Modified polyvinyl alcohol and chitosan composite membrane material for sterilizing and adsorbing antibiotic resistance genes and preparation method of modified polyvinyl alcohol and chitosan composite membrane material

The long-chain quaternary ammonium salt-modified polyvinyl alcohol and chitosan composite membrane material sterilizes and adsorbs antibiotic resistance genes at room temperature, solving the problem that traditional sewage treatment technology cannot effectively remove antibiotic resistance genes and achieving efficient simultaneous sterilization. and removal effect, ensuring environmental safety.

CN118807701AActive Publication Date: 2024-10-22YANSHAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410811194.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Traditional sewage treatment technology cannot effectively remove antibiotic resistance genes, causing them to spread in the environment and endanger human health. When existing methods destroy bacterial cell membranes, antibiotic resistance genes are released, and there is a lack of simultaneous sterilization and removal methods.

Method used

Long-chain quaternary ammonium salt-modified polyvinyl alcohol and chitosan composite membrane materials are used to achieve simultaneous sterilization and removal by sterilizing and adsorbing antibiotic resistance genes at room temperature. The material is composed of chitosan and polyvinyl alcohol as film-forming agents, combined with long-chain quaternary ammonium salt modifications to form a composite film that can destroy bacterial cell membranes and adsorb antibiotic resistance genes.

Benefits of technology

It achieves a sterilization rate of more than 99% and an antibiotic resistance gene adsorption rate of more than 70% at normal temperature. It has a low loss rate and low energy consumption, avoids secondary pollution, and effectively removes antibiotic resistance genes inside and outside cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807701A_ABST
    Figure CN118807701A_ABST
Patent Text Reader

Abstract

The invention discloses a modified polyvinyl alcohol and chitosan composite membrane material for sterilizing and adsorbing antibiotic resistance genes and a preparation method, and belongs to the technical field of sewage treatment materials. The modified polyvinyl alcohol and chitosan composite membrane material is obtained by taking polyvinyl alcohol (PVA), chitosan (CS) and long-chain quaternary ammonium salt modified polyvinyl alcohol as raw materials, mixing, evaporating to dryness and uncovering a membrane. According to the composite membrane material, the composite membrane material is mixed with a bacterial solution at room temperature, the adsorbability of a cell membrane and a membrane to antibiotic resistance genes in a solution is destroyed through long-chain quaternary ammonium salt, the antibiotic resistance genes inside and outside cells can be effectively and synchronously removed, and the composite membrane material has the advantages of being simple in technology and free of secondary pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage treatment materials, and specifically relates to a modified polyvinyl alcohol and chitosan composite membrane material and a preparation method and application thereof. Background Art

[0002] Antibiotic resistance genes (ARGs) play a key role in the formation of superbugs, thus affecting the clinical therapeutic effect of antibiotics, posing a great threat and challenge to human public health. In recent years, antibiotic resistance genes have been considered as an emerging pollutant. Unlike conventional pollutants, antibiotic resistance genes are DNA fragments that encode antibiotic resistance proteins. There are two forms of existence: intracellular antibiotic resistance genes and extracellular antibiotic resistance genes. The two types of antibiotic resistance genes have different forms of transmission. Extracellular antibiotic resistance genes can exist stably in different environmental media for up to several months and enter competent cells existing under natural conditions through transformation; intracellular antibiotic resistance genes can amplify as the host microorganisms reproduce, and can also be transmitted between different microbial hosts by horizontal gene transfer mediated by mobile gene units.

[0003] However, traditional sewage treatment technology is designed for nutrients such as N and P in water bodies, and has little effect on the removal of antibiotic resistance genes. Traditional water treatment methods including chlorine, ozone and ultraviolet disinfection cannot effectively destroy antibiotic resistance genes, and will release antibiotic resistance genes into the environment by destroying the bacterial cell membrane. In addition, although 90% to 99% of microorganisms are effectively removed in treated urban sewage, the absolute number of bacteria is large, with the total coliform count between 104 and 105 / L, and there are pathogens and drug-resistant bacteria. Studies have shown that after recycled water is discharged into environmental water bodies, the abundance of antibiotic resistance genes in the receiving water body or soil environment increases. In the process of reclaimed water reuse, attention should be paid to its antibiotic resistance gene carrying situation to prevent recycled water from becoming a medium for the spread of antibiotic resistance genes.

