Sargassum horneri carbon quantum dot / bismuth molybdate composite photocatalyst and application thereof

By combining copper algae-based carbon quantum dots with bismuth molybdate to form a composite photocatalyst, it solves the problem of insufficient response of BMO photocatalysts to visible light and achieves efficient degradation of ciprofloxacin and environmentally friendly treatment effects.

CN118807730APending Publication Date: 2024-10-22ZHEJIANG OCEAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410705341.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing bismuth molybdate (BMO) photocatalysts have a low response range to visible light and insufficient charge carrier loading rates, making it difficult to effectively degrade ciprofloxacin in aqueous environments.

Method used

Copper algae-based carbon quantum dots (SCQD) were prepared using a low-cost hydrothermal method, and were combined with BMO through a solvothermal method to form a copper algae carbon quantum dot/bismuth molybdate composite photocatalyst (SCQD/BMO) to improve photocatalysis active.

Benefits of technology

It achieves efficient degradation of ciprofloxacin, has higher photogenerated carrier separation efficiency and faster electron transmission rate, does not produce additional toxic substances, and avoids secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention relates to the technical field of medicines, in particular to a sargassum horneri carbon quantum dot / bismuth molybdate composite photocatalyst and application thereof. The SCQD is uniformly loaded on the surface of the BMO, when the SCQD doping ratio is 0.75% (0.75 CB), the prepared sample has the highest photocatalytic degradation effect, and the 0.75 CB has higher photon-generated carrier separation efficiency and higher electron transmission rate than the BMO, has the forbidden band width of 2.78 eV and has better absorption efficiency on visible light. In-vitro cell experiments show that no extra toxic species are generated in the degradation process of ciprofloxacin, and no secondary pollution is caused.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of medical technology, and in particular to a copper algae carbon quantum dot / bismuth molybdate composite photocatalyst and application thereof. Background Art

[0002] Carbon quantum dots (CQDs) are a new type of zero-dimensional fluorescent carbon nanomaterial, composed of quasi-spherical carbon nanoparticles with a size less than 10nm. Compared with traditional semiconductor quantum dots (QDs), CQDs have many advantages such as small molecular weight, low toxicity, diverse raw material sources, low cost, high fluorescence stability, adjustable emission wavelength, and good biocompatibility. As a traditional semiconductor photocatalyst, Bi2MoO6 (BMO) has the advantages of non-toxicity, simple preparation, and cheap raw materials. However, BMO has problems such as a low visible light response range and a high charge carrier load rate. Summary of the invention

[0003] The present invention uses low-value copper algae as raw materials, adopts a green and low-cost hydrothermal method to prepare copper algae-based carbon quantum dots (SCQDs), and then uses a solvothermal method to compound SCQDs with BMO to prepare copper algae-based carbon quantum dots / bismuth molybdate composite photocatalysts (SCQD / BMO, CB) with high photocatalytic activity, which are used to degrade ciprofloxacin (CIP) in water environments.

[0004] In one aspect, the present invention provides a method for preparing a copper algae carbon quantum dot / bismuth molybdate composite photocatalyst, which comprises the following steps:

[0005] 1) Pretreatment of copper algae: Use deionized water to repeatedly wash the copper algae, place the washed copper algae in an oven to dry, crush, sieve, take the copper algae powder in a beaker, add deionized water, use an ultrasonic crusher in an ice bath, and obtain a copper algae homogenate;

[0006] 2) Preparation of copper algae-based carbon quantum dots: The copper algae homogenate prepared above was transferred to a tetrafluoroethylene liner, placed in a high-pressure reactor, hydrothermally pyrolyzed, the obtained pyrolysis liquid was centrifuged, the supernatant was filtered with a 0.22 μm needle filter, and dialyzed. After the dialysis, the liquid in the dialysis bag was frozen in a refrigerator, and dried with a freeze dryer to obtain copper algae-based carbon quantum dots (SCQD);

[0007] 3) Na2MoO4·2H2O and Bi(NO3)3·5H2O were added to two beakers respectively, ethylene glycol was added respectively and stirred on a magnetic stirrer until completely dissolved, Na2MoO4·2H2O was added dropwise to Bi(NO3)3·5H2O, and different masses of SCQDs and anhydrous ethanol were added, and after stirring, the mixed solution was transferred to a tetrafluoroethylene liner for hydrothermal reaction, the reaction product was filtered through a filter membrane, repeatedly washed with water and anhydrous ethanol, and dried to obtain the copper algae carbon quantum dots / bismuth molybdate composite photocatalyst 0.75CB.

[0008] Preferably, in step 1), the weight volume ratio of copper algae to deionized water is 0.5 g:50 ml.

[0009] Preferably, in step 2), the volume ratio of copper algae homogenate to tetrafluoroethylene is 1:2.

