Bifunctional catalyst for directly preparing light aromatic hydrocarbon from synthesis gas as well as preparation method and application of bifunctional catalyst
By using potassium-iron composite oxide and metal Mo-modified mesoporous HZSM-5 molecular sieve catalyst, the problems of low CO conversion rate and aromatic hydrocarbon yield in the existing technology have been solved, and efficient aromatic hydrocarbon generation and catalyst stability have been achieved, with Good industrial application prospects.
Patent Information
- Application Number
- CN202410786636.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-22
AI Technical Summary
Existing dual-functional catalysts for directly producing light aromatics from synthesis gas suffer from low CO conversion rates and low aromatic hydrocarbon yields due to mismatch in Fischer-Tropsch synthesis and aromatization reaction temperatures and poor diffusion of intermediate products.
Potassium-iron composite oxide is used as the Fischer-Tropsch synthesis catalyst and metal Mo-modified mesoporous HZSM-5 molecular sieve is used as the aromatization molecular sieve catalyst. A bifunctional catalyst is synthesized through a specific preparation method to improve the activity and stability of the catalyst.
It improves the CO conversion rate and aromatic hydrocarbon yield, reduces the selectivity of the by-product CH4, and enhances the catalyst's resistance to sintering and carbon deposition, and has good industrial application prospects.
Smart Images

Figure BDA0004898796480000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of synthesis gas conversion, and in particular to a bifunctional catalyst for directly preparing aromatics from synthesis gas, and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Light aromatics (Benzene-Toluene-Xylene, BTX) include benzene, toluene and xylene, all of which are important chemical raw materials, mainly derived from the cracking of petroleum. With the reduction of crude oil resources and the increasing prominence of environmental problems, it is challenging to obtain olefins and aromatics from petroleum routes, and it has become unsustainable. Therefore, it is necessary to develop a process route for producing aromatics from non-petroleum routes, through catalytic synthesis gas (CO+H 2 or CO 2 +H 2 )The process route for preparing light aromatics has attracted more and more attention.
[0004] The process of preparing light aromatics from syngas that has been reported so far is mainly achieved by placing two catalysts with syngas conversion function and dehydrogenation aromatization function in a series of two-bed reactors, or placing them in a single-bed reactor in a mixed manner between particles or within particles. The two catalysts are distributed in different reactors and adopt different catalytic processes. The reaction process is complicated and difficult to operate, the energy utilization efficiency is low, and the cost is high. Compared with the two-step method for preparing aromatics from syngas, the one-step method for preparing aromatics places two catalysts in the same reactor for operation, which significantly improves the conversion rate of the reaction and reduces the production cost. However, the existing bifunctional catalysts for directly preparing light aromatics are mostly a mixture of Fischer-Tropsch synthesis and molecular sieve catalysts. Because the reaction temperatures of Fischer-Tropsch synthesis and aromatization cannot be effectively matched, and the intermediate products cannot be effectively diffused, the conversion of syngas and the generation of aromatic compounds are limited, resulting in low CO conversion rate and low aromatics yield. Summary of the invention
[0005] In order to overcome the above problems, the present invention provides a bifunctional catalyst for directly preparing aromatics from synthesis gas, and a preparation method and application thereof.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides a bifunctional catalyst for directly preparing aromatics from synthesis gas, comprising a Fischer-Tropsch synthesis catalyst and an aromatization molecular sieve catalyst, wherein the Fischer-Tropsch synthesis catalyst is a potassium-iron composite oxide, and the aromatization molecular sieve catalyst is a mesoporous HZSM-5 molecular sieve catalyst modified with metal Mo.
[0008] The second aspect of the present invention provides a method for preparing the above-mentioned bifunctional catalyst for directly converting synthesis gas into aromatics, comprising:
[0009] (1) dropping ammonia water into an iron salt solution, heating and stirring to uniformly age, centrifuging and washing, drying and removing water, calcining, and grinding and sieving after cooling;
[0010] (2) Immerse the sample prepared in step (1) in K 2 CO 3 The solution is dried to remove water after ultrasonic treatment, and then ground and sieved after calcination to obtain a Fischer-Tropsch synthesis catalyst;
[0011] (3) Add HZSM-5 to NaOH solution, heat and stir, centrifuge and wash, then add NH 4 Cl solution, centrifugally washed, and then ion exchanged 1 to 5 times using the same ion exchange method, and then dried to remove water, calcined, ground and sieved to obtain a mesoporous HZSM-5 molecular sieve;
[0012] (4) Immerse the sample in step (4) into (NH 4 ) 2 MoO 4 In the solution, drying is performed to remove water after ultrasonic treatment, grinding and sieving are performed after calcination to obtain an aromatization molecular sieve catalyst;
[0013] (5) The Fischer-Tropsch synthesis catalyst obtained in step (2) and the aromatization molecular sieve catalyst obtained in step (4) are respectively shaped and sieved, and the two sieved catalysts are mixed to obtain a bifunctional catalyst for directly converting synthesis gas to aromatics.
