Method for reducing chromium content in converter steel slag
Through multi-stage ball milling and magnetic separation technology, the non-magnetic characteristics of perovskite are used to successfully reduce the chromium content in converter steel slag, solving the problem of difficulty in reducing the chromium content in the existing technology and improving the recycling rate of resources.
Patent Information
- Application Number
- CN202411054061.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-22
AI Technical Summary
It is difficult to effectively reduce the chromium content in converter steel slag with existing technology, resulting in the presence of a certain amount of chromium in the recycling of steel slag, which affects human health.
Through multi-stage ball milling and magnetic separation technology, including primary screening, ball milling and multi-stage magnetic separation, the non-magnetic characteristics of perovskite are used to separate chromium and reduce the chromium content in converter steel slag.
It effectively reduces the chromium content in converter steel slag and improves the utilization rate of waste resources. The Cr content of low-chromium steel slag can reach 0.003%, which is suitable for cement and other industries.
Smart Images

Figure CN118807934A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of effective utilization of waste resources, and in particular to a method for reducing the chromium content in converter slag. Background Art
[0002] During the converter steelmaking process, 8%-10% of steel slag will be produced. The total Cr content in the steel slag is 0.05%-0.3%, and the main valence states are +2, +3, +6, etc. Among them, +3 valent chromium is beneficial to the human body, while +6 valent chromium is harmful to the human body.
[0003] After slag turning, water pumping and hot stuffing, steel slag enters the steel slag production line, and finally forms iron-containing materials and tailings. The iron-containing materials are returned to the blast furnace and converter for reuse, and the tailings enter the cement and other industries. Iron-containing materials carrying a small amount of Cr entering the blast furnace or converter will have a certain impact on the furnace mine, and chromium-containing tailings enter the cement industry. In the cement production process, +3 valent chromium is easily oxidized to +6 valent chromium. Subsequently, cement enters people's lives in various forms, which is very likely to have a greater impact on human physical and mental health.
[0004] At present, the methods for reducing the chromium content in converter slag mainly include the following methods: first, using the principle of element selection oxidation, blowing oxygen into the molten pool, and adding coolant to control the temperature of the molten pool, so as to oxidize and separate the chromium in the molten iron; second, by adjusting the process parameters such as the blowing system and slag making system of the converter, the converter smelting process is optimized to improve the oxidation rate and removal rate of chromium; third, in the converter smelting process, some specific dechroming agents, such as oxidants, dechroming alloys, etc., are added. These dechroming agents can react with the chromium in the molten steel to generate easily separable chromium compounds, thereby reducing the chromium content in the molten steel; fourth, the slag-steel separation operation during the converter steel-making process is strengthened to ensure that as much chromium in the slag as possible remains in the slag instead of entering the molten steel. However, these methods still inevitably produce a certain amount of chromium in the slag produced. Therefore, recycling the produced slag to extract valuable elements such as chromium in the slag is still a technical problem that needs to be solved in this field.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide a method for reducing the chromium content in converter steel slag, which can effectively reduce the chromium content in converter steel slag and improve the effective utilization rate of waste resources.
[0007] The present invention provides a method for reducing the chromium content in converter slag, comprising the following steps:
[0008] S1. Performing primary screening on the steel slag to obtain primary oversize material and primary undersize material;
[0009] S2, the primary undersize material is subjected to the first-stage ball milling and the first-stage screening to obtain the first-stage oversize material and the first-stage undersize material, and the first-stage oversize material is subjected to the first-stage magnetic separation to obtain the first magnetic separation residue and the first iron-containing material;
[0010] S3, the first-stage undersize material is subjected to second-stage ball milling and second-stage screening to obtain second-stage oversize material and second-stage undersize material, and the second-stage oversize material is subjected to second-stage magnetic separation to obtain second magnetic separation residue and second iron-containing material;
[0011] S4, the second-stage undersize material is subjected to third-stage ball milling and third-stage screening to obtain third-stage oversize material and third-stage undersize material, and the third-stage oversize material is subjected to third-stage magnetic separation to obtain third magnetic separation residue and third iron-containing material;
[0012] S5. The third-stage undersize material is processed by the fourth-stage magnetic separation and the fifth-stage magnetic separation in turn to obtain iron-containing material, low-chromium steel slag and high-chromium steel slag respectively.
