Hot-rolled bearing steel bar network carbide control model
By setting the initial rolling, final rolling and water cooling temperature ranges during the rolling process, determining the fixed rolling speed and cooling parameters, a network carbide control model suitable for specific specifications of bars was established, solving the existing problems The problem of unstable network carbide control in technology has been achieved to stabilize the quality and improve the service life of bearing steel.
Patent Information
- Application Number
- CN202410960662.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The existing technology makes it difficult to achieve stable control of the network carbides in bearing steel during the rolling process, resulting in reduced service life, and requires real-time adjustment of water cooling pressure and flow, which increases workers' labor and makes quality control unstable.
A network carbide control model for hot-rolled bearing steel bars was established. By setting the initial rolling temperature range, final rolling temperature range and water cooling temperature range, fixed rolling speed and cooling parameters were determined, and controlled cold rolling was established. The rolling model is suitable for rolling bars with diameters ranging from a to b, reducing the complexity of on-site operations and quality fluctuations.
It achieves the controllability of the bearing steel mesh carbide, reduces the labor of on-site workers, and ensures the stability of rolling quality and the improvement of service life.
Smart Images

Figure CN118808318A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot rolling of bearing steel, in particular to a network carbide control model for hot-rolled bearing steel bars. Background Art
[0002] Carbides are an important component phase in bearing steel. They have the functions of wear resistance, inhibiting grain growth, and absorbing alloy elements to obtain satisfactory performance of steel after heat treatment. However, coarse, polygonal and segregated carbides are very harmful to the service life of bearings. Microsegregation in bearing steel is mainly manifested as the uneven distribution of alloy carbides. According to the shape, distribution and formation reasons of carbides in the microstructure of rolled materials, carbides in bearing steel can be divided into banded carbides and network carbides. Among them, network carbides are excess carbides precipitated in a network along the austenite grain boundaries during the cooling process of hypereutectoid steel. Bearing steel belongs to hypereutectoid steel. During the cooling process after rolling, the diffusion rate of carbide-forming elements along the austenite grain boundaries is much greater than the diffusion rate within the grain. Therefore, secondary carbides are mostly precipitated along the grain boundaries, thus forming a discontinuous or continuous network. Carbide networks will increase the brittleness of bearing steel and reduce the fatigue life of bearing parts. Therefore, severe carbide networks are not allowed to exist in the bearing structure under use.
[0003] In order to reduce the carbide network structure in bearing steel, a control method known in the art is to control the temperature of the rolled piece entering the sizing unit, and cool the rolled piece to the temperature range of the austenite and carbide two-phase region through the first water cooling forced cooling, about 720-900°C, and deform in the two-phase region so that the first precipitated carbides and the unrecrystallized austenite are simultaneously subjected to plastic deformation. The unrecrystallized austenite is deformed, the grains are elongated, the deformation bands and dislocation density in the grains are increased, and at the same time, the first precipitated carbides form a large number of dislocations due to plastic deformation, so that the first precipitated carbides form fine and dispersed carbide particles, thereby reducing the size of the carbides. The rolled piece is quickly cooled by the second water cooling, and the precipitation and growth of carbides are further reduced by passing through the carbide precipitation temperature zone of 900°C to 700°C. For example, Chinese patent document CN106086353A (201610750155.6) discloses a rolling method for controlling the precipitation of network carbides in large-section GCr15 bearing steel, which limits the temperature range of the rolled piece after the first water cooling and the second water cooling, and limits the value range of the water cooling pressure and flow rate of the first water cooling and the second water cooling based on the value range of the water cooling speed. However, the existing method only gives the value range of the water cooling pressure and flow rate of the first water cooling and the second water cooling. In actual production, the water cooling effect is affected by the rolling speed and the billet size. When the rolling speed and the billet size change, the specific values of the water cooling pressure and flow rate of the first water cooling and the second water cooling need to be adjusted in real time, which increases the workload of on-site workers and causes unstable quality control. Summary of the invention
[0004] The purpose of the present invention is to establish a network carbide control model for hot-rolled bearing steel bars, which is used for rolling control of bars of certain rolling specifications. When it is convenient for actual operation, data can be directly input into the computer control system, which is convenient for on-site operation and realizes the controllable network carbide level of the bearing steel.