[0014] The third aspect of the present invention provides the use of the above-mentioned bifunctional catalyst for directly preparing aromatics from synthesis gas in the hydrogenation reaction of carbon monoxide or carbon dioxide.
[0015] The beneficial effects of the present invention are:
[0016] In the present invention, by adding the auxiliary active component K 2 O modifies metallic Fe and enhances Fe 2 O 3The carburizing ability of the catalyst is improved to promote the formation of olefin products and increase the yield of aromatics. On the other hand, the active component MoO and alkali solution are added to prepare the mesoporous HZSM-5 molecular sieve, which increases the adsorption and desorption rate of aromatic compounds in the pores, inhibits the alkylation reaction, and promotes the formation of BTX compounds. A fixed bed reaction device is used, and the syngas is used as the raw material to evaluate the catalyst activity of CO conversion rate and aromatics yield. The study found that compared with the traditional syngas to aromatics catalyst, the bifunctional catalyst provided by the present invention has the following advantages in the catalytic process: high CO conversion rate and aromatics yield, and the byproduct CH 4 It has the characteristics of low selectivity, strong resistance to sintering and carbon deposition, and has good industrial application prospects. DETAILED DESCRIPTION
[0017] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0018] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0019] A first typical embodiment of the present invention provides a bifunctional catalyst for directly preparing aromatics from synthesis gas, comprising a Fischer-Tropsch synthesis catalyst and an aromatization molecular sieve catalyst, wherein the Fischer-Tropsch synthesis catalyst is a potassium-iron composite oxide, and the aromatization molecular sieve catalyst is a mesoporous HZSM-5 molecular sieve catalyst modified with metal Mo.
[0020] In one or more embodiments, the Fischer-Tropsch synthesis catalyst is a mixture of iron oxide and potassium oxide; and the aromatization molecular sieve catalyst is a mesoporous HZSM-5 molecular sieve catalyst loaded with molybdenum oxide.
[0021] Preferably, the bifunctional catalyst for directly converting synthesis gas to aromatics comprises the following components in parts by weight: 15 to 45 parts of iron oxide, 1 to 5 parts of potassium oxide, 1 to 10 parts of molybdenum oxide, and 45 to 80 parts of mesoporous HZSM-5 molecular sieve.
[0022] A second typical embodiment of the present invention provides a method for preparing the above-mentioned bifunctional catalyst for directly converting synthesis gas into aromatics, comprising:
[0023] (1) dropping ammonia water into an iron salt solution, heating and stirring to uniformly age, centrifuging and washing, drying and removing water, calcining, and grinding and sieving after cooling;
[0024] (2) Immerse the sample prepared in step (1) in K 2 CO 3 The solution is dried to remove water after ultrasonic treatment, and then ground and sieved after calcination to obtain a Fischer-Tropsch synthesis catalyst;
[0025] (3) Add HZSM-5 to NaOH solution, heat and stir, centrifuge and wash, then add NH 4 Cl solution, centrifugally washed, and then ion exchanged 1 to 5 times using the same ion exchange method, and then dried to remove water, calcined, ground and sieved to obtain a mesoporous HZSM-5 molecular sieve;
[0026] (4) Immerse the sample in step (4) into (NH 4 ) 2 MoO 4 In the solution, drying is performed to remove water after ultrasonic treatment, grinding and sieving are performed after calcination to obtain an aromatization molecular sieve catalyst;
[0027] (5) The Fischer-Tropsch synthesis catalyst obtained in step (2) and the aromatization molecular sieve catalyst obtained in step (4) are respectively shaped and sieved, and the two sieved catalysts are mixed to obtain a bifunctional catalyst for directly converting synthesis gas to aromatics.