[0013] As a preferred embodiment of the present technical solution, in step S1, during the primary screening, a square hole sieve with a side length of 140-160 mm is selected.
[0014] As a preferred embodiment of the present technical solution, in step S1, the material on the primary screen is hit multiple times with a stone steel hammer, and the material hit with the stone steel hammer is sieved separately with a square hole sieve with square holes of 140-160 mm, and the obtained undersize material is mixed with the primary undersize material and then subjected to the first stage ball milling.
[0015] After being hit several times by the stone-steel hammer, a small amount of iron-containing materials are broken, and the non-iron-containing materials on the surface and inside are broken and fall off. When screened again by the square hole sieve, the Cr-containing perovskite passes through the sieve into the part under the sieve and is separated from the iron-containing materials on the part above the sieve.
[0016] In addition, in order to make the screening process more thorough, after the normal production slag screening is completed, the material hit by the stone steel hammer is screened again using the corresponding square hole screen, and the materials on and under the screen are stacked separately.
[0017] Finally, the primary undersize material screened out during normal production and the undersize material screened out after being hit with a stone steel hammer are mixed evenly in a certain proportion and then ground in three stages. After grinding, they are separated by multi-stage magnetic separation using magnetic separators with different magnetic field strengths.
[0018] As a preferred embodiment of the present technical solution, in step S2, the primary undersize material screened out during normal production and the undersize material screened out after being hit by a stone steel hammer are mixed in a ratio of 3:1 and then subjected to the first-stage ball milling. The first ball mill used for the first-stage ball milling can be a φ1500×5700mm ball mill. The steel balls are added at 30-50% of the allowed addition amount. The ratio of steel balls is φ120:φ100=4:6. The grinding time is controlled by the feeding speed of the first ball mill and the amount of flushing water, preferably 30-40 minutes.
[0019] After the first stage of ball milling, a square hole sieve with a side length of 50-60 mm is tied at the outlet of the first ball mill for the first stage of screening to obtain the first stage of oversize material and the first stage of undersize material;
[0020] The material on the first stage screen is subjected to the first stage magnetic separation by a magnetic separator with a magnetic field strength of 600-800Gs to obtain a first magnetic separation residue and a first iron-containing material, wherein the first iron-containing material is stacked separately, and the first magnetic separation residue is returned to the first ball mill for cyclic grinding. After grinding in the first ball mill, all the iron-containing materials on the screen can be returned to steelmaking and directly used in the converter.
[0021] Step S2 is mainly to separate magnetic minerals from non-magnetic minerals under low magnetic field strength to screen out clean iron.
[0022] As a preferred embodiment of the present technical solution, in step S3, the first-stage undersize material at the outlet of the first ball mill enters the second ball mill, the second ball mill can be a φ1500×4500mm ball mill, the steel balls are added at 70-80% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, and the grinding time is controlled by the feeding speed of the second ball mill and the size of the flushing water, preferably 30-40 minutes;
[0023] After the second stage of ball milling, a square hole sieve with a side length of 15-20mm is bundled at the outlet of the second ball mill for second stage screening treatment to obtain second stage screen material and second stage screen material. The second stage screen material is subjected to second stage magnetic separation using a magnetic separator with a magnetic field strength of 1600-2000Gs to obtain a second magnetic separation residue and a second iron-containing material. The second iron-containing material is stacked separately, and the second magnetic separation residue is returned to the second ball mill for cyclic grinding.
