Heating precoated sand as well as preparation method and application thereof

By using heating coated sand prepared from silica sand aggregate, phenolic resin and other materials, the problems of heating riser pollution and single function in existing casting materials are solved, achieving high-efficiency heat preservation and heating effects without fluorine, and significantly prolonging the molten metal. The solidification time and the compensation shrinkage efficiency of the casting are improved.

CN118808539APending Publication Date: 2024-10-22NANYANG RENCHUANG SAND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410695716.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The heating material used in the heating riser of existing casting materials contains fluorine, which causes contamination of the molten metal and molding sand. Moreover, the insulation and heating functions are single, making it difficult to effectively delay the solidification time of the molten metal and improve the compensation shrinkage efficiency.

Method used

Use heat-generating coated sand composed of silica sand aggregate, phenolic resin, curing agent, lubricant and heat-generating agent. The heat-generating agent includes heat preservation agent, combustion accelerator, oxidant, heating agent and water supply agent. Through specific mixing ratio and preparation method , forming a riser with insulation and heating functions to delay the solidification time of molten metal.

Benefits of technology

The fluorine-free heating coated sand is realized, which significantly extends the solidification time of the molten metal, improves the shrinkage compensation efficiency, enhances the thermal insulation performance of the riser, and reduces transportation costs. It is suitable for the production of complex-sized risers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808539A_ABST
    Figure CN118808539A_ABST
Patent Text Reader

Abstract

The invention provides heating precoated sand and a preparation method and application thereof, and belongs to the technical field of casting materials. The heating precoated sand is composed of silica sand aggregate, phenolic resin, a curing agent, a lubricating agent and a heating agent. The heating agent is composed of a heat preservation agent, a combustion improver, an oxidizing agent, a heat supply agent and a water supply agent. The water supply agent is at least one of copper sulfate pentahydrate, zinc sulfate heptahydrate and manganese sulfate heptahydrate; the mass of the heating agent accounts for 0.5%-1% of the mass of the silica sand aggregate. The riser prepared from the precoated sand has the functions of heat preservation and heating, the solidification time of molten metal in the riser can be effectively delayed, and the compensation shrinkage efficiency of the molten metal when a casting is solidified is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting materials, and in particular relates to a kind of heating coated sand and a preparation method and application thereof. Background Art

[0002] Cast steel, cast iron and nonferrous alloy castings are prone to shrinkage and shrinkage defects inside the castings due to their large volume shrinkage during the solidification process, which leads to serious deterioration of the mechanical properties and service life of the castings. Therefore, in order to effectively prevent shrinkage and shrinkage defects from occurring in castings, risers are usually set at appropriate positions of the castings to compensate for the solidification shrinkage of the castings. At present, the measures to increase the riser compensation shrinkage rate mainly include increasing the pressure inside the riser and extending the insulation time of the molten metal in the riser. Among them, there are two main ways to extend the insulation time of the molten metal in the riser, one is to prepare a riser with insulation effect, and the other is to prepare a riser with heating function. Both methods can effectively extend the solidification time of the molten metal in the riser, but the effects of both methods are relatively simple.

[0003] A method for preparing a heat-generating and heat-insulating riser is disclosed in the Chinese patent application publication CN112846089A. The raw sand, heat-insulating material and resin are first placed in a first sand mixer, and then a curing agent is added and mixed evenly to obtain heat-insulating coated sand; the heat-generating material is placed in a second sand mixer, and a binder is added and mixed evenly to obtain a heat-generating core material, and the heat-generating core material is prepared into a heat-generating core; the heat-generating core is then placed in a riser mold, and heat-insulating coated sand is injected into the mold, and the mold is formed and filled to obtain a wet riser, and finally heated and dried to obtain a heat-generating and heat-insulating riser finished product. The riser prepared by this method has both heat-generating and heat-insulating functions, but the heat-generating material used in this method contains fluorine, and fluorine can cause serious pollution to the molten metal and the molding sand. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a heat-generating coated sand. The heat-generating coated sand has both heat-insulating and heat-generating functions, and the raw material does not contain fluorine elements; the riser prepared by using the heat-generating coated sand also has the functions of heat-insulating and heat-generating, which can effectively delay the solidification time of the molten metal and improve the efficiency of compensating shrinkage.

