Preparation method of three-dimensional stacked structure iron molybdate nanosheet compound coated modified positive electrode material
The positive electrode material is coated with iron molybdate nanosheet compounds in the three-dimensional stacking structure, which solves the problem of low capacity attenuation and stability of the positive electrode material of lithium-ion battery during the cycle process, improves electrochemical activity and cycle stability, and is suitable for electric vehicles. Battery and other applications.
Patent Information
- Application Number
- CN202411035139.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing lithium-ion battery positive electrode materials have problems such as fast capacity decay, low stability and low activity during the charge and discharge cycle. Especially in high-demand electric vehicle batteries, the electronic conductivity and diffusion coefficient of the ternary positive electrode materials are low. Causes insufficient cycle life and safety.
The preparation method of coating the modified positive electrode material with a three-dimensional stacked structure is adopted. The surface of the positive electrode material is coated by the iron molybdate nanosheet compound to improve its activity, surface stability and cycling performance. The specific steps include adding surfactant and cosurfactant to the oil phase, mixing molybdate and iron salts to form a reverse microemulsion, and microwave carbonization to form a three-dimensional stacked iron molybdate nanosheet compound coating layer. .
Significantly improve the electrochemical activity, conductivity and mechanical properties of the positive electrode material, enhance cycling stability, reduce volume changes during lithium ion embedding/detachment, optimize cycling performance, improve electronic conductivity, and extend battery service life.
Smart Images

Figure BDA0004970878690000081 
Figure HDA0004970878810000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of modified preparation of positive electrode materials, and specifically relates to a preparation method of a positive electrode material coated with a modified iron molybdate nanosheet compound with a three-dimensional stacked structure. Background Art
[0002] With the surge in global energy demand, people's reliance on efficient and environmentally friendly energy storage solutions continues to rise. As traditional energy sources become increasingly tight in the world, it is necessary to choose a safer and more reliable energy alternative. In today's electrical age, lithium-ion batteries (LIBs), as a rapidly developing and efficient energy storage technology, have become a hot topic of research due to their excellent portability, high energy density and stable cycle performance. They are widely used in portable electronics, automobiles, aerospace and other fields. Although current battery technology has made significant progress, its endurance and cost are still the main obstacles.
[0003] The cathode material is a key determinant of the performance of lithium-ion batteries, and the current development focus is on improving its safety, economic benefits, long cycle performance and capacity. Lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and ternary cathode materials (such as NCM and NCA) are the main choices for existing cathode materials, each carrying different characteristics and challenges. Lithium cobalt oxide has an ideal ion diffusion rate and electronic conductivity, which makes the battery have higher performance. Its high specific capacity (theoretical specific capacity is up to 274mAh / g) and stable operating voltage bring it huge advantages. However, in actual situations, lithium cobalt oxide can only release a specific capacity of about 140mAh / g, because during the discharge process, when more than 50% of lithium ions are released, its monoclinic crystal structure will replace the original crystal structure, so the actual specific capacity is seriously affected. Therefore, during use, the capacity can only be released by up to 50%, that is, the actual specific capacity is about 140mAh / g. Lithium cobalt oxide also has the advantages of good rate performance, excellent cycle stability and simple synthesis process, but its actual working specific capacity deviation is large, there is a risk of thermal runaway and the synthesis cost is high. At the same time, it has certain damage to the environment, which greatly limits its application scenarios and is mainly used in small or medium-sized electronic products. The unique spinel structure of lithium iron phosphate is good enough to protect Li + When excessive diffusion occurs, Fe 2+ The stability of the supporting material structure will not cause the destruction of the crystal structure. 4It has abundant raw material reserves and low prices, stable working voltage that meets most working requirements, a theoretical specific capacity of 170mAh / g, a structure that remains stable during the cycle, and can meet more high and low temperature applications and long cycle stability. It is far superior to other positive electrode materials, environmentally friendly, and will not explode even if a fire occurs. However, it has a very low electronic conductivity and exhibits disadvantages such as poor ion diffusion rate, which makes the material unable to meet the needs of fast charging and discharging.
