High-adsorption-capacity salt lake lithium extraction adsorbent and preparation method thereof

By using porous fly ash carriers to synthesize LiAl-LDHs spherical adsorbents, the problems of high cost and low efficiency of existing lithium adsorbents in extracting lithium from brine with high Mg2+/Li+ ratio are solved, achieving high adsorption capacity, low cost, and Environmentally friendly lithium recycling effect.

CN118807684AActive Publication Date: 2024-10-22WUHAN UNIV OF SCI & TECH +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411224532.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-22
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing lithium adsorbents have high cost and low efficiency in the process of extracting lithium from brine with high Mg2+/Li+ ratio, and the powdery preparation process leads to problems such as poor fluidity, easy dissolution damage, and equipment clogging, which reduces the durability of its recycling. and efficiency.

Method used

Using porous fly ash as a carrier, by mixing coal fly ash, kaolin, attapulgite and pore-forming agent, after calcination, add AlCl3 and NaAlO2 to boric acid and sodium hexametaphosphate solution, control the pH value and temperature, and generate LiAl- LDHs spherical adsorbent has high adsorption capacity and strength.

Benefits of technology

It achieves high adsorption capacity, low cost, and environmentally friendly lithium recovery. The lithium adsorbent has high strength, low dissolution rate, and good regeneration performance. It is suitable for efficient extraction of lithium from brine with high Mg2+/Li+ ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807684A_ABST
    Figure CN118807684A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of materials, and particularly relates to a high-adsorption-capacity salt lake lithium extraction adsorbent and a preparation method thereof. The method comprises the following steps: firstly preparing a filler carrier, then respectively dissolving AlCl3 and NaAlO2 into a mixed solution of boric acid and sodium hexametaphosphate, adding the filler carrier into the mixed solution containing AlCl3, standing, adding a mixed solution containing NaAlO2 and a LiCl solution, then slowly adding an ammonia water solution, and controlling the pH value to be 4-5 and the temperature to be 50-60 DEG C; after centrifuging, taking precipitate and drying; and eluting for 5-8 hours to obtain the high-adsorption-capacity salt lake lithium extraction adsorbent. The adsorbent is LiAl-LDHs and is a unique layered material composed of monovalent Li < + > and trivalent Al < 3 + >, Li < + > selectively enters a solid phase to form LiAl-LDHs, and the adsorbent has excellent performance in the field of lithium extraction from salt lakes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of materials, and relates to a salt lake lithium extraction adsorbent and a preparation method thereof, and specifically relates to a salt lake lithium extraction adsorbent with high adsorption capacity and a preparation method thereof. Background Art

[0002] As the global demand for renewable energy continues to grow, lithium batteries have become one of the core components of modern energy storage solutions. Lithium resources exist in three main forms: brine lithium mines in closed basins, pegmatite-type hard rock lithium mines, and sedimentary clay lithium mines, which are mainly distributed in Bolivia, Argentina, the United States, Chile, Australia and other countries. Among them, brine lithium resources are highly concentrated in the arid zones of the northern and southern hemispheres. There are only five salt lakes with more than 1 million tons of metallic lithium resources, and only 16 with more than 100,000 tons, which are located in Bolivia, Chile, China, Argentina, the United States, and Canada, of which China accounts for 5.

[0003] In terms of reserves, my country has proven 6.8 million tons of lithium resources, including salt lakes and hard rock lithium mines. Salt lake brine is the main form of lithium resources in my country, mainly in Qinghai and Tibet inland plateau salt lakes. In terms of mineral quality, my country's hard rock lithium mines are mainly low-quality lithium mica, while the lithium content of salt lake brine mines is generally low, such as K + 、Na + , Ca 2+ Mg 2+ The content of impurities is high, and extraction is difficult. Some high-quality salt lake lithium resources are distributed in Tibet, Sichuan and other areas with fragile ecological environment or harsh natural conditions. The development and utilization process is slow, which to a certain extent leads to high cost of lithium resource extraction in my country and the profitability of minerals is far below the international level.