[0028] In one or more embodiments, in step (1), the iron salt is one or more of ferric nitrate, ferric chloride, ferric sulfate, and ferric acetate, preferably ferric nitrate.
[0029] In one or more embodiments, in step (1), NH 3 ·H 2 The molar ratio of O to iron salt is 3 to 5:1.
[0030] In one or more embodiments, in step (1), the temperature of heating and stirring is 30 to 100°C.
[0031] In one or more embodiments, in step (1), the heating, stirring and aging time is 1 to 24 hours.
[0032] In one or more embodiments, in step (1), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours.
[0033] In one or more embodiments, in step (1), the grinding and screening is 10-200 mesh.
[0034] In one or more embodiments, in step (2), K 2CO 3 The concentration of the solution is 0.5~1 mol / L.
[0035] In one or more embodiments, in step (2), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours.
[0036] In one or more embodiments, in step (2), the grinding and screening is 10-200 mesh.
[0037] In one or more embodiments, in step (3), the mass ratio of HZSM-5 to NaOH is 1 / 10 to 1 / 20.
[0038] In one or more embodiments, in step (3), the concentration of the NaOH solution is 0.5 to 2 mol / L.
[0039] In one or more embodiments, in step (3), the temperature of heating and stirring is 30 to 100° C., and the time of heating and stirring is 2 to 10 hours.
[0040] In one or more embodiments, in step (3), NH 4 The concentration of Cl solution is 0.5~2mol / L.
[0041] In one or more embodiments, in step (3), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours.
[0042] In one or more embodiments, in step (3), the grinding and screening is 10 to 200 meshes.
[0043] In one or more embodiments, in step (4), (NH 4 ) 2 MoO 4 The concentration of the solution is 0.5~1 mol / L.
[0044] In one or more embodiments, in step (4), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours.
[0045] In one or more embodiments, in step (4), the grinding and screening is 10-200 mesh.
[0046] In one or more embodiments, in step (5), the Fischer-Tropsch synthesis catalyst with a mesh size of 30 to 40 and the aromatization molecular sieve catalyst with a mesh size of 30 to 40 are obtained by forming and screening.
[0047] A third typical embodiment of the present invention provides the use of the above-mentioned bifunctional catalyst for directly preparing aromatics from synthesis gas in the hydrogenation reaction of carbon monoxide or carbon dioxide.
[0048] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0049] Example 1
[0050] (1) Preparation of Fischer-Tropsch main active components: NH 3 ·H 2 O drops into Fe(NO 3 ) 3 9H 2 O solution, heated and stirred at 80°C, aged for 2 h, washed by centrifugation 3 times, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0051] (2) Introduction of Fischer-Tropsch active components: The sample prepared in step (1) was immersed in 1 mol / L K 2 CO 3 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, to obtain a Fischer-Tropsch synthesis catalyst.
[0052] (3) Preparation of molecular sieve pore structure: HZSM-5 was added to 1 mol / L NaOH solution, heated and stirred at 80°C for 2 h, centrifuged and washed 3 times, dried at 120°C for 12 h, added to 1 mol / L NH4Cl solution for ion exchange treatment, heated and stirred at 80°C for uniformity, centrifuged and washed 3 times, ion exchanged 3 times in the same way, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0053] (4) Introduction of molecular sieve active components: The sample in step (3) was impregnated with 0.81 mol / L (NH 4 ) 2 MoO 4 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, and an aromatization molecular sieve catalyst was obtained.
[0054] (5) Catalyst molding: The catalysts obtained in step (2) and step (4) are molded and sieved respectively to obtain 30-40 mesh Fischer-Tropsch synthesis catalyst and aromatization molecular sieve catalyst respectively, and the catalysts are mixed to obtain a bifunctional catalyst for direct synthesis of aromatics from synthesis gas. The content of each component is by weight: iron oxide: 30 parts; potassium oxide: 3 parts; molybdenum oxide: 7 parts; HZSM-5 molecular sieve: 60 parts.
[0055] Comparative Example 1
[0056] (1) Preparation of Fischer-Tropsch main active components: NH 3 ·H 2 O drops into Fe(NO 3 ) 3 9H 2 O solution, heated and stirred at 80°C, aged for 2 h, washed by centrifugation 3 times, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0057] (2) Introduction of Fischer-Tropsch active components: The sample prepared in step (1) was immersed in 1 mol / L K 2 CO 3 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, to obtain a Fischer-Tropsch synthesis catalyst.
