 8.2 0.72 91.22 Embodiment 5 8.2 0.93 88.66

[0053] It can be seen from the table that the phosphorus removal adsorbent prepared in the present invention significantly improves the phosphorus removal effect on sewage compared with the natural bentonite adsorbent, and adding more slag to the raw material within a certain proportion range improves the adsorption effect on phosphorus.

[0054] Experimental Example 2

[0055] The wastewater to be tested was divided into four groups, each containing 1L, and the initial phosphorus content was measured. Then, 1g of natural bentonite adsorbent and the phosphorus removal adsorbent prepared in Examples 1, 6 and 7 were added to the corresponding wastewater. After 24 hours, the phosphorus content was tested again and the removal rate was calculated. The results are shown in the following table:

[0056] Phosphorus removal adsorbent Initial concentration (mg / L) Concentration after removal (mg / L) Removal rate (100%) Natural bentonite 8.2 7.21 12.07 Embodiment 1 8.2 1.32 83.90 Embodiment 6 8.2 0.74 90.9 Embodiment 7 8.2 1.53 81.34

[0057] It can be seen from the table that the phosphorus removal adsorbent prepared in the present invention significantly improves the phosphorus removal effect on sewage compared with the natural bentonite adsorbent, and the adsorption effect on phosphorus is improved by adding the content of the modified premix within a reasonable range.

[0058] Experimental Example 3

[0059] The wastewater to be tested was divided into four groups, each containing 1L, and the initial phosphorus content was measured. Then, 1g of natural bentonite adsorbent and the phosphorus removal adsorbent prepared in Examples 1, 8, 9, and 10 were added to the corresponding wastewater. After 24 hours, the phosphorus content was tested again and the removal rate was calculated. The results are shown in the following table:

[0060] Phosphorus removal adsorbent Initial concentration (mg / L) Concentration after removal (mg / L) Removal rate (100%) Natural bentonite 8.2 7.21 12.07 Embodiment 1 8.2 1.32 83.90 Embodiment 8 8.2 1.13 86.22 Embodiment 9 8.2 0.97 88.17 Embodiment 10 8.2 1.07 86.95

[0061] It can be seen from the table that the phosphorus removal adsorbent prepared in the present invention significantly improves the phosphorus removal effect on sewage compared with the natural bentonite adsorbent, and by increasing the concentration of sodium ions and magnesium ions in the catalytic premix within a reasonable range, the interlayer spacing of the adsorbent is increased, thereby improving the adsorption effect on phosphorus.

[0062] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited thereto, and various changes can be made within the knowledge scope of technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A highly efficient phosphorus removal adsorbent for sewage, characterized in that: The invention comprises the following components in parts by weight: 4-5 parts of powdered premix, 0.1-0.2 parts of modified premix and 80-100 parts of catalytic premix, and in a weight ratio of catalytic premix: powdered premix = 20:

1.

2. The high-efficiency phosphorus removal adsorbent for sewage according to claim 1, characterized in that: The powdered premix comprises bentonite and slag, and the weight ratio of bentonite to slag is 10:1.5-2.5, and the content of montmorillonite in the bentonite is 60%-70%.

3. The high-efficiency phosphorus removal adsorbent for sewage according to claim 1, characterized in that: The modified premixed liquid includes hexadecyltrimethylammonium bromide and sodium alkyl ether sulfate, and the weight ratio of hexadecyltrimethylammonium bromide to sodium alkyl ether sulfate is 3:

1.

4. The high-efficiency phosphorus removal adsorbent for sewage according to claim 1, characterized in that: The catalytic premix includes water, calcium ions and magnesium ions, the concentration of calcium ions is 80-120 mmol / L, the concentration of magnesium ions is 40-60 mmol / L, and the molar ratio of calcium ions to magnesium ions is 2:

1.

5. A method for preparing a highly efficient phosphorus removal adsorbent for sewage, which is applied to the highly efficient phosphorus removal adsorbent for sewage according to any one of claims 1 to 4, comprising the following steps: S1. Weigh a certain amount of industrial bentonite and slag, grind and mix them, and pass them through a 100-mesh sieve to obtain a powdery premix; S2, cetyl trimethyl ammonium bromide and alkyl ether sodium sulfate are mixed uniformly in a certain proportion to form a modified premixed liquid, which is then poured into the powdered premix, and the two are stirred for 2-4 hours using a temperature-controlled stirrer to maintain a constant temperature and a constant speed to form a mixture; S3, weighing a certain amount of calcium chloride and magnesium chloride and mixing them with water to form a catalytic premixed liquid, injecting the mixture into the catalytic premixed liquid, stirring at room temperature with a magnetic stirrer for 3-5 hours, filtering and washing the solid-liquid mixture to obtain a solid product; S4, drying the solid product, and then calcining it at high temperature using a calcination device to obtain a dephosphorization adsorbent.

6. The method for preparing a highly efficient phosphorus removal adsorbent for sewage according to claim 5, characterized in that: The drying method in step S4 can be air drying, air drying and oven drying, wherein the drying temperature needs to be less than 90°C, and the calcination temperature needs to be controlled at 600°C-800°C.

Citation Information

Patent Citations

  • Preparation method of modified illite adsorbent for removing naphthol green B

    CN105561916A

  • Organic-inorganic composite bentonite material and preparation method and application thereof

    CN107282021A

  • Adsorption material for treatment of domestic sewage and preparation method and application thereof

    CN109499531A