[0004] With the iteration and progress of lithium-ion battery technology, comprehensive LiCoO 2 The cycling stability of LiNiO 2 The high specific capacity and LiMnO 2 LiNi has many advantages such as high safety and low cost. x Co y Mn 1-x-y O 2 (NCM) materials were invented, covering the advantages of the three materials and avoiding the disadvantages, making it advantageous in fields with high energy density requirements such as electric vehicles. At the same time, NCM materials have a higher operating voltage, which means that higher power output can be provided at the same current, thus meeting application scenarios with high power output requirements. NCM materials also have good cycle life and relatively stable long cycle performance, which is crucial for the service life and reliability of batteries. However, there are many problems with batteries with ternary positive electrode materials at the current stage: low electronic conductivity and diffusion coefficient, poor rate performance; the electrolyte is severely decomposed by the active material at a voltage above 4.3V, resulting in serious gas production during the charging and discharging of the nickel-rich positive electrode; the active material is easy to deliquesce, which will seriously affect the cycle life of the battery; the secondary spherical particles have poor mechanical properties, and are prone to volumetric strain, expansion and contraction under high pressure, causing microcracks and particle damage. Microcracks react along the active material and the electrolyte, accelerating the disintegration of large particles and the decomposition of the electrolyte. The crushed particles cannot participate in the electrochemical reaction, resulting in rapid capacity decay.
[0005] To solve these problems, researchers have made a lot of efforts in the modification of ternary materials, mainly through surface coating, ion doping and single crystal treatment to improve performance. Surface coating technology reduces direct contact with the electrolyte by forming a protective layer on the surface of the electrode material to improve the chemical stability of the material and prevent the occurrence of side reactions, thereby improving the electrochemical performance of the positive electrode material. Ion doping can stabilize the lattice structure, enhance the battery capacity and improve its cycle stability; while single crystal treatment optimizes the microstructure of the material and improves the migration efficiency of lithium ions. The single crystalization of ternary positive electrode materials can make their particle size smaller and the surface smoother, increase the contact between the material and the electrolyte and the binder, and improve the diffusion rate of lithium ions in the material. The complete three-dimensional diffusion channel inside the single crystal material can reduce the difficulty of lithium ion deintercalation. However, although the coating modification of carbon materials and metal oxides has achieved certain results, the current modification effect still needs to be optimized. It is still necessary to continue to explore more efficient modification strategies to further promote the application of ternary positive electrode materials, especially in high-demand electric vehicle batteries. Summary of the invention
[0006] The present invention provides a method for preparing a three-dimensional stacked structure of an iron molybdate nanosheet compound coated modified cathode material. Aiming at the problems of rapid capacity decay, low stability and low activity of conventional cathode materials during charge and discharge cycles, the cathode materials are modified by coating with iron molybdate nanosheet compounds, thereby improving the activity and surface stability of the conventional cathode materials and improving their cycle performance.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a three-dimensional stacked iron molybdate nanosheet compound coated modified cathode material, the specific steps are as follows:
[0009] (1) Add the oil phase, surfactant, and co-surfactant into a round-bottom flask in proportion, stir until completely transparent to obtain a continuous phase, and add the positive electrode material into the continuous phase and mix quickly;
[0010] (2) taking a molybdate and an iron salt, adding them to water to dissolve to obtain a mixed solution, adding the mixed solution to the continuous phase containing the positive electrode material in step (1) to obtain a reverse microemulsion of a positive electrode material mixed with platinum ions and iron ions, and stirring the reaction to obtain a mixed material with deposits of platinum ions and iron ions;
[0011] (3) After the mixed material in step (2) is separated, washed and dried, it is subjected to microwave carbonization by microwave radiation heating in a nitrogen atmosphere to obtain a positive electrode material coated with a three-dimensional stacked structure of iron molybdate nanosheet compounds.