[0005] The technical problem to be solved by the present invention is achieved by the following technical scheme: a network carbide control model for hot-rolled bearing steel bars, the hot rolling process includes raw material heating, raw material rough rolling unit rolling, intermediate rolling unit rolling, finishing rolling unit rolling and sizing unit rolling, the first water cooling of the ingot is performed after the finishing unit, and the second water cooling is performed after the sizing unit;
[0006] Set the initial rolling temperature range, final rolling temperature range, temperature range entering the sizing mill and temperature range after the second water cooling in the control model;
[0007] A set of fixed rolling mill speeds is determined based on the initial rolling temperature range and the final rolling temperature range to be suitable for rolling bars with diameters of a to b at the same time; the rolling speed is fixed, and the rolling speed affects the temperature of the steel after the water tank is penetrated by water. The higher the rolling line speed, the higher the temperature after the water is penetrated. The goal of adjustment is to ensure the temperature entering the sizing unit and the temperature after the final water penetration, and to select a suitable rolling speed on the basis of meeting the requirements of the initial rolling temperature range and the final rolling temperature range; since the rolling system is fixed and the rolling distance is fixed, for different rolling systems, the main thing that needs to be adjusted is the rolling speed. The technical solution recorded in the present invention is to determine the establishment of a control model under the rolling system, and no specific rolling distance is limited here;
[0008] Setting of parameters in the raw material heating stage: based on the diameter of the bar billet in the range of a to b and the initial rolling temperature range, determine the temperature range of the preheating section and the heating time requirements of the preheating section, the temperature range of the heating section I and the heating time requirements of the heating section I, the temperature range of the heating section II and the heating time requirements of the heating section II, and the temperature range of the soaking section and the heating time requirements of the soaking section, so that the temperature of all billets after heating meets the requirements of the initial rolling temperature range;
[0009] Setting of the first water cooling and the second water cooling parameters: Based on the size of the billet after finish rolling, the final rolling temperature range, the temperature range entering the sizing unit and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the first water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; Based on the size of the finished bar, the temperature range entering the sizing unit, the temperature range after the second water cooling and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the second water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; Then, a controlled cold rolling model for the first water cooling and the second water cooling is established.
[0010] The rolling process control ideas of the present invention are: first, to ensure the appropriate final rolling temperature. The lower the final rolling temperature, the more conducive it is to reduce the water penetration temperature. Second, to ensure that the rolling temperature of the warp reduction unit is rolled within the two-phase temperature range. The temperature control is achieved through comprehensive control of raw material heating, the first water penetration cooling and the second water penetration cooling. The present invention measures the production process data through multiple on-site tests, accumulates data such as rolling speed, water volume, and water pressure, and finally determines the appropriate temperature system, rolling speed, and water tank data to set a network carbide control model for hot-rolled bearing steel bars within a certain specification range. The network carbide control model for bars of various specifications can be formulated. It is only necessary to select the control model according to the organizational requirements of the size specifications, which greatly reduces the workload of on-site workers and ensures the stability of the quality of the rolled bars.
[0011] Preferably, when the specification of the bearing steel bar is Φ50-55mm, the rolling mill speed is 2.97m / s, the initial rolling temperature range is 950-1050°C, the final rolling temperature range is 900-950°C, the temperature range entering the sizing unit is 800-850°C, and the temperature range after the second water cooling is 610-680°C;
[0012] During the raw material heating stage, the temperature of the preheating section is 500-850°C, the heating time of the preheating section is ≥100 minutes, the temperature of the heating section I is 900-1170°C, the heating time of the heating section I is ≥80 minutes, the temperature of the heating section II is 1170-1240°C, the heating time of the heating section II is ≥90 minutes, the temperature of the soaking section is 1180-1220°C, the heating time of the soaking section is ≥60 minutes, and the total heating time is ≥330 minutes.