[0058] (3) The HZSM-5 catalyst powder was calcined at 500°C for 12 h and then cooled to room temperature.
[0059] (4) The catalysts obtained in step (2) and step (3) are shaped and sieved respectively to obtain 30-40 mesh Fischer-Tropsch synthesis catalyst and HZSM-5 catalyst respectively, and the catalyst is obtained by mixing them. The content of each component is by weight: 30 parts of iron oxide, 3 parts of potassium oxide, and 67 parts of HZSM-5 catalyst.
[0060] Comparative Example 2
[0061] (1) Preparation of Fischer-Tropsch main active components: NH 3 ·H 2 O drops into Fe(NO 3 ) 3 9H 2 O solution, heated and stirred at 80°C, aged for 2 h, washed by centrifugation 3 times, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0062] (2) Introduction of Fischer-Tropsch active components: The sample prepared in step (1) was immersed in 1 mol / L K 2 CO 3 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, to obtain a Fischer-Tropsch synthesis catalyst.
[0063] (3) Preparation of molecular sieve pore structure: HZSM-5 was added to 1 mol / L NaOH solution, heated and stirred at 80°C for 2 h, centrifuged and washed 3 times, dried at 120°C for 12 h, added to 1 mol / L NH4Cl solution for ion exchange treatment, heated and stirred at 80°C for uniformity, centrifuged and washed 3 times, ion exchanged 3 times in the same way, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0064] (4) The catalysts obtained in step (2) and step (3) are shaped and sieved respectively to obtain 30-40 mesh Fischer-Tropsch synthesis catalyst and HZSM-5 catalyst respectively, and the catalyst is obtained by mixing them. The content of each component is by weight: 30 parts of iron oxide, 3 parts of potassium oxide, and 67 parts of HZSM-5 catalyst.
[0065] Comparative Example 3
[0066] (1) Preparation of Fischer-Tropsch main active components: NH 3 ·H 2 O drops into Fe(NO 3 ) 3 9H 2 O solution, heated and stirred at 80°C, aged for 2 h, washed by centrifugation 3 times, dried at 120°C for 12 h, calcined at 500°C for 12 h, cooled to room temperature, and ground and sieved to 200 mesh.
[0067] (2) Introduction of Fischer-Tropsch active components: The sample prepared in step (1) was immersed in 1 mol / L K 2 CO 3 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, to obtain a Fischer-Tropsch synthesis catalyst.
[0068] (3) Introduction of molecular sieve active components: HZSM-5 molecular sieve was impregnated with 0.8 mol / L (NH 4 ) 2 MoO 4 The solution was ultrasonicated for 2 h, dried at 120° C. for 12 h, calcined at 500° C. for 12 h, cooled to room temperature, ground and sieved to 200 mesh, and an aromatization molecular sieve catalyst was obtained.
[0069] (4) Catalyst molding: The catalysts obtained in step (2) and step (3) are molded and sieved respectively to obtain 30-40 mesh Fischer-Tropsch synthesis catalyst and aromatization molecular sieve catalyst respectively, and the two catalysts are mixed to obtain a bifunctional catalyst for direct synthesis of aromatics from synthesis gas. The content of each component is by weight: iron oxide: 30 parts; potassium oxide: 3 parts; molybdenum oxide: 7 parts; HZSM-5 molecular sieve: 60 parts.
[0070] The catalysts synthesized in Example 1 and Comparative Examples 1 to 3 were placed in a fixed bed reactor and reacted continuously for 60 hours under the reaction conditions of 350° C., 3.0 MPa and 1800 mL / g / h. The average conversion rate and the selectivity or distribution of each product are shown in Table 1.
[0071] Table 1 Catalytic performance of different catalysts
[0072]
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A bifunctional catalyst for direct conversion of synthesis gas to aromatics, characterized in that: The invention comprises a Fischer-Tropsch synthesis catalyst and an aromatization molecular sieve catalyst, wherein the Fischer-Tropsch synthesis catalyst is a potassium-iron composite oxide, and the aromatization molecular sieve catalyst is a mesoporous HZSM-5 molecular sieve catalyst modified by metal Mo.