[0004] Antibiotic resistance genes and competent bacteria carrying antibiotic resistance genes exist in water bodies such as medical wastewater and domestic wastewater, polluting the environment and endangering human health. Most of the existing methods destroy the cell membrane of pathogenic bacteria to achieve the purpose of removing pathogenic bacteria. The antibiotic resistance genes carried by the damaged bacterial cell membrane will be released into the water body and continue to endanger human health. Therefore, simultaneous sterilization and removal of antibiotic resistance genes are key. Patent applications with application numbers CN202311417225 and CN202311488893 report methods for sterilization and removal of antibiotic resistance genes. How to sterilize and remove antibiotic resistance genes efficiently and environmentally friendly has important practical significance and needs. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the object of the present invention is to design and provide a method for preparing a modified polyvinyl alcohol and chitosan composite membrane material and its application. The method of the present invention is based on a long-chain quaternary ammonium salt modified polyvinyl alcohol solution, and uses chitosan and polyvinyl alcohol solution as carriers to prepare a long-chain quaternary ammonium salt modified polyvinyl alcohol / chitosan composite membrane material. The material can sterilize pathogenic bacteria at room temperature, causing the cell membrane of pathogenic bacteria to rupture and die, and adsorbing the antibiotic resistance genes released into water by the death of pathogenic bacteria, thereby achieving synchronous sterilization and adsorption removal of antibiotic resistance genes in a relatively short time.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] On the one hand, the present invention provides a modified polyvinyl alcohol and chitosan composite membrane material, comprising a composite membrane material consisting of a polyvinyl alcohol and chitosan composite membrane and a long-chain quaternary ammonium salt modified polyvinyl alcohol membrane.

[0008] In a second aspect, the present invention provides a method for preparing the modified polyvinyl alcohol and chitosan composite film material, comprising the following steps:

[0009] (1) weighing chitosan solution and polyvinyl alcohol solution, controlling the temperature and stirring, adding a cross-linking agent (to enhance the film-forming property of the film solution), and then heating and stirring to obtain a polyvinyl alcohol and chitosan composite film solution; the chitosan and polyvinyl alcohol solutions are used as film-forming agents;

[0010] (2) weighing a polyvinyl alcohol solution, adding epichlorohydrin, adding a long-chain quaternary ammonium salt after high-temperature treatment, heating and stirring to load the quaternary ammonium salt, and obtaining a long-chain quaternary ammonium salt-modified polyvinyl alcohol membrane liquid;

[0011] (3) Weighing polyvinyl alcohol and chitosan composite membrane liquid and long-chain quaternary ammonium salt modified polyvinyl alcohol membrane liquid, stirring and mixing, and then ultrasonicating to make the membrane liquids evenly mixed, placing them in a culture dish, drying and peeling off the membrane to obtain a modified polyvinyl alcohol and chitosan composite membrane material.

[0012] In the preparation method, the controlled temperature in step (1) is 40-45° C.

[0013] The stirring time is 4 to 6 hours;

[0014] The heating and stirring conditions are: temperature 40-45°C, stirring time 4-6h;

[0015] The cross-linking agents are glutaraldehyde and glycerol;

[0016] The volume and mass ratio of the chitosan solution, the polyvinyl alcohol solution and the cross-linking agent is 100 mL:75 mL:3 g;

[0017] Preferably, the cross-linking agent is glutaraldehyde and glycerol, and the mass ratio of glutaraldehyde to glycerol is 1:5.

[0018] The preparation method of the chitosan solution in step (1) is as follows: weigh chitosan and stir at room temperature, dissolve it in acetic acid solution to prepare a chitosan solution;

[0019] The mass volume ratio of the chitosan to the acetic acid solution is 5-8 g:125-200 mL;

[0020] The concentration of the acetic acid solution is 2-5%.