[0004] It can be seen that my country's lithium mainly comes from ores and salt lake brine, the latter of which accounts for about 60% of the total. Compared with ore lithium resources, extracting lithium from brine has lower production costs and difficulty, and in addition to a slight water footprint, it has less impact on the environment. Therefore, an important way to achieve a sustainable supply of lithium is to develop a promising method for extracting lithium from brine. However, lithium in brine is usually accompanied by high concentrations of cations, such as Mg 2+ 、Na + , K + and Ca 2+ These cations, especially Mg 2+ , has similar properties to Li+, which makes it challenging to recover lithium from brines. 2+ / Li + When the ratio is less than 6, lithium can be economically extracted by soda precipitation. 2+ / Li +When the ratio is high, the cost of the precipitation process increases significantly. It is worth noting that a large number of brines have high Mg 2+ / Li + ratio, especially in China. In this context, people have proposed 2+ / Li + Alternative technologies for extracting lithium from brine include adsorption, nanofiltration, electrodialysis, reverse osmosis, and evaporation concentration.

[0005] Adsorption is not only a key step in the lithium extraction process, but is also considered the most direct technology for extracting lithium from brines, especially those with low grade and high Mg 2+ / Li + Compared with brine, lithium ions have high selectivity and recovery rate, high concentration function, cost-effectiveness and environmental advantages due to the small brine pretreatment requirements. It is worth noting that the lithium recovery efficiency depends significantly on the lithium adsorbent. The selection of lithium adsorbents usually depends on the performance of the adsorbent (including adsorption capacity, selectivity, stability, recycling, etc.), the structure of the adsorbent (including macro and micro structure), brine characteristics (including pH, lithium concentration, temperature, Mg 2+ / Li + ratio, etc.). Currently, lithium adsorbents in the industry are in powder form, which is greatly affected by the preparation and molding process, has poor fluidity and permeability, and is prone to loss of adsorbents during the production process. In addition, due to the poor fluidity of the powder, it is easy to cause dissolution damage, large pressure difference, equipment blockage, and dust explosion, which reduces the durability and efficiency of its recycling.

[0006] Fly ash is the fine ash collected from the flue gas after coal combustion. It is the main solid waste discharged by coal-fired power plants. The main oxide components of fly ash in my country's thermal power plants are: SiO2, Al2O3, FeO, Fe2O3, CaO, TiO2, etc. The aluminum oxide content in fly ash is generally around 40%, and can be as high as 50% in some areas. With the development of the power industry, the amount of fly ash discharged from coal-fired power plants has increased year by year, becoming one of the largest industrial waste residues in my country. Summary of the invention

[0007] The present invention overcomes the above-mentioned defects and provides a high-adsorption salt lake lithium extraction adsorbent and a preparation method thereof. The present invention has the characteristics of low cost and environmentally friendly lithium recovery.

[0008] The technical solution of the present invention is as follows:

[0009] A method for preparing a high adsorption capacity salt lake lithium extraction adsorbent comprises the following steps:

[0010] (1) coal fly ash, kaolin, attapulgite and a pore-forming agent are mixed, the materials are mixed with water, ground, centrifuged, the precipitate is extruded, and then calcined at 500 to 600° C. for 2 to 3 hours to obtain a treated filler carrier;

[0011] (2) AlCl3 and NaAlO2 are dissolved in a mixed solution of boric acid and sodium hexametaphosphate respectively, a filler carrier is added to the mixed solution of AlCl3, and after standing for 3-6 hours, a mixed solution of NaAlO2 and a LiCl solution are added, and then an ammonia solution is slowly added, and the pH value is controlled at 4-5 and the temperature is controlled at 50-60°C;

[0012] (3) After centrifugation, the precipitate is dried;

[0013] (4) Elution is performed in deionized water for 5 to 8 hours to obtain a salt lake lithium extraction adsorbent with a high adsorption capacity.

[0014] In the above method, in step (1), the pressing is to press the precipitate into a spherical state.

[0015] In the above method, in step (1), the material and water are added in a mass ratio of 1 to 2:1.

[0016] In the above method, in step (1), the added mass ratio of the coal fly ash, kaolin, attapulgite and pore-forming agent is: 5-10:15-20:5-10:8-10; the pore-forming agent is starch.

[0017] In the above method, in step (2), the molar ratio of boric acid to sodium hexametaphosphate in the mixed solution of boric acid and sodium hexametaphosphate is 1 to 2:1; and the concentration of boric acid in the mixed solution is 1 to 2 g / L.

[0018] In the above method, in step (2), the concentration of AlCl3 in the mixed solution is 10 to 30 g / L, and the concentration of NaAlO2 in the mixed solution is 5 to 20 g / L.

[0019] In the above method, in step (2), the concentration of the LiCl solution in the mixed solution is 1.5 to 10 g / L.

[0020] The above method is characterized in that the adsorption capacity of the adsorbent is: 2.0-4.0 mg / g.

[0021] The adsorbent of the present invention is used for extracting lithium from salt lakes.