[0024] As a preferred embodiment of the present technical solution, in step S4, the second-stage underscreen material at the outlet of the second ball mill enters the third ball mill, the third ball mill can be a φ1500×4500mm ball mill, the steel balls are added at 80-90% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, and the grinding time is controlled by the feeding speed of the third ball mill and the size of the flushing water, preferably 30-40 minutes;
[0025] After the third stage of ball milling, a square hole sieve with a side length of 3-5mm is bundled at the outlet of the third ball mill for third stage screening treatment to obtain third stage on-screen material and third stage under-screen material. The third stage on-screen material is subjected to third stage magnetic separation using a magnetic separator with a magnetic field strength of 2600-3000Gs to obtain a third magnetic separation residue and a third iron-containing material, wherein the third iron-containing material is stacked separately, and the third magnetic separation residue is returned to the third ball mill for cyclic grinding, and all the second iron-containing materials and the third iron-containing materials obtained after grinding in the second ball mill and the third ball mill can be returned to the blast furnace for direct use.
[0026] As a preferred embodiment of the present technical solution, in step S5, during the fourth stage magnetic separation, a magnetic separation device with a magnetic field strength of 2600-3000 Gs is selected, and during the fifth stage magnetic separation, a magnetic separation device with a magnetic field strength of 10000-12000 Gs is selected.
[0027] Cr in steel slag mainly exists in perovskite in an amorphous valence state, and perovskite is mainly a symbiotic product formed by CaO and TiO2, and has no magnetism itself. In the present invention, after three-stage grinding by first-stage ball milling, second-stage ball milling and third-stage ball milling, the iron-containing material and other materials are crushed and dissociated. Since the iron-containing material is magnetic, while the perovskite and other materials are not magnetic, the difference in magnetism between the two is utilized to separate them by magnetic separation. The iron-containing material belongs to the magnetically extracted material, while the non-magnetic materials such as the perovskite belong to the magnetically separated residual material. Therefore, the Cr in the converter steel slag of the present invention finally exists in the third magnetically separated residual material in the form of a non-magnetic material.
[0028] As a preferred embodiment of the present technical solution, during the first stage ball milling, the second stage ball milling and the third stage ball milling, and Any one of the ball mills, wherein the first stage ball mill is preferably Ball mill, the second stage ball mill is preferably a φ1500×4500mm ball mill, and the third stage ball mill is preferably a φ1500×4500mm ball mill. The larger the ball mill model, the higher the crushing efficiency during grinding.
[0029] Since the ball mill material contains a small amount of steel blocks, the principle of adding steel balls in the first ball mill is to add a small amount of steel balls. During the grinding process, when the steel balls hit the materials, a small amount of steel blocks can also participate in the impact of the materials.
[0030] In addition, the larger the ball mill model, the smaller the proportion added and the shorter the grinding time, based on the allowable loading capacity of the ball mill steel balls.
[0031] As a preferred embodiment of the present technical solution, the Cr content in the primary screen material, the first iron-containing material, the second iron-containing material, the third iron-containing material and the low-chromium steel slag is less than 0.01%, and the total output of the above materials can reach 90%, among which the first iron-containing material can be returned to steelmaking and directly used in the converter, the low-chromium steel slag can be used for cement or for sintering, and the second iron-containing material and the third iron-containing material can be used in the blast furnace.