2. The bifunctional catalyst according to claim 1, characterized in that The Fischer-Tropsch synthesis catalyst is a mixture of iron oxide and potassium oxide; the aromatization molecular sieve catalyst is a mesoporous HZSM-5 molecular sieve catalyst loaded with molybdenum oxide.
3. The bifunctional catalyst as claimed in claim 2, characterized in that The bifunctional catalyst for directly preparing aromatics from synthesis gas comprises the following components in parts by weight: 15 to 45 parts of iron oxide, 1 to 5 parts of potassium oxide, 1 to 10 parts of molybdenum oxide, and 45 to 80 parts of mesoporous HZSM-5 molecular sieve.
4. The method for preparing a bifunctional catalyst according to any one of claims 1 to 3, characterized in that: include: (1) dropping ammonia water into an iron salt solution, heating and stirring to uniformly age, centrifuging and washing, drying and removing water, calcining, and grinding and screening after cooling; (2) immersing the sample prepared in step (1) into a K2CO3 solution, drying and removing water after ultrasonic treatment, grinding and sieving after calcination to obtain a Fischer-Tropsch synthesis catalyst; (3) adding HZSM-5 to a NaOH solution, heating and stirring, centrifugally washing, and then adding it to an NH4Cl solution for ion exchange, centrifugally washing, and then using the same ion exchange method to perform ion exchange again for 1 to 5 times, and then drying to remove water, calcining, and grinding and sieving to obtain a mesoporous HZSM-5 molecular sieve; (4) impregnating the sample in step (4) into a (NH4)2MoO4 solution, drying and removing water after ultrasonic treatment, grinding and sieving after calcination to obtain an aromatization molecular sieve catalyst; (5) The Fischer-Tropsch synthesis catalyst obtained in step (2) and the aromatization molecular sieve catalyst obtained in step (4) are respectively shaped and sieved, and the two sieved catalysts are mixed to obtain a bifunctional catalyst for directly converting synthesis gas to aromatics.
5. The preparation method according to claim 4, characterized in that: In step (1), the iron salt is one or more of ferric nitrate, ferric chloride, ferric sulfate, and ferric acetate, preferably ferric nitrate; Or, in step (1), the molar ratio of NH3·H2O to iron salt in aqueous ammonia is 3 to 5:1; Or, in step (1), the temperature of heating and stirring is 30 to 100° C.; Or, in step (1), the heating, stirring and aging time is 1 to 24 hours; Or, in step (1), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours; Or, in step (1), grinding and screening is 10-200 mesh.
6. The preparation method according to claim 4, characterized in that: In step (2), the concentration of the K2CO3 solution is 0.5-1 mol / L; Or, in step (2), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours; Or, in step (2), grinding and screening is 10-200 mesh.
7. The preparation method according to claim 4, characterized in that: In step (3), the mass ratio of HZSM-5 to NaOH is 1 / 10 to 1 / 20; Or, in step (3), the concentration of the NaOH solution is 0.5 to 2 mol / L; Or, in step (3), the temperature of heating and stirring is 30 to 100° C., and the time of heating and stirring is 2 to 10 hours; Or, in step (3), the concentration of the NH4Cl solution is 0.5 to 2 mol / L; Or, in step (3), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours; Or, in step (3), grinding and screening 10 to 200 meshes.
8. The preparation method according to claim 4, characterized in that: In step (4), the concentration of the (NH4)2MoO4 solution is 0.5 to 1 mol / L; Or, in step (4), the calcination temperature is 200 to 1000° C., and the calcination time is 2 to 12 hours; Or, in step (4), grinding and screening to 10-200 mesh.
9. The preparation method according to claim 4, characterized in that: In step (5), the 30-40 mesh Fischer-Tropsch synthesis catalyst and the 30-40 mesh aromatization molecular sieve catalyst are obtained by forming and screening.
10. Use of the bifunctional catalyst according to any one of claims 1 to 3 or the bifunctional catalyst prepared by the preparation method according to any one of claims 4 to 9 in the hydrogenation reaction of carbon monoxide or carbon dioxide.
Citation Information
Patent Citations
Modification treatment method and application of HZSM-5 molecular sieve catalyst
CN106215970A
Composite catalyst for directly preparing high-value arene from synthesis gas, preparation method and application
CN110201709A
Cited By
Catalyst for preparing light aromatic hydrocarbon from synthesis gas through one-step method and preparation method
CN119368222A