[0010] Preferably, the hydrothermal decomposition temperature in step 2) is 220° C. and the hydrolysis time is 18 h.

[0011] Preferably, the dialysis process in step 2) is to transfer the filtrate to a dialysis bag with a molecular weight of 1000 and dialyze for 24 hours, with the deionized water being replaced every 8 hours.

[0012] Preferably, in step 3), the weight ratio of Na2MoO4·2H2O to Bi(NO3)3·5H2O is 0.195g:0.780g.

[0013] Preferably, in step 3), the volume ratio of Na2MoO4·2H2O to ethylene glycol is 0.195 g:20 ml, and the volume ratio of Bi(NO3)3·5H2O to ethylene glycol is 0.780 g:20 ml.

[0014] Preferably, in the step 3), the weight ratio of Na2MoO4·2H2O to SCQD is 0.195 g:3.8 mg, and the weight-volume ratio of SCQD to anhydrous ethanol is 3.8 mg:30 mL.

[0015] Preferably, in step 3), the volume ratio of anhydrous ethanol to tetrafluoroethylene is 30 ml:100 ml.

[0016] Preferably, the hydrothermal reaction temperature in step 3) is 160° C., and the hydrothermal reaction time is 12 h.

[0017] On the other hand, the present invention provides a copper algae carbon quantum dot / bismuth molybdate composite photocatalyst prepared by the above method.

[0018] On the other hand, the present invention provides the use of the copper algae carbon quantum dots / bismuth molybdate composite photocatalyst in the degradation of ciprofloxacin (CIP).

[0019] Furthermore, the conditions for degrading ciprofloxacin (CIP) are: 0.75CB dosage is 0.5 g / L, CIP concentration is 0.01 g / L, degradation time is 180 min, and pH=7.0.

[0020] The present invention prepares SCQD / BMO composite photocatalysts with different SCQD doping ratios by a solvothermal method, and uses scanning electron microscopy (SEM), transmission electron microscopy (TEM), X-ray diffraction (XRD), specific surface area test (BET), Fourier transform infrared absorption spectroscopy (FTIR), X-ray photoelectron spectroscopy (XPS), ultraviolet visible diffuse reflectance spectroscopy (UV-vis DRS), electrochemical impedance spectroscopy (EIS), photoluminescence spectroscopy (PL) and other characterization methods to analyze the morphological structure, crystal phase composition, pore size characteristics, surface functional groups, chemical element state, element composition, optical properties, electrochemical properties and other physical and chemical properties; and investigates the effects of photocatalyst dosage, CIP initial concentration and pH on the CIP degradation performance of 0.75CB through batch degradation experiments. The results show that SCQD is uniformly loaded on the surface of BMO. The sample prepared when the SCQD doping ratio is 0.75% (0.75CB) has the highest photocatalytic degradation effect. 0.75CB has a higher photogenerated carrier separation efficiency and faster electron transfer rate than BMO, with a bandgap width of 2.78eV and good absorption efficiency for visible light. In vitro cell experiments show that no additional toxic substances are produced during the degradation of ciprofloxacin, and no secondary pollution will be caused. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 SEM images of 0.5CB, 0.75CB, 1.0CB and BMO.

[0022] Figure 2 The element distribution diagram and EDS energy spectrum of the 0.75CB sample.

[0023] Figure 3 TEM image of the 0.75CB sample.

[0024] Figure 4 BET curves and pore size distribution diagrams of 0.5CB, 0.75CB, and 1.0CB.

[0025] Figure 5 FT-IR images of 0.5CB, 0.75CB, 1.0CB and BMO.

[0026] Figure 6 These are the XRD phase analysis results of 0.5CB, 0.75CB, 1.0CB and BMO samples.

[0027] Figure 7 Surface element composition and electrochemical state of 0.5CB, 0.75CB, 1.0CB and BMO.

[0028] Figure 8 PC and EIS images of 0.75CB and BMO samples.

[0029] Fig. 9 (a) The photocatalytic degradation effect of CIP by different catalysts 0.5CB, 0.75CB, 1.0CB and BMO.

[0030] Fig. 9 (b) The degradation kinetics curves of CIP by each catalyst.

[0031] Fig.10 The effect of 0.75CB on the initial concentration of CIP in the CIP degradation system was tested and analyzed.

[0032] Fig.11 The effect of 0.75CB on the pH in the CIP degradation system was tested and analyzed.

[0033] Fig.12 The effect of 0.75CB on the amount of photocatalyst in the CIP degradation system was tested and analyzed.

[0034] Fig.13 A cyclic degradation experiment was carried out for 0.75CB.

[0035] Fig.14 The degradation rate of CIP by 0.75CB in the presence of different quenchers.

[0036] Fig.15 This is the degradation pathway of ciprofloxacin by KSBC.