[0032] The method for reducing the chromium content in converter slag of the present invention has at least the following beneficial effects:
[0033] In the method of reducing the chromium content in converter slag of the present invention, the Cr in the slag mainly exists in the perovskite in an amorphous state, and the perovskite is mainly a symbiotic product formed by CaO and TiO2, and has no magnetism itself. After the first stage ball milling, the second stage ball milling and the third stage ball milling, the iron-containing material and other materials are crushed and dissociated. Since the iron-containing material is magnetic, and the perovskite and other materials are not magnetic, the difference in the magnetism between the two is utilized, and the separation is carried out by magnetic separation, so that the Cr in the converter slag can be present in the third magnetic separation residue in the form of non-magnetic material; the third under-screen material first uses a magnetic separation device with a certain magnetic field strength to separate the iron-containing material, and the magnetic separation residue is further separated into low-magnetic material and non-magnetic material by using a magnetic separation device with a higher magnetic field strength, wherein the low-magnetic material belongs to low-chromium slag, and the non-magnetic material belongs to high-chromium slag. Therefore, the present invention can effectively reduce the chromium content in converter slag, thereby improving the effective utilization rate of waste resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 The present invention is a flow chart of the method for reducing the chromium content in converter slag. DETAILED DESCRIPTION
[0036] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0037] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] like Figure 1 As shown, this embodiment provides a method for reducing the chromium content in a converter steel slag, and the chemical indicators of the converter steel slag are shown in Table 1:
[0041] Table 1 Chemical indexes of converter slag
[0042] Element MFe <![CDATA[Fe2O3]]> CaO <![CDATA[SiO2]]> MgO Total Cr % 2.16 21.49 40.73 11.43 9.23 0.17
[0043] S1. The converter slag is subjected to primary screening through a square hole sieve with a side length of 150 mm. After screening, primary screened material and primary screened material are obtained. The primary screened material is spread at a designated position and smashed multiple times with a steel hammer. During the smashing, a loader is used to turn the material to ensure that the smashing process is more thorough. After the smashing is completed, the loader is used to stack the material to the designated position. After the primary screening of the steel slag produced normally is completed, the material smashed by the steel hammer is separately screened with a square hole sieve with a square hole of 150 mm. The screened material is an iron-containing block material and is separately stacked. The screened material is mixed with the primary screened material and then subjected to the first-stage ball milling;
[0044] S2. The primary undersize material obtained by primary screening during normal production and the undersize material obtained by slamming with a stone steel hammer are mixed in a ratio of 3:1 and then subjected to the first stage of ball milling. The first ball mill used for the first stage of ball milling is a φ1500×5700mm ball mill. Steel balls are added at 30% of the allowable amount. The ratio of steel balls is φ120:φ100=4:6. The grinding time is controlled by the feeding speed of the first ball mill and the amount of flushing water, preferably 35 minutes. After the first stage of ball milling, After the first-stage screening treatment of the square hole sieve with a side length of 50 mm at the outlet bundle, the first-stage screen material and the first-stage screen material are obtained. The first-stage screen material is subjected to the first-stage magnetic separation by a magnetic separator with a magnetic field strength of 600 Gs to obtain the first magnetic separation residue and the first iron-containing material, wherein the first iron-containing material is stacked separately, and the first magnetic separation residue is returned to the first ball mill for cyclic grinding. After the first ball mill is ground, all the iron-containing materials on the screen and the primary screen material can be returned to the steelmaking and directly used in the converter, and the total Cr content is 0.007%;
[0045] S3, the first-stage undersize material at the outlet of the first ball mill enters the second ball mill, the second ball mill selects a φ1500×4500mm ball mill, steel balls are added at 70% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, the grinding time is controlled by the feeding speed of the second ball mill and the size of the flushing water, preferably 35 minutes; after the second-stage ball milling is completed, a square hole sieve with a side length of 15mm is tied at the outlet of the second ball mill for second-stage screening treatment to obtain second-stage oversize material and second-stage undersize material, the second-stage oversize material is selected from a magnetic separator with a magnetic field strength of 1600Gs for second-stage magnetic separation to obtain a second magnetic separation residue and a second iron-containing material, wherein the second iron-containing material can be returned to the blast furnace for direct use, and its total Cr content is 0.005%, and the second magnetic separation residue is returned to the second ball mill for cyclic grinding;
[0046] S4, the second-stage undersize material at the outlet of the second ball mill enters the third ball mill, the third ball mill selects a φ1500×4500mm ball mill, steel balls are added at 70% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, the grinding time is controlled by the feeding speed of the third ball mill and the size of the flushing water, preferably 35 minutes, after the third-stage ball milling is completed, a square hole sieve with a side length of 5mm is tied at the outlet of the third ball mill for third-stage screening treatment to obtain third-stage oversize material and third-stage undersize material, the third-stage oversize material is selected from a magnetic separator with a magnetic field strength of 2600Gs for third-stage magnetic separation to obtain a third magnetic separation residue and a third iron-containing material, wherein the third iron-containing material can be returned to the blast furnace for direct use, and its total Cr content is 0.004%, and the third magnetic separation residue is returned to the third ball mill for circulating grinding material;
[0047] S5. The third-stage undersize material is subjected to the fourth-stage magnetic separation by a magnetic separator with a magnetic field strength of 2600 Gs to obtain iron-containing material and magnetic separation residue. The magnetic separation residue is subjected to the fifth-stage magnetic separation by a magnetic separator with a magnetic field strength of 10000 Gs to obtain low-chromium steel slag and high-chromium steel slag, wherein the total Cr content of the low-chromium steel slag is 0.004%, the total Cr content of the high-chromium steel slag is 1.53%, and the high-chromium steel slag accounts for 10.82% of the total converter steel slag.