[0013] Preferably, in the first water cooling, three groups of water tanks No. 1 to No. 3 are set after the finishing mill, and the temperature of the water cooling box is controlled to be 800-850°C. After rolling, the bar enters the No. 1 water cooling box with a water pressure of 2.13MPa and a water flow rate of 190m 3 / h, the outlet water cooling box temperature is controlled at 950℃;
[0014] The bar enters the No. 2 water cooling box from the No. 1 water cooling box, the water pressure is 1.65MPa, and the water flow rate is 170m 3 / h, the outlet water cooling box temperature is controlled at 750℃;
[0015] The bar enters the No. 3 water cooling box from the No. 2 water cooling box, the water pressure is 1.45MPa, and the water flow rate is 150m 3 / h, and the outlet water cooling box temperature is controlled at 700℃. The water inlet of each water cooling box for the first water cooling is set in parallel, and cooling water of the same temperature is introduced. The approximate temperature of the bar billet is judged based on the outlet water temperature of each water cooling box to ensure that the rolled piece quickly passes through the carbide precipitation temperature zone of 900℃~700℃, and ensures that the rolling temperature entering the warping unit is within the two-phase temperature range.
[0016] Preferably, in the second water cooling, three groups of water tanks No. 4 to No. 6 are set after the sizing unit, and the temperature of the water cooling box is controlled to be 500-580°C. The bar enters the No. 4 water cooling box with a water pressure of 1.3MPa and a water flow rate of 140m 3 / h, the outlet water cooling box temperature is controlled at 660℃;
[0017] The bar enters the No. 5 water cooling box from the No. 4 water cooling box, the water pressure is 0.9MPa, and the water flow rate is 90m 3 / h, the outlet water cooling box temperature is controlled at 600℃;
[0018] The bar enters the No. 6 water cooling box from the No. 5 water cooling box, the water pressure is 0.5MPa, and the water flow rate is 70m 3 / h, and the outlet water cooling box temperature is controlled at 580℃. The water inlet of each water cooling box for the second water cooling is also set in parallel, and the cooling water of the same temperature is introduced. The approximate temperature of the bar billet is judged based on the outlet water temperature of each water cooling box to ensure the subsequent cooling temperature on the bed.
[0019] Preferably, the hot rolling process of the present invention further comprises air cooling on a step-type cooling bed and slow cooling in a pit;
[0020] After the bar is cooled by the water tank, it enters the double-length cooling bed for cooling. The temperature of the upper cooling bed is 610-680℃, and the temperature of the lower cooling bed is 290-350℃.
[0021] The bars are sawn, segmented, collected and bundled, and then put into the pit for slow cooling. The temperature of the pit is 260-320℃. The bars are fully slow cooled in the slow cooling pit for 24 hours, and the temperature out of the pit is ≤100℃. Controlling the temperature of the upper and lower cooling beds can control the final temperature of the steel entering the pit, which has a positive effect on eliminating the stress of the steel after rolling. The temperature of 260-320℃ is effective in eliminating the stress after rolling. If the temperature out of the pit is too high, it will affect the stress release of the steel.
[0022] Preferably, the rough rolling mill group of the present invention is composed of 7 rolling mills, and the rolling mills are short stress line high rigidity rolling mills, which are arranged alternately horizontally and vertically;
[0023] The intermediate rolling mill group consists of 6 rolling mills, which adopt short stress line and high rigidity rolling mills, arranged alternately horizontally and vertically;
[0024] The finishing mill consists of 4 rolling mills, which adopt short stress line and high rigidity rolling mills, arranged alternately horizontally and vertically;
[0025] The sizing unit includes 4 rolling mills. The number of rolling mills affects the rolling stroke, which in turn affects the temperature change of the billet. The horizontal and vertical alternating arrangement avoids steel turning over and improves rolling efficiency.
[0026] Preferably, in the controlled cold rolling model of the first water cooling and the second water cooling of the present invention, the same rolling mill speed can correspond to a combination of multiple groups of fixed values of cooling parameters of the cooling equipment corresponding to the first water cooling and cooling parameters of the cooling equipment corresponding to the second water cooling.
[0027] Preferably, the model of the sizing reducing unit is a KOCKS sizing reducing unit.