[0037] Fig.16 Toxicity analysis of intermediate products of BMO. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below with reference to the accompanying drawings. The abbreviations used in the present invention are as follows:

[0039] CIP: ciprofloxacin;

[0040] SCQD: copper algae-based carbon quantum dots;

[0041] BMO: bismuth molybdate;

[0042] CB: SCQD / BMO, copper algae-based carbon quantum dots / bismuth molybdate composite photocatalyst;

[0043] Copper algae were purchased from Wuzhoufeng Agricultural Technology Co., Ltd.

[0044] Example 1 Preparation of copper algae-based carbon quantum dots

[0045] (1) Pretreatment of copper algae: Use deionized water to wash the copper algae repeatedly for 3-4 times, and remove large impurities at the same time. Place the washed copper algae in an oven at 80°C and dry for 24 hours. After intermittent crushing by a grinder for 4 times, use a 100-mesh standard sieve to sieve and obtain 100-mesh copper algae powder. Take 0.5g of copper algae powder in a beaker, add 50mL of deionized water, and use an ultrasonic crusher to crush in an ice bath for 180min, ultrasonicate for 3s each time, and take 2s intervals to obtain 50mL of copper algae homogenate.

[0046] (2) Preparation of copper algae-based carbon quantum dots: The copper algae homogenate prepared above was transferred to a 100 mL tetrafluoroethylene liner, placed in a high-pressure reactor, and hydrothermally pyrolyzed at 220°C for 18 hours. The obtained pyrolysis solution was centrifuged at 10,000 r / min for 15 minutes, the supernatant was filtered with a 0.22 μm needle filter, and the filtrate was transferred to a 1000 molecular weight dialysis bag for 24 hours, and the deionized water was replaced every 8 hours. After the dialysis, the liquid in the dialysis bag was frozen in a refrigerator for 12 hours, and finally dried in a freeze dryer for 48 hours to obtain copper algae-based carbon quantum dots (SCQD).

[0047] Example 2 Preparation of copper algae-based carbon quantum dots / bismuth molybdate composite photocatalyst

[0048] 0.195g of Na2MoO4·2H2O and 0.780g of Bi(NO3)3·5H2O were added to two beakers, 20mL of ethylene glycol was added to each beaker and stirred on a magnetic stirrer until completely dissolved. Na2MoO4·2H2O was added dropwise to Bi(NO3)3·5H2O, and different masses of SCQD (2.0, 3.8, 5.0mg) and 30mL of anhydrous ethanol were added. After stirring for 30min, the mixture was transferred to a 100mL tetrafluoroethylene liner and subjected to a hydrothermal reaction at 160℃ for 12h. The reaction product was filtered using a 0.45μm filter membrane in a sand core funnel, washed repeatedly with water and anhydrous ethanol for 3-4 times, and dried at 60℃ to obtain composite materials modified with different mass fractions of SCQD, which were named 0.5CB, 0.75CB, and 1.0CB, respectively.

[0049] Example 3 Characterization of copper algae-based carbon quantum dots / bismuth molybdate composite photocatalyst

[0050] The microscopic morphology, crystal structure, functional groups, and surface element composition of BMO, 0.5CB, 0.75CB, and 1.0CB were characterized. The microscopic morphology of BMO, 0.5CB, 0.75CB, and 1.0CB samples was observed by scanning electron microscopy (SEM), and the 0.75CB sample was scanned by EDS-mapping to observe the uniformity of the distribution of the five elements C, N, O, Bi, and Mo on the sample surface; high-resolution imaging was provided by high-power transmission electron microscopy (HRTEM), and the morphology, structure, atomic arrangement, etc. of the 0.75CB sample were observed, and the exposed crystal plane was analyzed based on the lattice fringe spacing; the specific surface area and pore size distribution characteristics of the 0.5CB, 0.75CB, and 1.0CB samples were analyzed by a specific surface area analyzer, and the samples were placed in a vacuum chamber and pre-degassed at a temperature of 150°C for 24 hours. In a constant low temperature environment (77K), the adsorption and desorption of nitrogen by the samples were measured, the specific surface area of ​​the samples was calculated by the Barrett-Emmett-Teller (BET) method, and the pore size distribution of the samples was calculated by the Barrett-Joyner-Halanda (BJH) model. The absorption of infrared light of different wavelengths by BMO, 0.5CB, 0.75CB, and 1.0CB samples was measured by Fourier transform infrared spectroscopy (FTIR) to determine the chemical bonds and functional groups present in the samples. The powder samples were evenly ground with potassium bromide (the mass ratio of the sample to potassium bromide was 100:1) by the potassium bromide tableting method, and then pressed into a thin sheet to be tested on a tableting machine, and then heated at 4000-400cm -1 The test was carried out in the range of 100 nm; X-ray diffractometer (XRD) was used to measure the Cu-K radiation (wavelength )BMO, 0.5CB, 0.75CB, 1.0CB samples were scanned in the range of 2θ=10-85° to analyze their phase states; X-ray photoelectron spectroscopy (XPS) was used to determine the types of elements, element valence states, surface energy states, etc. present in 0.5CB, 0.75CB, 1.0CB and BMO samples according to the positions of characteristic spectral lines in the spectrum. The photocurrent (PC) and electrochemical impedance spectroscopy (EIS) of the composite materials were analyzed and tested by an electrochemical workstation. The test conditions were: using Pt electrode and Ag / AgCl electrode as the counter electrode and reference electrode respectively, and FTO conductive glass (1cm×1cm) as the working electrode, at 0.1mol / L The working electrode was prepared by weighing 5 mg of the catalyst, adding 1 mL of ethanol solution and 20 μL of naphthol (Nafion) solution, ultrasonicating for 30 min until the catalyst was evenly dispersed, and spin-coating 10 μL of the prepared solution on the FTO glass with a pipette to dry it, and spin-coating it again for 5-6 times; the light absorption properties of BMO, 0.5CB, 0.75CB, and 1.0CB samples were analyzed using a solid-state UV-visible diffuse reflectance spectrometer (DRS). Before the test, the samples were compacted in the sample tank, with BaSO4 as a reference, and the measurement band was 800-200 nm; the electronic transition and recombination process of BMO, 0.5CB, 0.75CB, and 1.0CB samples were analyzed using a steady-state fluorescence spectrum (PL) at an excitation wavelength of 296 nm, and the results are as follows:

[0051] Figure 1 The SEM images of 0.5CB, 0.75CB, 1.0CB and BMO show that the 0.5CB, 0.75CB and 1.0CB samples show a three-dimensional flower ball structure composed of nanorods with a particle size of about 1μm, while BMO has a three-dimensional flower ball structure composed of nanosheets and nanorods. The flower-like surface morphology is due to the fact that the ethylene glycol solvent inhibits their inherent anisotropic growth. These nuclei have different levels of BMO nanostructures during the solvent thermal reaction. The introduction of SCQD may have changed the crystal structure of some BMO, changing it from nanosheets to nanorods. Due to the tiny particle size of SCQD (2-4.5nm), it is difficult to directly observe it in each sample.

[0052] Figure 2 The element distribution diagram and EDS energy spectrum diagram of the 0.75CB sample. 0.75CB is composed of five elements: C, N, O, Bi, and Mo. The C and N elements contained in SCQD are evenly distributed on BMO without agglomeration. The weight ratio and atomic ratio of each element are shown in Table 1. The atomic ratio of Bi and Mo in the sample is less than 2:1, which indicates that Bi may be lost during the preparation process.

[0053] Table 1 shows the results of EDS quantitative analysis.

[0054]

[0055] Figure 3 This is the TEM image of the 0.75CB sample. The nanorod-like structures clustered on the sample surface can be magnified and the lattice fringe spacings are 0.2772nm and 0.3158nm, corresponding to the (-2 3 1) crystal plane and (0 32) crystal plane of γ-BMO, respectively, proving the existence of γ-BMO in the composite material.

[0056] Figure 4 The BET curves and pore size distribution diagrams of 0.5CB, 0.75CB, and 1.0CB are shown below. Figure 4 (a) It can be seen that the three samples have a hysteresis loop at P / P0=0.7, and the N2 adsorption-desorption isotherms of the three samples belong to type IV isotherms. Figure 4 It can be seen that the three samples are mainly mesopores. Table 2 shows the specific surface area, pore volume and pore size of the three samples. It can be seen that 0.75CB has the largest specific surface area, pore volume and pore size.

[0057] Table 2 Specific surface area, pore volume and pore size of different samples

[0058]

[0059] Figure 5 FT-IR images of 0.5CB, 0.75CB, 1.0CB and BMO. The 500-1000cm -1 The characteristic strong absorption peaks between them are attributed to the stretching vibration and deformation vibration of Bi-O and Mo-O. The FT-IR spectra of the four samples are very similar, and compared with the pure BMO sample, the peak intensity of the 1.0CB sample is weakened due to the large amount of Bi 3+ After adding SCQDs, it is difficult to observe the appearance of new absorption peaks in the FT-IR spectrum. This may be due to the low addition amount of SCQDs. However, at 1735 cm -1 With 1460cm -1 By zooming in, weak absorption peaks were found that may be caused by SCQD, which were attributed to the absorption peaks of C=O and -COO - This also indicates that there is electronic coupling between the interface of SCQD and BMO.