[0048] Example 2
[0049] like Figure 1 As shown, this embodiment provides a method for reducing the chromium content in a converter steel slag, and the chemical indicators of the converter steel slag are shown in Table 2:
[0050] Table 2 Chemical indexes of converter slag
[0051] Element MFe <![CDATA[Fe2O3]]> CaO <![CDATA[SiO2]]> MgO Total Cr % 2.79 21.83 40.55 10.93 10.55 0.21
[0052] S1. Primary screening of converter slag through a square hole sieve with a side length of 140 mm. Primary screened material and primary screened material are obtained after screening. The primary screened material is spread at a designated location and smashed multiple times with a steel hammer. A loader is used to turn the material during smashing to ensure that the smashing process is more thorough. After the smashing is completed, the loader is used to stack the material at the designated location. After the primary screening of the steel slag produced normally is completed, the material smashed by the steel hammer is separately screened with a square hole sieve with a square hole of 140 mm. The screened material is an iron-containing block material and is separately stacked. The screened material is mixed with the primary screened material and then subjected to the first-stage ball milling;
[0053] S2. The primary undersize material screened out during normal production and the undersize material screened out after being hit by a stone steel hammer are mixed in a ratio of 4:1 and then subjected to the first stage of ball milling. The first ball mill used for the first stage of ball milling is a φ1500×5700mm ball mill. Steel balls are added at 30% of the allowable amount, and the ratio of steel balls is φ120:φ100=4:6. The grinding time is controlled by the feeding speed of the first ball mill and the amount of flushing water, preferably 35 minutes. After the first stage of ball milling, After the first-stage screening treatment of the square hole sieve with a side length of 60 mm at the outlet bundle, the first-stage screen material and the first-stage screen material are obtained. The first-stage screen material is subjected to the first-stage magnetic separation by a magnetic separator with a magnetic field strength of 800 Gs to obtain the first magnetic separation residue and the first iron-containing material, wherein the first iron-containing material is stacked separately, and the first magnetic separation residue is returned to the first ball mill for cyclic grinding. After the first ball mill is ground, all the iron-containing materials on the screen and the primary screen material can be returned to the steelmaking and directly used in the converter, and the total Cr content is 0.006%;
[0054] S3, the first-stage undersize material at the outlet of the first ball mill enters the second ball mill, the second ball mill selects a φ1500×4500mm ball mill, steel balls are added at 70% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, the grinding time is controlled by the feeding speed of the second ball mill and the size of the flushing water, preferably 35 minutes; after the second-stage ball milling is completed, a square hole sieve with a side length of 20mm is tied at the outlet of the second ball mill for second-stage screening treatment to obtain second-stage oversize material and second-stage undersize material, the second-stage oversize material is selected from a magnetic separator with a magnetic field strength of 2000Gs for second-stage magnetic separation to obtain a second magnetic separation residue and a second iron-containing material, wherein the second iron-containing material can be returned to the blast furnace for direct use, and its total Cr content is 0.004%, and the second magnetic separation residue is returned to the second ball mill for cyclic grinding;
[0055] S4. The second-stage screened material at the outlet of the second ball mill enters the third ball mill. The third ball mill is a φ1500×4500mm ball mill. Steel balls are added at 70% of the allowable amount. The steel ball ratio is φ150:φ120=5:5. The grinding time is controlled by the feeding speed of the third ball mill and the amount of flushing water. 35 minutes is appropriate. After the third-stage ball milling is completed, a square hole screen with a side length of 3mm is tied at the outlet of the third ball mill for the third-stage screening process. The third-stage sieve material and the third-stage sieve under material are obtained by the third-stage magnetic separation of the third-stage sieve material using a magnetic separator with a magnetic field strength of 3000Gs to obtain a third magnetic separation residue and a third iron-containing material, wherein the third iron-containing material is stacked separately, and the third magnetic separation residue is returned to the third ball mill for recycling grinding material, and all the second iron-containing materials and the third iron-containing materials obtained after grinding in the second ball mill and the third ball mill can be returned to the blast furnace for direct use, and the total Cr content thereof is 0.003%;