[0028] Preferably, the water cooling boxes are all venturi type water cooling boxes.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention is to establish a data model for setting rolling specifications, which is convenient for actual operation and can directly input data into the computer control system for on-site operation.
[0030] The present invention determines a set of fixed rolling mill speeds based on the initial rolling temperature range and the final rolling temperature range, so as to be applicable to the rolling of bars with diameters of a to b.
[0031] Based on the size of the bar billet with diameter a to b and the initial rolling temperature range, determine the temperature range of the preheating section and the heating time requirements of the preheating section, the temperature range of the heating section I and the heating time requirements of the heating section I, the temperature range of the heating section II and the heating time requirements of the heating section II, and the temperature range of the equalizing section and the heating time requirements of the equalizing section, so that the temperature of all billets after heating meets the requirements of the initial rolling temperature range.
[0032] Based on the size of the billet after finish rolling, the final rolling temperature range, the temperature range entering the sizing mill and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the first water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; based on the size of the finished bar, the temperature range entering the sizing mill, the temperature range after the second water cooling and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the second water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; and then a controlled cold rolling model for the first water cooling and the second water cooling is established.
[0033] The control model of the present invention is based on the initial rolling temperature range, the final rolling temperature range, the temperature range entering the sizing unit and the temperature range after the second water cooling in the set control model, and combined with the preset rolling specifications and the performance of the cooling equipment. Since the parameters of the rolling system corresponding to the preset rolling specifications are uniquely determined, the rolling speed of the rolling system and the fixed parameter data of the cooling equipment are determined during rolling, forming a fixed combination model of rolling speed and rolling cooling data suitable for bars of preset rolling specifications. During production, it is only necessary to input various data in the computer control module based on the rolling specifications or directly call the corresponding rolling model, thereby ensuring the stability and controllability of the rolling quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is the cooling trend diagram of the water tank;
[0035] Figure 2 This is the inspection diagram of network carbides in bearing steel. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings.
[0037] The present invention provides a network carbide control model for hot-rolled bearing steel bars, which is suitable for rolling bars with a bearing specification of Φ50-55mm, including raw material heating, raw material rough rolling mill rolling, intermediate rolling mill rolling, finishing mill rolling, KOCKS sizing mill rolling, first water cooling, second water cooling, walking cooling bed air cooling and pit slow cooling process.
[0038] 1. The raw material is heated in a three-stage heating furnace. The billet specification is 260X300mm. Billet heating is an extremely important process. It is necessary not only to ensure that the billet is evenly heated to the specified temperature to provide good organizational and plastic conditions for rolling, but also to reduce the degree of dendritic segregation in the steel during the heating process to achieve the purpose of eliminating the uneven network of carbides.
[0039] The structure of bearing steel cooled to room temperature in equilibrium is pearlite and secondary carbides. As a result of dendrite segregation, a large number of large eutectic carbides will appear between dendrites. If the segregation is heavy, the large eutectic carbides can be gradually dissolved during heating, but carbide-forming elements such as carbon and chromium are not fully diffused and uniform. In the high concentration zone, it is easy to precipitate carbide networks along the austenite grain boundaries. The diffusion process of segregated elements at high temperatures will increase sharply with the increase of temperature, so the heating temperature of the bearing steel billet is as high as possible, and there is a certain holding time. On the other hand, the final rolling temperature has a significant effect on the carbide network structure of bearing steel. As the final rolling temperature decreases, the grains of the steel after rolling are more refined, so that the carbides precipitated along the grain boundaries are distributed on larger grain boundaries, which are relatively thin and have more contact surfaces with the matrix. This carbide network is easy to dissolve in the subsequent spheroidizing annealing process, and a lower network level can be obtained. That is, the final rolling temperature should not be too high. If the final rolling temperature is too high, due to the deformation induction effect, the deformation will cause the austenite to precipitate secondary cementite in advance at a higher temperature. After slow cooling, the carbides will be coarse and numerous.