[0060] Figure 6These are the XRD phase analysis results of 0.5CB, 0.75CB, 1.0CB and BMO samples. All samples have strong diffraction peaks at around 28.1°, 32.5°, 46.6°, and 55.5°, corresponding to the (131), (2 0 0), (2 0 2), and (1 3 3) crystal planes in the γ-BMO standard card PDF#21-0102, respectively, proving that the γ-BMO was successfully prepared. No diffraction peaks of SCQD were observed in the spectrum, which may be due to the low amount of SCQD added. However, obvious diffraction peaks were observed at 27.1°, 37.9°, and 39.8° in the 1.0CB, 0.75CB, and 0.5CB samples, corresponding to the (0 12), (1 0 4), and (1 1 0) crystal planes in the Bi standard card PDF#85-1329, respectively. Among them, the Bi diffraction peak of the 1.0CB sample is the strongest. Compared with the XRD spectrum of BMO, it can be seen that ethylene glycol and ethanol will not reduce the Bi in the material. 3+ This is because SCQD has a reducing property, which can reduce Bi 3+ It is reduced to Bi element, and after the Bi element is generated, only part of the Bi element is deposited on the surface of the material, resulting in a decrease in the atomic ratio of Bi and Mo, which is consistent with the conclusion in EDS. At the same time, the generation of a large amount of Bi element may block the pores of the material and reduce the specific surface area of ​​the material.

[0061] Figure 7 The surface element composition and electrochemical state of 0.5CB, 0.75CB, 1.0CB and BMO are shown in Table 1. Figure 7 In (a), elements such as O, Bi, Mo, and C were found on the sample surface, and the measured binding energy was corrected based on the binding energy of C1s, 284.8 eV. Figure 7 (b) is the detailed spectrum of Bi4f of the four samples. The two strong peaks around 159.3 eV and 164.6 eV are attributed to the oxidized Bi in the BMO of the four samples. 3+ It is worth noting that weak peaks of Bi were observed around 155.9 eV and 161.2 eV in the three SCQD / BMO composite samples, proving that Bi 3+ was reduced to simple Bi, but no peak of simple Bi was found in the Bi4f fine spectrum of pure BMO, which can be inferred that 3+ It is SCQD rather than ethylene glycol and ethanol that plays a reducing role, which is consistent with the conclusion of FT-IR analysis. In addition, since the amount of SCQD added is the highest in 1.0CB, the characteristic peak intensity of Bi element is also the highest, which is consistent with the results of XRD. Figure 7 (c) is the fine spectrum of Mo3d, and Mo3d is found near 235.3eV and 232.2eV in all samples. 3 / 2and Mo3d 5 / 2 The peak at 231.2 eV and 234.0 eV is attributed to the orthorhombic phase of γ-BMO, while the two broad peaks at 231.2 eV and 234.0 eV correspond to the cubic phase of BMO. The impure orthorhombic phase of γ-BMO in the composite sample may be caused by two reasons. On the one hand, SCQD converts Bi 3+ Reduction to Bi element, resulting in nBi 3+ / nMo 6+ On the other hand, studies have shown that the pH during the synthesis process affects the crystal phase of BMO, and γ-BMO is more easily obtained at high pH values. Since the surface of SCQD is rich in oxygen-containing functional groups such as carboxyl and hydroxyl groups, the addition of SCQD may lead to a decrease in the pH of the system. At the same time, SCQD reduces Bi 3+ , which may aggravate the decrease in pH value, resulting in the generation of impure orthorhombic γ-BMO at low pH. It is worth noting that the ratio of the peak area of ​​orthorhombic Mo and cubic Mo in the 1.0CB sample is the smallest, which means that there are more cubic BMO in the 1.0CB sample, which will affect its Aurivillius structure and band structure, resulting in a significant decrease in the photocatalytic performance. Figure 7 (d) is the fine spectrum of O1s. The peaks at 529.9 eV and 531.0 eV correspond to Bi-O and Mo-O, indicating that the oxidation state Mo 6+ The characteristic peak of lattice oxygen may be included in the Mo-O peak. In addition, the OH found in 1.0CB may be caused by the sample absorbing water. In addition, the O1s spectrum of the composite sample moves toward the direction of small binding energy as a whole, indicating that the addition of SCQD increases the electron cloud density of the composite material.

[0062] Figure 8 PC and EIS images of 0.75CB and BMO samples. Figure 8 (a) is the PC spectra of 0.75CB and BMO samples. It can be seen that the photocurrent response intensity of 0.75CB is higher than that of BMO. Figure 8 The radius of 0.75CB in (b) is also smaller than that of BMO, which indicates that 0.75CB has higher photogenerated carrier separation efficiency and faster electron transfer rate than BMO.

[0063] Example 4 Experiment on degradation of CIP by copper algae-based carbon quantum dots / bismuth molybdate composite photocatalyst

[0064] At room temperature, 20 mg CB was weighed and added to 100 mL of 20 mg / L CIP solution. The solution was protected from light for 30 min to reach a dynamic equilibrium of dark adsorption. Subsequently, the xenon lamp was turned on to simulate light exposure on the CIP system. 1 mL of sample was taken at fixed time points (5, 10, 20, 30, 40, 50, 60, 90, 120, and 180 min) and filtered with a 0.22 μm filter membrane. The absorbance of the sample solution was measured at 277 nm using a UV spectrophotometer, and the concentration of the solution was calculated.