[0056] S5. The third-stage undersize material is subjected to the fourth-stage magnetic separation by a magnetic separator with a magnetic field strength of 3000 Gs to obtain iron-containing material and magnetic separation residue. The magnetic separation residue is subjected to the fifth-stage magnetic separation by a magnetic separator with a magnetic field strength of 12000 Gs to obtain low-chromium steel slag and high-chromium steel slag, wherein the total Cr content of the low-chromium steel slag is 0.003%, the total Cr content of the high-chromium steel slag is 1.58%, and the high-chromium steel slag accounts for 11.05% of the total amount of converter steel slag.
[0057] Example 3
[0058] like Figure 1 As shown, this embodiment provides a method for reducing the chromium content in a converter steel slag. The chemical indicators of the converter steel slag are shown in Table 3:
[0059] Table 3 Chemical indexes of converter slag
[0060] Element MFe <![CDATA[Fe2O3]]> CaO <![CDATA[SiO2]]> MgO Total Cr % 3.05 21.49 40.12 11.83 10.12 0.19
[0061] S1. Primary screening of converter slag through a square hole sieve with a side length of 160 mm. Primary screened material and primary screened material are obtained after screening. The primary screened material is spread at a designated position and smashed multiple times with a steel hammer. A loader is used to turn the material during smashing to ensure that the smashing process is more thorough. After the smashing is completed, the loader is used to stack the material at the designated position. After the primary screening of the steel slag produced normally is completed, the material smashed by the steel hammer is separately screened with a square hole sieve with a square hole of 160 mm. The screened material is an iron-containing block material and is separately stacked. The screened material is mixed with the primary screened material and then subjected to the first-stage ball milling;
[0062] S2. The primary undersize material obtained by primary screening during normal production and the undersize material obtained by slamming with a stone steel hammer are mixed in a ratio of 3:1 and then subjected to the first stage of ball milling. The first ball mill used for the first stage of ball milling is a φ1500×5700mm ball mill. Steel balls are added at 30% of the allowable amount. The ratio of steel balls is φ120:φ100=4:6. The grinding time is controlled by the feeding speed of the first ball mill and the amount of flushing water, preferably 35 minutes. After the first stage of ball milling, After the first-stage screening treatment of the square hole sieve with a side length of 55 mm at the outlet bundle, the first-stage screen material and the first-stage screen material are obtained. The first-stage screen material is subjected to the first-stage magnetic separation by a magnetic separator with a magnetic field strength of 700 Gs to obtain the first magnetic separation residue and the first iron-containing material, wherein the first iron-containing material is stacked separately, and the first magnetic separation residue is returned to the first ball mill for cyclic grinding. After the first ball mill is ground, all the iron-containing materials on the screen and the primary screen material can be returned to the steelmaking and directly used in the converter, and the total Cr content is 0.007%;
[0063] S3, the first-stage undersize material at the outlet of the first ball mill enters the second ball mill, the second ball mill selects a φ1500×4500mm ball mill, steel balls are added at 70% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, the grinding time is controlled by the feeding speed of the second ball mill and the size of the flushing water, preferably 35 minutes; after the second-stage ball milling is completed, a square hole sieve with a side length of 20mm is bundled at the outlet of the second ball mill for second-stage screening treatment to obtain second-stage oversize material and second-stage undersize material, the second-stage oversize material is selected from a magnetic separator with a magnetic field strength of 1800Gs for second-stage magnetic separation to obtain a second magnetic separation residue and a second iron-containing material, wherein the second iron-containing material can be returned to the blast furnace for direct use, and its total Cr content is 0.004%, and the second magnetic separation residue is returned to the second ball mill for cyclic grinding;