[0012] The oil phase in step (1) can be composed of various water-insoluble organic substances, including but not limited to: cyclohexane, n-hexane, n-octane, etc. (mainly C6 -C 10 Alkanes); the surfactant can be composed of various ionic surfactants, including but not limited to the following substances: sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, etc., and can also be composed of various non-ionic surfactants, including but not limited to the following substances: TritonX series, Span series, octylphenol polyoxyethylene ether, etc.; the co-surfactant can be composed of various water-soluble alcohols, including but not limited to: n-hexanol, n-butanol, n-pentanol, etc. in the continuous phase; the volume ratio of the oil phase, the surfactant, and the co-surfactant is 10:2:3.
[0013] In step (1), the positive electrode material is LiNi x Co y Mn 1-x-y O 2 、LiNi x Co y Al 1-x-y O 2 、LiCoO 2 、LiMnO 2 、LiFePO 4 、LiMn 2 O 4 , Li 4 Ti 5 O 12 、LiMn 1.5 Ni 0.5 O 4 One of, but not limited to, the following; wherein LiNi x Co y Mn 1-x-y O 2 LiNi 0.8 Co 0.1 Mn 0.1 O 2 、LiNi 0.9 Co 0.05 Mn 0.05 O 2 、LiNi 0.6 Co 0.2 Mn 0.2 O 2 、LiNi 0.5 Co 0.2 Mn 0.3 O 2 One of them, LiNi x Co y Al 1-x-y O 2 LiNi 0.8 Co 0.15 Al 0.05 O2 、LiNi 0.815 Co 0.15 Al 0.035 O 2 One of the above; the mol:mL ratio of positive electrode material to continuous phase is 0.05:210~240.
[0014] The stirring speed of step (1) is 200-400 rpm.
[0015] In step (2), the molybdate is Na 2 MoO 4 NH 4 ) 6 Mo 7 O 24 ·4H 2 O、(NH 4 ) 2 MoO 4 One or more of the above are mixed in any proportion.
[0016] In step (2), the iron salt is FeCl 3 、Fe(NO 3 ) 3 9H 2 O, Fe(NO 3 ) 3 One or more of the above are mixed in any proportion.
[0017] In step (2), the molybdate and the iron salt are mixed in a ratio to generate iron molybdate, and the molar ratio of the positive electrode material to the iron molybdate is calculated as 1:0.01 to 1:0.2.
[0018] In step (2), the stirring speed is 200-400 rpm and the reaction time is 2-6 h.
[0019] In step (3), the washing solvent is any one of ethanol, deionized water, etc., or a mixture of the two; the drying temperature is 80-120° C., and the drying time is 8-12 hours.
[0020] In step (3), the microwave carbonization power is 500-800W, and the carbonization time is 10-30min.
[0021] The beneficial effects of the present invention are:
[0022] (1) The iron molybdate nanosheet compound of the present invention has a variety of possible stoichiometric compositions, crystal structures, valence states and nanocrystalline forms, and is used to coat the surface of the positive electrode material, which makes the positive electrode material have higher electrochemical activity. In addition, the positive electrode material coated with the iron molybdate nanosheet compound has better conductivity, mechanical properties and cycle stability.
[0023] (2) The positive electrode material coated with the iron molybdate nanosheet compound with a three-dimensional stacking structure in the present invention has better sphericity and a more obvious crystal structure, which greatly improves the stability of the positive electrode material structure and reduces the volume change and lattice expansion during the lithium ion insertion / extraction process, thereby optimizing the cycle performance.