[0021] The preparation method of the polyvinyl alcohol solution in step (1) is as follows: weigh polyvinyl alcohol, heat it at 90-95°C, stir it and dissolve it in water to prepare a 40g / L polyvinyl alcohol solution.

[0022] In the preparation method, the conditions for high temperature treatment in step (2) are: temperature 80-85° C., time 2-3 h;

[0023] The heating and stirring conditions are: temperature 80-85° C., time 3-4 h.

[0024] In the preparation method, the long-chain quaternary ammonium salt in step (2) is selected from one of NN-dimethyldodecylamine, NN-dimethyltetradecylamine or NN-dimethylhexadecylamine;

[0025] The volume ratio of the polyvinyl alcohol solution, epichlorohydrin and long-chain quaternary ammonium salt is 3:1-2:1-2.

[0026] In the preparation method, the stirring and mixing time in step (3) is 2 to 5 minutes;

[0027] The ultrasonic conditions are: time 30 to 60 minutes, repeated 3 to 5 times.

[0028] In the preparation method, the mass ratio of the polyvinyl alcohol and chitosan composite membrane liquid to the long-chain quaternary ammonium salt modified polyvinyl alcohol membrane liquid in step (3) is 1:7-10;

[0029] The drying conditions are: temperature 30-40° C., time 72-96 h.

[0030] In a third aspect, the present invention provides the modified polyvinyl alcohol and chitosan composite membrane material, or the modified polyvinyl alcohol and chitosan composite membrane material prepared by the method, for use in sterilization and adsorption of antibiotic resistance genes during sewage treatment.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. When treating sewage, the modified chitosan / polyvinyl alcohol composite membrane material of the present invention can simultaneously achieve sterilization and adsorption of antibiotic resistance genes in sewage.

[0033] 2. The present invention uses chitosan and polyvinyl alcohol as film-forming agents and quaternary ammonium salt as a modifier to prepare a chitosan / polyvinyl alcohol composite membrane material modified by a long-chain quaternary ammonium salt under the action of epichlorohydrin. It has structural advantages in sewage treatment.

[0034] 3. The modified chitosan and polyvinyl alcohol composite membrane material of the present invention can be applied to sewage treatment sterilization and adsorption of antibiotic resistance genes. At 37°C, the composite membrane material is mixed with the bacterial solution, and the cell membrane and the membrane's adsorption of antibiotic resistance genes in the solution are destroyed by long-chain quaternary ammonium salts. The composite material of the present invention can be used at room temperature, without additional heat, and can be achieved by oscillating and stirring. The reaction cycle is 24 hours, the sterilization rate is as high as more than 99%, and the composite membrane material has the advantages of low loss rate, low energy consumption, high efficiency, and no secondary pollution, which can effectively achieve simultaneous sterilization and removal of intracellular and extracellular antibiotic resistance genes. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a scanning electron microscope image of the 12C modified membrane material obtained in Example 1;

[0036] Figure 2 is the sterilization rate of the three membrane materials;

[0037] Figure 3 is the adsorption rate of antibiotic resistance genes by three membrane materials. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0039] Embodiment 1:

[0040] A method for preparing a modified polyvinyl alcohol and chitosan composite film material comprises:

[0041] (1) Weigh 4 g of chitosan and dissolve it in 100 mL of 2% acetic acid solution; then weigh 40 g of polyvinyl alcohol solution, dissolve it in water under heating and stirring at 95°C, and dilute to 1 L to prepare a 40 g / L polyvinyl alcohol solution; take 75 mL of polyvinyl alcohol solution and add it to 100 mL of chitosan solution, heat and stir at 40°C for 4 h, then add 2 g of glycerol and 0.5 g of 50% glutaraldehyde solution, continue heating and stirring for 4 h, and a composite membrane solution of polyvinyl alcohol and chitosan is obtained, which is recorded as PVA / CS.

[0042] (2) Take 75 mL of 40 g / L polyvinyl alcohol solution, add 12.5 mL of epichlorohydrin, heat to 85 ° C for 2 h, then add 12.5 mL of N-N-dimethyldodecylamine dropwise, heat to react for 3 h, and obtain a long-chain quaternary ammonium salt-modified polyvinyl alcohol solution, which is recorded as 12C-PVA.