[0064] S4, the second-stage undersize material at the outlet of the second ball mill enters the third ball mill, the third ball mill selects a φ1500×4500mm ball mill, steel balls are added at 70% of the allowable addition amount, the steel ball ratio is φ150:φ120=5:5, the grinding time is controlled by the feeding speed of the third ball mill and the size of the flushing water, preferably 35 minutes, after the third-stage ball milling is completed, a square hole sieve with a side length of 4mm is bundled at the outlet of the third ball mill for third-stage screening treatment to obtain third-stage oversize material and third-stage undersize material, the third-stage oversize material is selected from a magnetic separator with a magnetic field strength of 2800Gs for third-stage magnetic separation to obtain a third magnetic separation residue and a third iron-containing material, wherein the third iron-containing material can be returned to the blast furnace for direct use, and its total Cr content is 0.005%, and the third magnetic separation residue is returned to the third ball mill for circulating grinding material;
[0065] S5. The third-stage undersize material is subjected to the fourth-stage magnetic separation using a magnetic separator with a magnetic field strength of 2800 Gs to obtain iron-containing material and magnetic separation residue. The magnetic separation residue is subjected to the fifth-stage magnetic separation using a magnetic separator with a magnetic field strength of 11000 Gs to obtain low-chromium steel slag and high-chromium steel slag, wherein the total Cr content of the low-chromium steel slag is 0.005%, the total Cr content of the high-chromium steel slag is 1.64%, and the high-chromium steel slag accounts for 11.13% of the total converter steel slag.
[0066] Comparative Example 1
[0067] This control example is basically the same as Example 1, except that: in this control example, during the primary screening, the side length of the square hole sieve is 150 mm; during the first stage screening treatment, the side length of the square hole sieve is 80 mm, and the magnetic field strength is 1000 Gs during the first stage magnetic separation; during the second stage screening treatment, the side length of the square hole sieve is 25 mm, and the magnetic field strength is 1000 Gs during the second stage magnetic separation; during the third stage screening treatment, the side length of the square hole sieve is 10 mm, and the magnetic field strength is 1000 Gs during the third stage magnetic separation; during the fourth stage magnetic separation, the magnetic field strength is 1000 Gs; during the fifth stage magnetic separation, the magnetic field strength is 6000 Gs.
[0068] Comparative Example 2
[0069] This control example is basically the same as Example 1, except that: in this control example, during the primary screening, the side length of the square hole sieve is 160 mm; during the first stage screening treatment, the side length of the square hole sieve is 80 mm, and the magnetic field strength is 1500 Gs during the first stage magnetic separation; during the second stage screening treatment, the side length of the square hole sieve is 30 mm, and the magnetic field strength is 1500 Gs during the second stage magnetic separation; during the third stage screening treatment, the side length of the square hole sieve is 8 mm, and the magnetic field strength is 1500 Gs during the third stage magnetic separation; during the fourth stage magnetic separation, the magnetic field strength is 1500 Gs; during the fifth stage magnetic separation, the magnetic field strength is 7000 Gs.
[0070] Comparative Example 3
[0071] This control example is basically the same as Example 1, except that: in this control example, during the primary screening, the side length of the square hole sieve is 150 mm; during the first stage screening treatment, the side length of the square hole sieve is 70 mm, and the magnetic field strength is 2000 Gs during the first stage magnetic separation; during the second stage screening treatment, the side length of the square hole sieve is 25 mm, and the magnetic field strength is 2000 Gs during the second stage magnetic separation; during the third stage screening treatment, the side length of the square hole sieve is 10 mm, and the magnetic field strength is 2000 Gs during the third stage magnetic separation; during the fourth stage magnetic separation, the magnetic field strength is 2000 Gs; during the fifth stage magnetic separation, the magnetic field strength is 8000 Gs.