[0024] (3) The three-dimensional stacking structure of the present invention is combined with the positive electrode material to form a unique composite structure, which effectively improves the electronic conductivity of the material and accelerates the Li + The diffusion rate of the electrode materials with low activity and low stability provides a reference for improving their high performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 (a) Uncoated and modified polycrystalline commercial NCM811; (b) Detailed enlarged image of uncoated and modified polycrystalline commercial NCM811; (c) Fe 2 (MoO 4 ) 3 Polycrystalline commercial NCM811 modified by nanosheet compound coating - Example 3; (d) Fe 2 (MoO 4 ) 3 Detailed enlargement of the modified polycrystalline commercial NCM811 coated with nanosheet compounds - Example 3. DETAILED DESCRIPTION
[0026] In order to better reflect the content of the present invention, the present invention is further described in detail below through specific embodiments, but the protection scope of the present invention is not limited to the content.
[0027] Example 1
[0028] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0029] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 200 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0030] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.03 Weigh 1.09g of sodium molybdate Na 2 MoO4 and 0.488 g ferric chloride FeCl 3 20 mL of water was added to fully dissolve, and then added dropwise to the mixed phase of step (1) to form a reverse microemulsion, and reacted at a speed of 200 rpm for 6 h to obtain a mixed material with deposited molybdenum ions and iron ions;
[0031] (3) The mixed material obtained in step (2) was separated and washed with ethanol, dried at 80° C. for 12 h, and then carbonized by radiation heating at a power of 650 W for 25 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%Fe 2 (MoO 4 ) 3 Nickel-rich positive electrode material.
[0032] Example 2
[0033] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0034] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 300 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0035] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.03. Weigh 0.882g of ammonium molybdate (NH 4 ) 2 MoO 4 and 0.726 g ferric nitrate Fe(NO 3 ) 3 Add 20 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 300 rpm for 5 hours to obtain a mixed material with deposited molybdenum ions and iron ions;
[0036] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 100° C. for 10 h, and then carbonized by radiation heating at a power of 800 W for 10 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%Fe 2 (MoO 4 ) 3 Nickel-rich positive electrode material.
[0037] Example 3
[0038] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0039] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 400 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0040] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.03. Weigh 0.882g of ammonium molybdate (NH 4 ) 2 MoO 4 and 0.726 g ferric nitrate Fe(NO 3 ) 3 Add 30 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 400 rpm for 4 hours to obtain a mixed material with deposited molybdenum ions and iron ions;
[0041] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 120° C. for 8 h, and then carbonized by radiation heating at a power of 650 W for 25 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%Fe 2 (MoO 4 )3 Nickel-rich positive electrode material.
[0042] Example 4
[0043] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0044] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 400 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0045] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.2 Weigh 7.26g of sodium molybdate Na 2 MoO 4 and 3.25 g ferric chloride FeCl 3 Add 25 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 400 rpm for 4 hours to obtain a mixed material with deposited molybdenum ions and iron ions;
[0046] (3) The mixed material obtained in step (2) was separated and washed with ethanol, dried at 80° C. for 12 h, and then carbonized by radiation heating at a power of 650 W for 25 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @20at%Fe 2 (MoO 4 ) 3 Nickel-rich positive electrode material.
[0047] Example 5
[0048] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0049] (1) 165 mL of cyclohexane, 33 mL of octylphenol polyoxyethylene ether (OP-10) and 45.5 mL of n-hexanol were added to a round-bottom flask and stirred at 350 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0050] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.03. Weigh 0.795 g of ammonium molybdate tetrahydrate (NH 4 ) 6 Mo 7 O 24 ·4H 2 O and 1.21 g of ferric nitrate nonahydrate Fe(NO 3 ) 3 9H 2 O was fully dissolved by adding 25 mL of water; then added dropwise to the mixed phase of step (1) to form a reverse microemulsion, and reacted at a speed of 300 rpm for 5 h to obtain a mixed material with deposited molybdenum ions and iron ions;
[0051] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 100° C. for 10 h, and then carbonized by radiation heating at a power of 650 W for 25 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%Fe 2 (MoO 4 ) 3 Nickel-rich positive electrode material.