[0022] The present invention makes the most of porous coal fly ash to provide a carrier for the subsequent synthesis of LiAl-LDHs. To a certain extent, waste is utilized, waste is turned into treasure, and environmental pressure is reduced. Aluminum hydroxide crystals are directly generated on the surface of the filler by a crystallization method, which can effectively improve the strength and adsorption capacity of the aluminum-based adsorbent. The method provides that the fly ash particles used in the present invention have a porous honeycomb structure, a large specific surface area, and a high adsorption activity. The particle size range of the particles is 300 to 600 μm. It has a porous structure, a porosity of up to 50%-80%, and strong water absorption.

[0023] In the present invention, step 1 synthesizes a porous filler carrier, and the pores of the filler carrier are evenly distributed through the pore-forming agent. At the same time, kaolin and attapulgite can also shape the internal filler channels of the porous channels, and attapulgite plays the role of bonding fly ash. In step 2, a mixed solution of boric acid and sodium hexametaphosphate, as well as precise control of the pH value, is used to finally synthesize a spherical object loaded with LiAl-LDHs. In this application, pH and a synthesis temperature of 50 to 60°C are both key parameters. After verification by the applicant, this condition plays an important role in the generation of layered crystals. When the temperature and pH value are exceeded, the generated LiAl-LDHs will dissolve and form a powder after drying.

[0024] The adsorption principle of the present invention is:

[0025] The adsorbent of the present invention can be used as Li + Selective capture materials, namely Li + Selectively enter the solid phase to form LiAl-LDHs, while other ions remain in the liquid phase. This is because Li+ can be combined into the structural vacancies of LiAl-LDHs. Due to the memory effect and steric hindrance effect, it can achieve highly selective adsorption of Li+ in brine, while other impurity ions cannot enter. LiAl-LDHs is a kind of Li+ composed of monovalent Li + and trivalent Al 3+ Unique layered material composed of Li + Insertion into the lattice vacancies in the octahedral framework of Al(OH)3 produces a positively charged structure.

[0026] Compared with the prior art, the advantages of the present invention are:

[0027] The adsorbent in the present invention is a spherical lithium adsorbent, which has the characteristics of high strength, low dissolution rate, strong adsorption capacity, good regeneration performance, etc. The adsorbent of the present invention has excellent performance in lithium extraction from salt lakes. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is an electron microscope scanning image of the high adsorption capacity salt lake lithium extraction adsorbent obtained in Example 1.

[0029] Figure 2 This is an electron microscope scanning image of the high adsorption capacity salt lake lithium extraction adsorbent obtained in Example 1.

[0030] Figure 3 This is a schematic diagram of the device structure in Example 3. DETAILED DESCRIPTION

[0031] Example 1

[0032] (1) 5 kg of coal fly ash, 20 kg of kaolin, 7 kg of attapulgite and 8 kg of starch were mixed, the materials were mixed with 25 kg of water, ground, centrifuged, the precipitate was taken, extruded into a spherical state, and then calcined at 5° C. for 3 h to obtain a treated filler carrier;

[0033] (2) First, take 100g of boric acid and 100g of sodium hexametaphosphate, add them to 100L of water to prepare a mixed solution of boric acid and sodium hexametaphosphate; take 1500g of AlCl3 and 700g of NaAlO2 and dissolve them in the mixed solution of boric acid and sodium hexametaphosphate (take 50L each), add 15kg of filler carrier to the mixed solution of AlCl3, let it stand for 5h, and then place the solution in a water bath, and control the water bath temperature to 55°C; add the NaAlO2 mixed solution and 50L of LiCl solution (15g / L), and then slowly add ammonia solution to control the pH value to 4-5;

[0034] (3) Centrifuge at 150 r / min for 20 min and dry the precipitate;

[0035] (4) Elution was performed in deionized water for 5 h to obtain a salt lake lithium extraction adsorbent with a high adsorption capacity.

[0036] The electron microscope scanning image of the adsorbent obtained in this example is as follows Figure 1 and Figure 2 Shown

[0037] The scanning electron micrograph shows that the lithium adsorbent has good stability, is spherical, has uniform size, and has good adsorption and mechanical strength.