[0065] After each photocatalytic degradation of ciprofloxacin (180 min), the catalyst in the solution was recovered, washed with anhydrous ethanol and deionized water and dried, and then used in the next photocatalytic degradation experiment. The cycle was repeated three times, and the photocatalytic degradation performance was measured each time. The changes in photocatalytic activity were compared and the photocatalytic stability was analyzed.

[0066] Example 5 Photocatalytic degradation performance of different materials

[0067] The photocatalytic degradation effects of different catalysts 0.5CB, 0.75CB, 1.0CB and BMO on CIP were analyzed and compared. Fig. 9 (a) As shown. 0.75CB has an excellent degradation effect on CIP. The degradation rate of CIP reaches 83.3% at 180 min. In the dark reaction stage, due to the low adsorption performance caused by the low specific surface area of ​​the material, only a small amount of CIP is adsorbed, indicating that the degradation of CIP is mainly photocatalytic degradation. Comparing the four materials, the degradation effect is 0.75CB>0.5CB>BMO>1.0CB. This may be due to the large amount of Bi contained in the 0.5CB and 1.0CB samples. On the one hand, too much Bi occupies too many adsorption sites, resulting in a decrease in the adsorption performance of the sample and a reduction in photocatalytic active sites. On the other hand, too much Bi is easy to agglomerate into a recombination center of photogenerated carriers, increasing the recombination rate of electrons and holes and reducing their chances of participating in photocatalytic reactions; the impure orthorhombic phase of 0.5CB and 1.0CB will also significantly reduce their photocatalytic activity. Fig. 9 (b) The degradation rate constants of CIP by each catalyst are 0.0064 min, 0.5 CB, 0.75 CB, 1.0 CB and BMO, respectively. -1 , 0.0092min -1 , 0.0041min -1 , 0.0035min -1 , the 0.75CB sample showed the fastest degradation rate.

[0068] Example 6 Effect of initial CIP concentration on degradation effect

[0069] The effect of 0.75CB on the initial concentration of CIP was tested and analyzed. The results are as follows Fig.10 As shown in the figure, when the CIP concentration gradually increased from 10 mg / L to 30 mg / L, the degradation rate decreased from 97.7% to 67.7%. This is because the increase in CIP concentration will increase the intermediate products produced during its degradation process. At the same time, the low specific surface area provides limited photocatalytic active sites, which will lead to continuous occupation of active sites, continuous accumulation of intermediate products, and affect the transmittance of the solution.

[0070] Example 7 Effect of pH on Degradation Effect

[0071] The effect of 0.75CB on the pH in the CIP degradation system was tested and analyzed. The results are as follows Fig.11 As shown in the figure, the amino groups containing piperazine and quinol structures in CIP are important factors affecting the photocatalytic reaction. The isoelectric point of CIP is pH = 7.4. In the pH range of 7-9, the photocatalytic degradation of CIP is related to zwitterions. When the CIP in the solution is positively or negatively charged as a whole, the degradation intermediates and pathways of CIP may be affected, reducing the degradation rate.

[0072] Example 8 Effect of Photocatalyst Dosage on Degradation Effect

[0073] The effect of the amount of photocatalyst added in the CIP degradation system was tested and analyzed using 0.75CB. The results are as follows: Fig.12 As shown in the figure, with the increase of the dosage of photocatalyst, the degradation efficiency of CIP generally shows an increasing trend. When the dosage reaches 50 mg, the degradation efficiency of CIP by the photocatalyst is increased to 93.2%. This is because the increase in the dosage of photocatalyst increases the number of photocatalytic active sites, thereby improving the degradation efficiency of CIP.

[0074] Example 9 Cyclic degradation experiment

[0075] The cyclic degradation experiment was carried out using 0.75CB. The results are as follows Fig.13 As shown, the degradation rates of the three cycles were 78.5%, 74.7% and 74.3% respectively. After three cycles, the degradation rate of 0.75CB for CIP still reached 74% within 180 min, indicating that the composite photocatalyst has good stability, but the loss during the sample recovery process leads to a continuous decrease in the degradation effect.

[0076] Example 10 Free Radical Capture Experiment

[0077] In 50mL of 20mg / L CIP solution, 10mg of 0.75CB was added, and the photocatalytic degradation of CIP was carried out at room temperature. Benzoquinone (BQ), sodium ethylenediaminetetraacetate (EDTA-2Na), isopropyl alcohol (IPA) and silver nitrate (AgNO3) were used as O2 ·- 、h + , OH and e - The concentration of the capture agent was 100 mmol / L and the amount added was 2 mL.