[0052] Example 6
[0053] A method for preparing a high-nickel NCM811 positive electrode material by coating and modifying a three-dimensional stacked iron molybdate nanosheet compound, the specific steps are as follows:
[0054] (1) 135 mL of cyclohexane, 27 mL of octylphenol polyoxyethylene ether (OP-10) and 40.5 mL of n-hexanol were added to a round-bottom flask and stirred at 350 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 O2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0055] (2) Based on the molar ratio (NCM811:Fe 2 (MoO 4 ) 3 ) is 1:0.01. Weigh 0.294 g of ammonium molybdate (NH 4 ) 2 MoO 4 and 0.242 g ferric nitrate Fe(NO 3 ) 3 Add 20 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 300 rpm for 6 hours to obtain a mixed material with deposited molybdenum ions and iron ions;
[0056] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 120° C. for 8 h, and then carbonized by radiation heating at a power of 500 W for 30 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @1at%Fe 2 (MoO 4 ) 3 Nickel-rich positive electrode material.
[0057] Example 7
[0058] Preparation of LiFePO by coating and modification of three-dimensional stacked iron molybdate nanosheet compounds 4 The method of positive electrode material, the specific steps are as follows:
[0059] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 250 rpm until completely transparent to prepare a continuous phase. 7.89 g of commercial LiFePO 4 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0060] (2) By molar ratio (LiFePO 4 :Fe 2 (MoO 4 ) 3 ) is 1:0.03. Weigh 0.882g of ammonium molybdate (NH 4 ) 2 MoO 4 and 0.726 g ferric nitrate Fe(NO 3 ) 3Add 20 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 300 rpm for 6 hours to obtain a mixed material with deposited molybdenum ions and iron ions;
[0061] (3) The mixed material obtained in step (2) was separated and washed with water and ethanol, dried at 120° C. for 8 h, and then carbonized by radiation heating at a power of 650 W for 25 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of LiFePO 4 @3at%Fe 2 (MoO 4 ) 3 Positive electrode material.
[0062] Comparative Example 1
[0063] A method for preparing high-nickel NCM811 positive electrode material by coating and modifying iron oxide, the specific steps are as follows:
[0064] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 400 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0065] (2) By molar ratio (LiFePO 4 :Fe 2 O 3 ) is 1:0.03. Weigh 0.726 g of iron nitrate Fe(NO 3 ) 3 Add 30 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at 300 rpm for 5 hours to obtain a mixed material with iron ion deposition;
[0066] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 100° C. for 10 h, and then radiated and heated in a microwave reactor under nitrogen atmosphere with a carbonization power of 800 W for 10 min to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%Fe 2 O 3 Nickel-rich positive electrode material.
[0067] Comparative Example 2
[0068] A method for preparing high-nickel NCM811 positive electrode material by coating and modifying molybdenum oxide, the specific steps are as follows:
[0069] (1) 150 mL of cyclohexane, 30 mL of octylphenol polyoxyethylene ether (OP-10) and 45 mL of n-hexanol were added to a round-bottom flask and stirred at 300 rpm until completely transparent to prepare a continuous phase. 4.86 g of commercial nickel-rich cathode material LiNi 0.8 Co 0.1 Mn 0.1 O 2 The powder is added to the continuous phase and stirred to obtain a mixed phase;
[0070] (2) By molar ratio (LiFePO 4 :MoO 3 ) is 1:0.03. Weigh 0.294 g of ammonium molybdate (NH 4 ) 2 MoO 4 Add 30 mL of water to fully dissolve; then add dropwise to the mixed phase of step (1) to form a reverse microemulsion, and react at a speed of 300 rpm for 5 hours to obtain a mixed material with deposited molybdenum ions;
[0071] (3) After the mixed material obtained in step (2) was separated and washed with water and ethanol, it was dried at 100° C. for 10 h, and then carbonized by radiation heating at a power of 800 W for 10 min in a microwave reactor under nitrogen atmosphere to obtain a three-dimensional stacked structure of Li(Ni 0.8 Co 0.1 Mn 0.1 ) 2 @3at%MoO 3 Nickel-rich positive electrode material.