[0043] (3) Take 2 mL of PVA / CS solution and 14 mL of 12C-PVA, vortex and oscillate for 2 min, and ultrasonicate for 30 min, repeat 3 times to fully mix the two, take 20 mL of the mixed solution and place it in a 90 mm culture dish, cover it with a film, heat it in an oven at 40°C for 72 h, then remove the film and wipe off the surface residue to obtain a modified polyvinyl alcohol and chitosan composite film material. The scanning electron microscopy of the composite film material is as follows Figure 1 shown.

[0044] Embodiment 2:

[0045] The other steps were the same as those in Example 1, except that the step (2) of "dropwise addition of 12.5 mL of N-N-dimethyldodecylamine" was changed to "dropwise addition of 12.5 mL of N-N-dimethyltetradecylamine".

[0046] Embodiment 3:

[0047] The other steps are the same as those in Example 1, except that the step (2) of "dropwise addition of 12.5 mL of N-N-dimethyldodecylamine" is changed to "dropwise addition of 12.5 mL of N-N-dimethylhexadecylamine".

[0048] Embodiment 4:

[0049] Take 0.1g, 0.3g and 0.5g of the modified polyvinyl alcohol and chitosan composite membrane materials of Examples 1, 2 and 3 respectively and add them to 100mL OD 600 = 1 in the E. coli liquid, and the control group was the E. coli liquid without the modified composite membrane material. After 24 hours of oscillation reaction at 37°C and 180rpm, 100uL of the liquid was taken and spread on the plate to observe the sterilization situation. Figure 2 As shown, the sterilization rates of the three modified polyvinyl alcohol and chitosan composite membrane materials of Examples 1, 2 and 3 are all above 90%. Among them, the sterilization rate of the long-chain quaternary ammonium salt modified polyvinyl alcohol / chitosan composite membrane material obtained in Example 1 reached 100% when the addition amount was 0.1g; the sterilization rate of the long-chain quaternary ammonium salt modified polyvinyl alcohol / chitosan composite membrane material obtained in Example 2 reached 100% when the addition amount was 0.3g; the sterilization rate of the long-chain quaternary ammonium salt modified polyvinyl alcohol / chitosan composite membrane material obtained in Example 3 reached 99% when the addition amount was 0.5g.

[0050] Embodiment 5:

[0051] Take 0.1g, 0.3g and 0.5g of the modified polyvinyl alcohol and chitosan composite membrane materials of Examples 1, 2 and 3 respectively and add them to 100mL OD 600 =1 in the competent E. coli liquid carrying the antibiotic resistance gene plasmid, and the control group was the E. coli liquid without the modified composite membrane material. After 24 hours of shaking reaction at 37°C and 180rpm, the liquid after the reaction was centrifuged and the supernatant was taken for qPCR detection to detect the gene concentration; 100uL of the liquid was taken for plate coating to observe the sterilization situation. The results are as follows Figure 3 As shown, the adsorption rate of the three membrane materials for the adsorption of antibiotic resistance genes reached more than 70%. Among them, 12C refers to the composite membrane material prepared in Example 1, 14C refers to the composite membrane material prepared in Example 2, and 16C refers to the composite membrane material prepared in Example 3.

[0052] Among them, the qPCR test method is: the sample preparation method of qPCR detection technology is as follows: the entire qPCR detection technology sample system is 20μL, and the reaction needs to use a 96-well PCR sample plate, wherein each system includes: 2μL sample DNA, 0.5μL upper primer (tetM-F, nucleotide sequence as shown in SEQ ID NO.1), 0.5μL lower primer (tetM-R, nucleotide sequence as shown in SEQ ID NO.2), 7μL ddH2O and 10μL SYBR Green PCR premix. After all samples are added, mix and centrifuge, and place on ice for testing. Each sample needs to be set up 3 parallels, and a set of negative controls needs to be set up as a whole. The qPCR instrument test program is set as follows: preheating 95℃, 150s, denaturation 94℃, 15s, extension 56℃, 30s, a total of 40 cycles. The nucleotide sequences of the primers are shown in Table 1 below.