[0038] Example 2

[0039] (1) 8 kg of coal fly ash, 15 kg of kaolin, 5 kg of attapulgite and 8 kg of starch were mixed, the materials were mixed with 18 kg of water, ground, centrifuged, the precipitate was taken, extruded into a spherical state, and then calcined at 500 ° C for 3 hours to obtain a treated filler carrier;

[0040] (2) First, take 100g of boric acid and 100g of sodium hexametaphosphate, add them to 100L of water to prepare a mixed solution of boric acid and sodium hexametaphosphate; take 1500g of AlCl3 and 700g of NaAlO2 and dissolve them in the mixed solution of boric acid and sodium hexametaphosphate (take 50L each), add 15kg of filler carrier to the mixed solution of AlCl3, let it stand for 5h, and then place the solution in a water bath, and control the water bath temperature to 55°C; add the NaAlO2 mixed solution and 50L of LiCl solution (15g / L), and then slowly add ammonia solution to control the pH value to 4-5;

[0041] (3) Centrifuge at 150 r / min for 20 min and dry the precipitate;

[0042] (4) Elution was performed in deionized water for 5 h to obtain a salt lake lithium extraction adsorbent with a high adsorption capacity.

[0043] Example 3

[0044] Method A: Take the adsorbent obtained in Example 1, take 80g of lithium adsorbent, clean it and wet-pack it into a column (such as Figure 3 The device simulates industrial operation conditions, and processes brine from a salt lake in Qinghai downstream through a resin column, taking samples at certain volume intervals for analysis. After testing, the lithium ion content in the brine from a salt lake in Qinghai is 0.533 mg / g.

[0045] Method B: Reload the adsorbent after adsorption in method A into a new resin column and use Figure 3 The device was then eluted with deionized water, and the eluate was collected in stages (once every 2 hours) for analysis.

[0046] Detailed parameters are shown in Table 1

[0047] Table 1

[0048]

[0049] Adsorption capacity = cumulative adsorption amount / lithium adsorbent mass

[0050] Desorption capacity = desorption amount / lithium adsorbent mass

[0051] Resolution = desorption capacity / adsorption capacity × adsorption mass.

Claims

1. A method for preparing a high adsorption capacity salt lake lithium extraction adsorbent, characterized in that: The steps include: (1) Mixing coal fly ash, kaolin, attapulgite and a pore-forming agent, mixing the materials with water, grinding, centrifuging, extruding the precipitate, and then calcining at 500-600° C. for 2-3 hours to obtain a treated filler carrier; (2) AlCl3 and NaAlO2 are dissolved in a mixed solution of boric acid and sodium hexametaphosphate respectively, and a filler carrier is added to the mixed solution containing AlCl3. After standing for 3-6 hours, a mixed solution containing NaAlO2 and a LiCl solution are added, and then an ammonia solution is slowly added. The pH value is controlled at 4-5 and the temperature is controlled at 50-60°C. (3) After centrifugation, the precipitate is taken and dried; (4) Elution was performed in deionized water for 5 to 8 hours to obtain a salt lake lithium extraction adsorbent with a high adsorption capacity.

2. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (1), the pressing is to press the precipitate into a spherical state.

3. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (1), the material and water are added in a mass ratio of 1 to 2:

1.

4. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (1), the added mass ratio of the coal fly ash, kaolin, attapulgite and pore-forming agent is: 5~10:15~20:5~10:8~10; the pore-forming agent is starch.

5. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (2), the molar ratio of boric acid to sodium hexametaphosphate in the mixed solution of boric acid and sodium hexametaphosphate is 1-2:1; and the concentration of boric acid in the mixed solution is 1-2 g / L.

6. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (2), the concentration of AlCl3 in the mixed solution is 10-30 g / L, and the concentration of NaAlO2 in the mixed solution is 5-20 g / L.

7. The method for preparing a high adsorption capacity salt lake lithium extraction adsorbent according to claim 1, characterized in that: In step (2), the concentration of the LiCl solution in the mixed solution is 1.5-10 g / L.

8. A high adsorption capacity salt lake lithium extraction adsorbent prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The adsorption capacity of the adsorbent is: 2.0-4.0 mg / g.

9. The adsorbent according to claim 8 is used for extracting lithium from salt lakes.

Citation Information

Patent Citations

  • Preparation method for high-adsorption-capacity granular aluminum salt lithium extraction adsorbent

    CA3215363A1

  • Aluminum salt adsorbing agent, preparation method of aluminum salt adsorbing agent, and separation method of lithium in salt lake brine

    CN108543514A

  • Aluminum salt lithium adsorbent, and preparation method and application thereof

    CN108993376A

  • Salt lake lithium extraction adsorbent and preparation method thereof

    CN114289000A

  • Fly ash loaded hydrotalcite-like compound adsorbent, preparation method and application

    CN114768752A