[0040] In summary, the specific initial rolling temperature range can be confirmed according to the heating purpose, and the parameters of the heating temperature in each stage can be further determined based on the size of the raw material and the specific initial rolling temperature range, as shown in Table 1: preheating section temperature 500-850°C, preheating section heating time ≥100 minutes, heating section temperature 900-1170°C, heating section heating time ≥80 minutes, heating section temperature 1170-1240°C, heating section heating time ≥100 minutes, soaking section temperature 1180-1220°C, soaking section heating time ≥60 minutes, total heating time ≥330 minutes.
[0041] Table 1 Billet temperature system
[0042]
[0043]
[0044] In Table 1, it is generally believed that the high temperature diffusion begins when the temperature is greater than 1180°C, that is, the high temperature diffusion time includes the soaking time and the heating time.
[0045] 2. The rough rolling unit consists of 7 rolling mills, which adopt short stress line and high rigidity rolling mills, and are arranged alternately horizontally and vertically.
[0046] The intermediate rolling mill group consists of 6 rolling mills, which adopt short stress line and high rigidity rolling mills, and are arranged alternately horizontally and vertically.
[0047] The finishing mill group consists of 4 rolling mills, which adopt short stress line and high rigidity rolling mills, and are arranged alternately horizontally and vertically.
[0048] The KOCKS sizing mill unit consists of 4 rolling mills.
[0049] 3. If Figure 1 As shown in Table 2, Figure 1 This is a water tank cooling trend diagram, which shows the cooling process trend of the rolled steel in water tanks 1-6. Figure 1 As shown in the figure, the surface temperature of the rolled piece will drop sharply when passing through the water tank, and the green curve represents the general temperature trend of the rolled piece after returning to temperature. Table 2 shows the controlled rolling and controlled cold rolling model of Φ50-55mm bearing steel, showing the linear identification diagram of the data parameters of water tanks 1-6.
[0050] The workpiece of the finishing mill is cooled by three groups of water tanks to ensure the temperature of the workpiece entering the sizing mill. The workpiece is cooled to the temperature range of the austenite and carbide two-phase region through forced cooling, and rolled at about 720-900℃. After deformation in the two-phase region, the first carbide and the unrecrystallized austenite are subjected to plastic deformation at the same time. The unrecrystallized austenite is deformed, the grains are elongated, the deformation bands and dislocation density in the grains are increased, and at the same time, the first carbide forms a large number of dislocations due to plastic deformation, so that the first carbide forms fine and dispersed carbide particles.
[0051] There are three water tanks behind the sizing unit to ensure that the steel can be cooled quickly after final rolling, so that the rolled piece can quickly pass through the carbide precipitation temperature zone of 900℃~700℃. The purpose of the water tank is to cool the steel, and 900℃~700℃ is the cooling trend.
[0052] Table 2 Φ50-55mm bearing steel controlled rolling and controlled cold rolling model
[0053]
[0054] In Table 2, the last stand rolling mill speed is the rolling speed, and the rolling mill speed is consistent throughout the entire rolling process.
[0055] 4. For the first water cooling, three water tanks are set after the finishing mill. After rolling, the bars enter the No. 1 water cooling tank with a water pressure of 2.34 MPa and a water flow of 184 m 3 / h, the outlet water cooling box temperature is controlled at 950℃; the bar enters the No. 2 water cooling box from the No. 1 water cooling box, the water pressure is 1.01MPa, and the water flow rate is 110m 3 / h, the outlet water cooling box temperature is controlled at 750℃; the bar enters the No. 3 water cooling box from the No. 2 water cooling box, the water pressure is 0.95MPa, and the water flow rate is 110m 3 / h, the outlet water cooling box temperature is controlled at 700℃. The water cooling box is a venturi type water cooling box.
[0056] 5. For the second water cooling, three water tanks are set after the KOCKS sizing unit. The bars enter the No. 4 water cooling tank with a water pressure of 2.34MPa and a water flow of 130m 3 / h, the outlet water cooling box temperature is controlled at 660℃; the bar enters the No. 5 water cooling box from the No. 4 water cooling box, the water pressure is 2.3MPa, and the water flow rate is 120m 3 / h, the outlet water cooling box temperature is controlled at 600℃; the bar enters the No. 6 water cooling box from the No. 5 water cooling box, the water pressure is 1.73MPa, and the water flow rate is 120m 3 / h, and the outlet water cooling box temperature is controlled at 580°C. The number of nozzles of the water cooling box for the first water cooling and the second water cooling is adjusted according to the water cooling effect.