[0078] Fig.14 The degradation rate of CIP by 0.75CB in the presence of different quenchers is shown in Figure 2. After adding IPA and EDTA-2Na, the degradation rate of CIP by 0.75CB did not change significantly, but after adding AgNO3 and BQ, the degradation of CIP was significantly inhibited. The inhibition of CIP degradation by different free radical quenchers is AgNO3>BQ>IPA>EDTA-2Na, which indicates that the free radical that plays the main role in the photodegradation of CIP is e - and O2 - .

[0079] Example 11 Analysis of Degradation Intermediate Products

[0080] In order to conduct a specific analysis of the products produced during the photocatalytic degradation process, 1 mL of samples were taken at degradation times of 0, 90, and 180 min and filtered using a 0.22 μm filter membrane. The substances contained in the obtained sample solution were analyzed by liquid chromatography-mass spectrometry (LC-MS).

[0081] Fig.15 This is the degradation pathway of ciprofloxacin by KSBC. In pathway I, the CIP molecule is continuously attacked by the active groups in the piperazine ring, resulting in the ring opening to form P1 (m / z=362), followed by the attack of CN in the ring opening to convert it into a monoaldehyde derivative P2 (m / z=334). Under the continuous attack of the active groups, P3 (m / z=291, P4 (m / z=263), and finally P5 (m / z=245) are obtained; in pathway II, CIP is attacked by the active groups to convert its pyridine ring into , F bond, and carboxyl group break to generate P7 (m / z=228), which is then opened to form P8 (m / z=114). In path III, the cyclopropyl group in CIP is destroyed and substitution occurs on the piperazine ring to generate P9 (m / z=352). Then the piperazine ring and cyclopropyl group are opened to generate intermediates P9 (m / z=239) and P10 (m / z=179). Finally, the quinolone ring (C=C) is attacked by the generated free radical to form P11 (m / z=110).

[0082] Example 12 Evaluation of cytotoxicity of degradation intermediates

[0083] Cell recovery

[0084] L929 mouse fibroblast culture medium: MEM+10% FBS+1% (Penicillin-Streptomycin Solution).

[0085] (1) Take out L929 mouse fibroblasts from liquid nitrogen and quickly transfer them to a preheated 37°C water bath. Gently shake the cryovial to accelerate the dissolution of the cryopreservation solution.

[0086] (2) After the cryopreservation solution is completely dissolved, transfer the cells to a centrifuge tube containing 5 mL of culture medium and centrifuge at 1000 rpm for 5 min at room temperature. After centrifugation, discard the supernatant;

[0087] (3) The cells were suspended in a complete medium for L929 mouse fibroblasts containing 10% FBS, inoculated into a culture dish and gently blown to ensure that the cells were evenly distributed. The culture dish was placed at 18-20° C., 100% AIR, and saturated humidity for culture.

[0088] Cell passaging

[0089] When the cell density reaches 80%, the cells are passaged:

[0090] (1) Discard the culture medium and wash once with PBS;

[0091] (2) Add 1-2 mL of 0.25% trypsin solution to digest the cells. Observe under a microscope. After digestion for 1-2 min, the cells gradually separate and become round, indicating that the digestion process is complete.

[0092] (3) Rapidly remove the trypsin solution, add complete culture medium, blow the cells to evenly disperse the cells in the culture medium to form a single cell suspension, subculture at a ratio of 1:2, and expand the cell culture at a temperature of 18-20°C, 100% AIR and saturated humidity.

[0093] Cell treatment

[0094] (1) Take L929 mouse fibroblasts in the logarithmic growth phase and in good growth condition, and add 5×10 3 The cells were inoculated into a 96-well cell culture plate at a density of 100 μL and placed in an incubator at 18-20°C and 100% AIR for overnight culture; (100 μL of sterile PBS was added to the wells around the cell wells)

[0095] (2) Treat the cells according to the groups in Table 3:

[0096] Table 3 Cell grouping

[0097]

[0098] The samples were diluted to corresponding concentrations using cell culture medium, and the drugs at each concentration were incubated with the cells for 24 h.

[0099] Cell CCK8 detection

[0100] (1) After the cell culture reaches the required time point, the culture medium is replaced with a clean culture medium to eliminate the color interference of residual drugs on subsequent experiments. Fresh complete culture medium containing 10% CCK8 is added to each well, and the total volume of the culture medium is 100 μL. The cells are placed in an environment of 18-20°C and continue to be cultured for 2 hours;

[0101] (2) Use an OD450 microplate reader to measure the absorbance of each well.

[0102] According to the evaluation criteria for cytotoxicity of medical products (Table 4), the experimental results were compared and analyzed.