[0072] Table 4 shows the sorting quality of low chromium steel slag and high chromium steel slag in Examples 1-3 and Comparative Examples 1-3.
[0073] Table 4
[0074]
[0075]
[0076] As can be seen from Table 1, the present invention selects a multi-stage ball milling, screening and magnetic separation treatment method according to the existence form and characteristics of chromium in the converter slag, and specifically defines the conditions of ball milling, screening and magnetic separation at each level. After treatment, the present invention effectively reduces the chromium content in the converter slag, and the total Cr content in the low-chromium slag can be as low as 0.003%, and the total Cr content of the primary screen material, the first iron-containing material, the second iron-containing material, the third iron-containing material and the low-chromium slag can be as low as 0.005%. Compared with control examples 1-3, excellent technical effects have been achieved.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for reducing the chromium content in converter slag, characterized in that: The following steps are involved: S1. Performing primary screening on the steel slag to obtain primary oversize material and primary undersize material; S2, the primary undersize material is subjected to the first-stage ball milling and the first-stage screening to obtain the first-stage oversize material and the first-stage undersize material, and the first-stage oversize material is subjected to the first-stage magnetic separation to obtain the first magnetic separation residue and the first iron-containing material; S3, the first-stage undersize material is subjected to second-stage ball milling and second-stage screening to obtain second-stage oversize material and second-stage undersize material, and the second-stage oversize material is subjected to second-stage magnetic separation to obtain second magnetic separation residue and second iron-containing material; S4, the second-stage undersize material is subjected to third-stage ball milling and third-stage screening to obtain third-stage oversize material and third-stage undersize material, and the third-stage oversize material is subjected to third-stage magnetic separation to obtain third magnetic separation residue and third iron-containing material; S5. The third-stage undersize material is processed by the fourth-stage magnetic separation and the fifth-stage magnetic separation in turn to obtain iron-containing material, low-chromium steel slag and high-chromium steel slag respectively.
2. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S1, during the primary screening, a square hole sieve with a side length of 140-160 mm is selected.
3. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S1, the material on the primary screen is hit multiple times with a steel hammer, and the material hit with the steel hammer is sieved separately with a square hole sieve with a square hole of 140-160 mm, and the obtained undersize material is mixed with the primary undersize material and then subjected to the first stage ball milling.
4. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S2, during the first stage screening, a square hole sieve with a side length of 50-60 mm is selected; During the first stage magnetic separation, a magnetic separation device with a magnetic field strength of 600-800Gs is selected.
5. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S3, during the second stage screening, a square hole sieve with a side length of 15-20 mm is selected; During the second stage magnetic separation, magnetic separation equipment with a magnetic field strength of 1600-2000Gs is selected.
6. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S4, during the third stage screening, a square hole sieve with a side length of 3-5 mm is selected; During the third stage magnetic separation, a magnetic separation device with a magnetic field strength of 2600-3000Gs is selected.
7. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S5, during the fourth stage magnetic separation, a magnetic separation device with a magnetic field strength of 2600-3000Gs is selected.
8. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: In step S5, during the fifth stage magnetic separation, a magnetic separation device with a magnetic field strength of 10000-12000 Gs is selected.
9. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: During the first-stage ball milling, the second-stage ball milling and the third-stage ball milling, any one of the ball mills of φ1500×3000mm, φ1500×4500mm, φ1500×5700mm and φ1800×4500mm is selected.
10. The method for reducing the chromium content in converter slag according to claim 1, characterized in that: The Cr content in the primary oversize material, the first iron-containing material, the second iron-containing material, the third iron-containing material and the low-chromium steel slag is less than 0.01%.
Citation Information
Patent Citations
Stainless steel slag treatment method
CN102586517A
Embedded-type all-grain-size dry magnetic separation technology for closed recycle of iron-containing minerals in steel slag
CN103586118A
High-efficiency economic secondary treatment process for steel slag
CN104004867A
Magnetite separation technology for increasing content of coarse-grained tailings and improving processing capability of mill
CN109013037A
Steel slag selecting method
CN110216009A