[0057] 6. After the bar is cooled by the water tank, it enters the double-length cooling bed for cooling. The temperature of the upper cooling bed is 610-680℃, and the temperature of the lower cooling bed is 290-350℃.
[0058] The bars are cut into sections, collected and bundled, and then put into a slow cooling pit, where the temperature is 260-320℃. The bars are fully slow cooled in the slow cooling pit for 24 hours, and the temperature out of the pit is ≤100℃.
[0059] The present invention controls the final rolling temperature at 900-950°C, that is, the final rolling temperature of fine rolling, adjusts the rolling line speed and cooperates with the research and use of cooling water tanks to establish a water tank controlled cooling use model during bearing steel rolling, thereby effectively ensuring that the network carbide level inspection of the bearing steel is qualified.
[0060] Billet Press Figure 1 The heating system is that after high-temperature diffusion during heating, the steel enters the roughing mill, the intermediate mill, the finishing mill, and the first water cooling. In this embodiment, the temperature is 800-850°C and enters the KOCKS reducing and sizing mill. After the second water cooling, the temperature is controlled at 500-580°C. After the rolled material is cooled on the cooling bed, it is cut into sections and slowly cooled in the pit.
[0061] like Figure 2As shown, according to the national standard for bearing steel testing, the illustrated level is 1.0, and the bearing steel network carbide inspection is qualified.
Claims
1. A network carbide control model for hot-rolled bearing steel bars, characterized in that: The hot rolling process includes raw material heating, raw material rough rolling, intermediate rolling, finishing and sizing mills. The first water cooling of the ingot is carried out after the finishing mill, and the second water cooling is carried out after the sizing mill. Set the initial rolling temperature range, final rolling temperature range, temperature range entering the sizing mill and temperature range after the second water cooling in the control model; A set of fixed rolling mill speeds is determined based on the initial rolling temperature range and the final rolling temperature range to simultaneously apply to the rolling of bars with diameters ranging from a to b; Setting of parameters in the raw material heating stage: based on the diameter of the bar billet in the range of a to b and the initial rolling temperature range, determine the temperature range of the preheating section and the heating time requirements of the preheating section, the temperature range of the heating section I and the heating time requirements of the heating section I, the temperature range of the heating section II and the heating time requirements of the heating section II, and the temperature range of the soaking section and the heating time requirements of the soaking section; Setting of the first water cooling and the second water cooling parameters: Based on the size of the billet after finish rolling, the final rolling temperature range, the temperature range entering the sizing unit and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the first water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; Based on the size of the finished bar, the temperature range entering the sizing unit, the temperature range after the second water cooling and the rolling mill speed, a set of fixed cooling parameters of the cooling equipment corresponding to the second water cooling is determined to be simultaneously applicable to the rolling of bars with diameters of a to b; Then, a controlled cold rolling model for the first water cooling and the second water cooling is established.
2. The network carbide control model for hot-rolled bearing steel bars according to claim 1, characterized in that: When the specification of bearing steel bar is Φ50-55mm, the rolling speed is 2.97m / s, the initial rolling temperature range is 950~1050℃, the final rolling temperature range is 900~950℃, the temperature range entering the sizing unit is 800~850℃, and the temperature range after the second water cooling is 610~680℃; During the raw material heating stage, the temperature of the preheating section is 500-850°C, the heating time of the preheating section is ≥100 minutes, the temperature of the heating section I is 900-1170°C, the heating time of the heating section I is ≥80 minutes, the temperature of the heating section II is 1170-1240°C, the heating time of the heating section II is ≥90 minutes, the temperature of the soaking section is 1180-1220°C, the heating time of the soaking section is ≥60 minutes, and the total heating time is ≥330 minutes.