[0103] Table 4 Evaluation criteria for in vitro cytotoxicity test

[0104]

[0105]

[0106] Fig.16 The toxicity analysis of the intermediate products of BMO showed that when the degradation time reached 10 min, the cell survival rate of L929 was 99.66%, with no cytotoxicity; when the degradation time was 20, 40, 80, and 160 min, the cell survival rates were 98.75%, 91.55%, 97.15%, and 94.91%, respectively, all with slight cytotoxicity. It can be seen that when the degradation is approaching the end, the degradation intermediate products of BMO to CIP are still slightly cytotoxic; Fig.16 (b) Toxicity analysis of the intermediate product of 0.75CB shows slight cytotoxicity only when the degradation time is 40 min, and there is no cytotoxicity at other times. When the degradation is near the end, the intermediate product is still non-cytotoxic, which indicates that for the photocatalytic degradation of CIP, the biosafety of 0.75CB is higher than that of BMO and is not easy to cause secondary pollution.

[0107] Finally, it should be noted that the above is only a specific embodiment of the present invention. Obviously, the present invention is not limited to the above embodiment, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.

Claims

1. A method for preparing a copper algae carbon quantum dot / bismuth molybdate composite photocatalyst, characterized in that: The following steps are involved: 1) Pretreatment of copper algae: Use deionized water to repeatedly wash the copper algae, place the washed copper algae in an oven to dry, crush, sieve, take the copper algae powder in a beaker, add deionized water, use an ultrasonic crusher in an ice bath, and obtain a copper algae homogenate; 2) Preparation of copper algae-based carbon quantum dots: The copper algae homogenate prepared above was transferred to a tetrafluoroethylene liner, placed in a high-pressure reactor, hydrothermally pyrolyzed, the obtained pyrolysis liquid was centrifuged, the supernatant was filtered with a 0.22 μm needle filter, and dialyzed. After the dialysis, the liquid in the dialysis bag was frozen in a refrigerator, and dried with a freeze dryer to obtain copper algae-based carbon quantum dots (SCQD); 3) Na2MoO4·2H2O and Bi(NO3)3·5H2O were added to two beakers respectively, ethylene glycol was added respectively and stirred on a magnetic stirrer until completely dissolved, Na2MoO4·2H2O was added dropwise to Bi(NO3)3·5H2O, and different masses of SCQDs and anhydrous ethanol were added, and after stirring, the mixed solution was transferred to a tetrafluoroethylene liner for hydrothermal reaction, the reaction product was filtered through a filter membrane, repeatedly washed with water and anhydrous ethanol, and dried to obtain the copper algae carbon quantum dots / bismuth molybdate composite photocatalyst 0.75CB.

2. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: In the step 1), the weight volume ratio of copper algae to deionized water is 0.5 g:50 ml.

3. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: In the step 2), the volume ratio of the copper algae homogenate to tetrafluoroethylene is 1:

2.

4. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: The hydrothermal decomposition temperature in step 2) is 220° C. and the hydrolysis time is 18 h.

5. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: The dialysis process in step 2) is to transfer the filtrate to a 1000 molecular weight dialysis bag for 24 hours, and replace the deionized water every 8 hours.

6. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: In the step 3), the weight ratio of Na2MoO4·2H2O to Bi(NO3)3·5H2O is 0.195g:0.780g.

7. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: In the step 3), the volume ratio of Na2MoO4·2H2O to ethylene glycol is 0.195 g:20 ml, and the volume ratio of Bi(NO3)3·5H2O to ethylene glycol is 0.780 g:20 ml.

8. The method for preparing a copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 1, characterized in that: In the step 3), the weight ratio of Na2MoO4·2H2O to SCQD is 0.195g:3.8mg, and the weight volume ratio of SCQD to anhydrous ethanol is 3.8mg:30mL; the volume ratio of anhydrous ethanol to tetrafluoroethylene in the step 3) is 30ml:100ml; the hydrothermal reaction temperature in the step 3) is 160°C, and the hydrothermal reaction time is 12h.

9. The copper algae carbon quantum dots / bismuth molybdate composite photocatalyst prepared by the preparation method according to any one of claims 1 to 8.

10. The use of the copper algae carbon quantum dots / bismuth molybdate composite photocatalyst according to claim 9 in the degradation of ciprofloxacin (CIP), preferably, the conditions for degrading ciprofloxacin (CIP) are: The dosage of 0.75CB is 0.5g / L, the CIP concentration is 0.01g / L, the degradation time is 180min, and the pH is 7.0.

Citation Information

Patent Citations

  • Bismuth oxide / bismuthyl carbonate / bismuth molybdate composite photocatalytic material and preparation method thereof

    CN110227526A

  • Preparation method of large marine plant-based carbon quantum dots

    CN111621292A

  • Preparation method and application of LCQDs / Bi2MoO6 ball-flower-shaped composite photocatalyst for degrading tetracycline

    CN117582977A

  • Bismuth oxide / bismuth subcarbonate / bismuth molybdate composite photocatalyst and preparation method thereof

    US20200406233A1