[0072] Figure 1 (a) Uncoated modified NCM811 cathode material - commercial NCM811; (b) Detailed enlarged image of uncoated modified NCM811 cathode material - commercial NCM811; (c) Fe 2 (MoO 4 ) 3 Polycrystalline NCM811 positive electrode material modified by coating with nanosheet compounds - Example 3; (d) Fe 2 (MoO 4 ) 3 A detailed enlarged image of the polycrystalline NCM811 positive electrode material modified by coating with nanosheet compounds - Example 3. As can be seen from the figure, a crystalline structure of lamellae is formed on the surface of the NCM811 positive electrode material coated with iron molybdate nanosheet compounds, and the crystal coating is relatively uniform and has good consistency.
[0073] The materials prepared in the above examples and commercial NCM811, commercial LiFePO 4 As the positive electrode, lithium metal as the negative electrode, polypropylene film (Celgard 2400) as the separator, ethylene carbonate containing 1M lithium hexafluorophosphate as the electrolyte, the button cell was assembled in a glove box filled with argon gas, the water content of the glove box was less than 0.01ppm, and the oxygen content was less than 0.01ppm; the positive electrode lithium ion NCM811 battery was tested at 2.8~4.3V, LiFePO 4 The battery has a capacity retention rate of 50 cycles at a charge and discharge rate of 1C at a voltage of 2.5 to 4.2V. The results are shown in Table 1 below:
[0074] Table 1
[0075]
[0076] Examples 1 to 3 and Examples 4 to 6 are respectively NCM811 positive electrode materials coated and modified by iron molybdate nanosheet compounds forming a three-dimensional stacking structure through different molybdenum sources and iron sources, wherein Example 1 and Example 4 use sodium molybdate and ferric chloride as ion sources of iron molybdate, Example 2, Example 3 and Example 6 use ammonium molybdate and ferric nitrate without bound water as ion sources of iron molybdate, and Example 5 uses ammonium molybdate tetrahydrate and ferric nitrate nonahydrate containing bound water as ion sources of iron molybdate; By comparing Example 3 with Example 5, it can be found that the iron molybdate formed by ammonium molybdate and ferric nitrate without bound water exhibits a higher initial discharge specific capacity and a capacity retention rate after 50 cycles, which is because the molybdenum salt and iron salt without bound water are more stable and easier to combine with the ternary positive electrode material and adhere to the surface of the material; and by comparing Example 2, Example 3 and Example 6, it can be found that the coated material formed by microwave carbonization power at 650W exhibits a higher initial specific capacity, which is because too high power can easily cause Fe 2 (MoO 4 ) 3 The material's lattice becomes smaller, hindering the Li + The removal and embedding process; if the power is too low, the coating quality of the material will be affected and the complete coating effect cannot be achieved.
[0077] Comparison between Example 2 and Comparative Examples 1 and 2 shows that the effect of single iron or molybdenum oxide on the initial capacity and capacity retention of NCM811 material is not as obvious as that of cerium-molybdenum composite oxide. This is because the formed iron oxide or molybdenum oxide shows a dense oxide layer on the surface of the material, which hinders the Li + The removal and embedding of LiO2 lead to a decrease in capacity and a decrease in capacity retention rate. As a unique three-dimensional stacking structure coating, iron molybdate nanosheet compounds can have a larger specific surface area and porosity, which is beneficial for Li+ The extraction and insertion process provides more active sites.