[0053] Table 1 Basic information of primers used in the experiment

[0054]

Claims

1. A modified polyvinyl alcohol and chitosan composite film material, characterized in that: The composite membrane material is formed by using chitosan and polyvinyl alcohol as carriers and composite long-chain quaternary ammonium salt-modified polyvinyl alcohol on the carriers.

2. The method for preparing a modified polyvinyl alcohol and chitosan composite film material according to claim 1, characterized in that: The following steps are involved: (1) weighing an acetic acid solution of chitosan and an aqueous solution of polyvinyl alcohol, controlling the temperature and stirring, adding a crosslinking agent, and heating and stirring again to obtain a polyvinyl alcohol and chitosan composite membrane solution; (2) weighing an aqueous solution of polyvinyl alcohol, adding epichlorohydrin, heating at high temperature for reaction, adding a long-chain quaternary ammonium salt, heating and stirring, and obtaining a long-chain quaternary ammonium salt-modified polyvinyl alcohol film liquid; (3) Weighing polyvinyl alcohol and chitosan composite membrane liquid and long-chain quaternary ammonium salt modified polyvinyl alcohol membrane liquid, oscillating and mixing, and then sonicating, placing in a culture dish, drying and peeling off the membrane to obtain a modified polyvinyl alcohol and chitosan composite membrane material.

3. The preparation method according to claim 2, characterized in that: The controlled temperature in step (1) is 40-45°C; The stirring time is 4 to 6 hours; The heating and stirring conditions are: temperature 40-45°C, stirring time 4-6h; The cross-linking agents are glutaraldehyde and glycerol; The volume and mass ratio of the chitosan solution, the polyvinyl alcohol solution and the cross-linking agent is 100 mL:75 mL:3 g; Preferably, the cross-linking agent is glutaraldehyde and glycerol, and the mass ratio of glutaraldehyde to glycerol is 1:

5.

4. The preparation method according to claim 2, characterized in that: The preparation method of the chitosan solution in step (1) is as follows: weigh chitosan, stir at room temperature, and dissolve it in acetic acid solution to prepare a chitosan solution; The mass volume ratio of the chitosan to the acetic acid solution is 5-8 g:125-200 mL; The concentration of the acetic acid solution is 2-5%.

5. The preparation method according to claim 2, characterized in that: The preparation method of the polyvinyl alcohol solution in step (1) is as follows: weigh polyvinyl alcohol, heat it at 90-95° C., stir it, and dissolve it in water to prepare a 40 g / L polyvinyl alcohol solution.

6. The preparation method according to claim 2, characterized in that: The conditions of the high temperature treatment in step (2) are: temperature 80-85°C, time 2-3h; The heating and stirring conditions are: temperature 80-85° C., time 3-4 h.

7. The preparation method according to claim 2, characterized in that: The long-chain quaternary ammonium salt in step (2) is selected from one of NN-dimethyldodecylamine, NN-dimethyltetradecylamine or NN-dimethylhexadecylamine; The volume ratio of the polyvinyl alcohol solution, epichlorohydrin and long-chain quaternary ammonium salt is 3:1-2:1-2.

8. The preparation method according to claim 2, characterized in that: The stirring and mixing time in step (3) is 2 to 5 minutes; The ultrasonic conditions are: time 30 to 60 minutes, repeated 3 to 5 times.

9. The preparation method according to claim 2, characterized in that: The mass ratio of the polyvinyl alcohol and chitosan composite membrane liquid to the long-chain quaternary ammonium salt modified polyvinyl alcohol membrane liquid in step (3) is 1:7-10; The drying conditions are: temperature 30-40° C., time 72-96 h.

10. Use of the modified polyvinyl alcohol and chitosan composite membrane material according to claim 1, or the modified polyvinyl alcohol and chitosan composite membrane material prepared by the method according to any one of claims 2 to 9 in sterilization and adsorption of antibiotic resistance genes in sewage treatment.

Citation Information

Patent Citations

  • Application of chitosan and derivative thereof in reduction of antibiotic resistance gene pollution in soil

    CN113637481A

  • Synthetic method and application of degradable chitosan composite membrane material

    CN117285752A