3. The network carbide control model for hot-rolled bearing steel bars according to claim 2, characterized in that: For the first water cooling, three groups of water tanks No. 1 to No. 3 are set after the finishing mill, and the temperature of the water cooling box is controlled at 800-850°C. After rolling, the bar enters the No. 1 water cooling box with a water pressure of 2.13MPa and a water flow of 190m 3 / h, the outlet water cooling box temperature is controlled at 950℃; The bar enters the No. 2 water cooling box from the No. 1 water cooling box, the water pressure is 1.65MPa, and the water flow rate is 170m 3 / h, the outlet water cooling box temperature is controlled at 750℃; The bar enters the No. 3 water cooling box from the No. 2 water cooling box, the water pressure is 1.45MPa, and the water flow rate is 150m 3 / h, and the outlet water cooling box temperature is controlled at 700℃.
4. The network carbide control model for hot-rolled bearing steel bars according to claim 3, characterized in that: For the second water cooling, three groups of water tanks No. 4 to No. 6 are set after the sizing unit, and the temperature of the water cooling box is controlled at 500-580°C. The bar enters the No. 4 water cooling box with a water pressure of 1.3MPa and a water flow rate of 140m 3 / h, the outlet water cooling box temperature is controlled at 660℃; The bar enters the No. 5 water cooling box from the No. 4 water cooling box, the water pressure is 0.9MPa, and the water flow rate is 90m 3 / h, the outlet water cooling box temperature is controlled at 600℃; The bar enters the No. 6 water cooling box from the No. 5 water cooling box, the water pressure is 0.5MPa, and the water flow rate is 70m 3 / h, and the outlet water cooling box temperature is controlled at 580℃.
5. The network carbide control model for hot-rolled bearing steel bars according to claim 4, characterized in that: The hot rolling process also includes air cooling on a walking cooling bed and slow cooling in a pit; After the bar is cooled by the water tank, it enters the double-length cooling bed for cooling. The temperature of the upper cooling bed is 610-680℃, and the temperature of the lower cooling bed is 290-350℃. The bars are sawn into sections, collected and bundled, and then put into a pit for slow cooling. The temperature entering the pit is 260-320℃. The bars are fully slow cooled in the slow cooling pit for 24 hours, and the temperature out of the pit is ≤100℃.
6. The network carbide control model for hot-rolled bearing steel bars according to claim 2, characterized in that: The rough rolling mill group consists of 7 rolling mills, which adopt short stress line and high rigidity rolling mills, arranged alternately horizontally and vertically; The intermediate rolling mill group consists of 6 rolling mills, which adopt short stress line and high rigidity rolling mills, arranged alternately horizontally and vertically; The finishing mill consists of 4 rolling mills, which adopt short stress line and high rigidity rolling mills, arranged alternately horizontally and vertically; The sizing unit includes 4 rolling mills.
7. The network carbide control model for hot-rolled bearing steel bars according to claim 1, characterized in that: In the controlled cold rolling model of the first water cooling and the second water cooling, the same rolling mill speed can correspond to multiple sets of fixed value combinations of cooling parameters of the cooling equipment corresponding to the first water cooling and cooling parameters of the cooling equipment corresponding to the second water cooling.
8. The network carbide control model for hot-rolled bearing steel bars according to claim 1 or 2, characterized in that: The model of the sizing reduction unit is a KOCKS sizing reduction unit.
9. The network carbide control model for hot-rolled bearing steel bars according to claim 4, characterized in that: The water cooling boxes are all venturi type water cooling boxes.
Citation Information
Patent Citations
Rolling method controlling network carbide precipitation of large-section GCr15 bearing steel
CN106086353A
Hot rolling cooling control method for low-alloy and high-strength bar with large size
CN111957745A
Long material rolling through-water cooling control system and method
CN112090968A
Hot rolling method for bearing steel with large compression ratio
CN112792126A
Method for controlling structure and performance of small-specification 20CrMnTi bar
CN115007661A
Cited By
Method for preparing hot-rolled middle rod for C-Mn series high-carbon wear-resistant steel ball based on continuous casting small square billet
CN122377868A