[0078] The positive electrode material used in Examples 1 to 6 and Comparative Examples 1 to 2 is NCM811, and the positive electrode material used in Example 7 is LiFePO 4 From the data in the table above, it can be seen that no matter whether the positive electrode material is NCM811 or LiFePO 4 Compared with the corresponding commercial cathode materials, the initial discharge capacity and cycle capacity retention rate of the coated materials have been improved to a certain extent, indicating that the coating modification of iron molybdate nanosheet compounds has a certain effect on NCM811 and LiFePO 4 The performance of the positive electrode material is improved to a certain extent. The active material reacts with the electrolyte, accelerating the disintegration of large particles and the decomposition of the electrolyte. The crushed particles cannot participate in the electrochemical reaction, resulting in rapid capacity decay. The use of coating methods to modify the positive electrode material can reduce the direct contact between the positive electrode material and the electrolyte, and to a certain extent increase its cycle life. In addition, the iron molybdate nanosheet compound has excellent conductivity, which can improve the transmission rate of electrons in the positive electrode material without adding a large amount of inactive conductive agent.
[0079] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a three-dimensional stacked structure of iron molybdate nanosheet compound coated modified positive electrode material, characterized in that: The specific steps are as follows: (1) Mixing the oil phase, surfactant, and co-surfactant and stirring until completely transparent to obtain a continuous phase, and adding the positive electrode material to the continuous phase and mixing; (2) taking a molybdate and an iron salt, adding them to water to dissolve to obtain a mixed solution, adding the mixed solution to the continuous phase containing the positive electrode material in step (1) to obtain a reverse microemulsion of a positive electrode material mixed with platinum ions and iron ions, and stirring the reaction to obtain a mixed material with deposits of platinum ions and iron ions; (3) After the mixed material in step (2) is separated, washed and dried, it is subjected to microwave carbonization under a nitrogen atmosphere to obtain a positive electrode material coated with a three-dimensional stacked structure of iron molybdate nanosheet compounds.
2. The preparation method according to claim 1, characterized in that: In step (1), the oil phase is cyclohexane, n-hexane or n-octane; the surfactant is sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, TritonX series, Span series or octylphenol polyoxyethylene ether; the co-surfactant is n-hexanol, n-butanol or n-pentanol; and the volume ratio of the oil phase, surfactant and co-surfactant in the continuous phase is 10:2:
3.
3. The preparation method according to claim 1, characterized in that: In step (1), the positive electrode material is LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co 0.05 Mn 0.05 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.815 Co 0.15 Al 0.035 One of O2; the mol:mL ratio of positive electrode material to continuous phase is 0.05:210~240.
4. The preparation method according to claim 1, characterized in that: The stirring speed of step (1) is 200-400 rpm.
5. The preparation method according to claim 1, characterized in that: The molybdate in step (2) is Na2MoO4, (NH4)6Mo7O 24 · One or more of 4H2O and (NH4)2MoO4 are mixed in any proportion.
6. The preparation method according to claim 1, characterized in that: In step (2), the iron salt is a mixture of one or more of FeCl3, Fe(NO3)3·9H2O, and Fe(NO3)3 in any proportion.
7. The preparation method according to claim 1, characterized in that: In step (2), the molybdate and the iron salt are mixed in a ratio to generate iron molybdate, and the molar ratio of the positive electrode material to iron molybdate is 1:0.01 to 1:0.
2.
8. The preparation method according to claim 1, characterized in that: The stirring speed of the stirring reaction in step (2) is 200 to 400 rpm, and the reaction time is 2 to 6 hours.
9. The preparation method according to claim 1, characterized in that: The drying temperature in step (3) is 80 to 120° C. and the drying time is 8 to 12 hours.
10. The preparation method according to claim 1, characterized in that: In step (3), the microwave carbonization power is 500-800W, and the carbonization time is 10-30min.
Citation Information
Patent Citations
Graphene clad Fe2(MoO4)3 nanoparticle and preparation method and application thereof
CN105742598A
Monoclinic structure Fe2(MoO4)3 nanowire as well as preparation method and application thereof
CN112850788A
Method for preparing positive electrode material through coating modification of cerium-molybdenum composite oxide
CN118299542A
Cited By
Catalyst, preparation method and application in methanol oxidation synthesis of formaldehyde
CN121669251A