[0005] Specifically, the present invention adopts the following technical solutions:

[0006] A kind of exothermic coated sand, which is composed of silica sand aggregate, phenolic resin, curing agent, lubricant and exothermic agent; the exothermic agent is composed of thermal insulation agent, combustion aid, oxidant, heat supply agent and water supply agent; the water supply agent is at least one of copper sulfate pentahydrate, zinc sulfate heptahydrate and manganese sulfate heptahydrate; the mass of the exothermic agent accounts for 0.5% to 1% of the mass of the silica sand aggregate.

[0007] In a preferred embodiment, in terms of mass percentage, the phenolic resin accounts for 1% to 3% of the silica sand aggregate, the curing agent accounts for 13% to 16% of the phenolic resin, and the lubricant accounts for 5% to 7% of the phenolic resin.

[0008] In a preferred embodiment, the heat-insulating agent is diatomaceous earth, the combustion-supporting agent is coke powder, the oxidizing agent is potassium permanganate, and the heating agent is aluminum powder and quicklime.

[0009] In a further preferred embodiment, the composition of the exothermic agent is, by mass percentage, 20% to 30% diatomaceous earth, 5% to 8% coke powder, 10% to 15% potassium permanganate, 20% to 30% aluminum powder, 20% to 30% quicklime, and 10% to 15% water supply agent.

[0010] In a preferred embodiment, the mesh size of the components of the exothermic agent is ≥300 mesh.

[0011] In a further preferred embodiment, the mesh size of the components of the exothermic agent is 300-500 mesh.

[0012] In a preferred embodiment, the curing agent is hexamethylenetetramine.

[0013] In a preferred embodiment, the lubricant is calcium stearate and / or magnesium stearate.

[0014] The present invention also provides a method for preparing the exothermic coated sand described in any one of the above schemes, comprising the following steps:

[0015] S1, heating the silica sand aggregate to 110-130° C.;

[0016] S2, adding the phenolic resin to the heated silica sand aggregate, mixing evenly, so that the silica sand aggregate is coated with the phenolic resin to obtain a first coated silica sand;

[0017] S3, uniformly mixing the first coated silica sand and the aqueous solution of the curing agent to obtain second coated silica sand;

[0018] S4, mixing the second coated silica sand, the lubricant and the water supply agent evenly to obtain third coated silica sand;

[0019] S5. Evenly mix the thermal insulation agent, the combustion aid, the oxidant, the heating agent and the third coated silica sand to obtain the heat-generating coated sand; the structure of the heat-generating coated sand is composed of a silica sand aggregate layer, a phenolic resin layer, a curing agent layer, a lubricant and water supply agent layer, and a heating layer from the inside to the outside.

[0020] In the above preparation method, the curing agent is prepared into an aqueous solution before use, and the concentration is not limited. Generally, the curing agent is prepared into an aqueous solution with a concentration of 20wt% to 40%.

[0021] The exothermic coated sand described in any of the above schemes of the present invention is prepared into an exothermic riser and / or an insulating riser, which can significantly prolong the solidification time of the molten metal and improve the supplementary shrinkage efficiency.

[0022] The technical solution of the present invention has the following beneficial effects: (1) The coated sand in the present invention has both heat generation and heat preservation functions. When the coated sand is used to prepare a riser, the resulting riser also has both heat generation and heat preservation functions. When the molten metal is injected into the riser, the riser prepared with the heat-generating coated sand will generate heat by itself, which can effectively slow down the cooling rate of the molten metal, slow down the solidification of the molten metal, and significantly improve the efficiency of compensating for shrinkage. (2) In the present invention, at least one compound selected from copper sulfate pentahydrate, zinc sulfate heptahydrate, and manganese sulfate heptahydrate is used as a water supply agent. The temperature for producing coated sand is generally 110-130°C. When the temperature does not exceed 130°C, these compounds only lose part of the crystal water or do not lose the crystal water, and will not destroy their own water supply characteristics; while the temperature in the production stage of the riser sand core is generally 220-240°C, the temperature at which copper sulfate pentahydrate loses all the crystal water is 258°C, and the temperature required for zinc sulfate heptahydrate and manganese sulfate heptahydrate to lose all the crystal water is higher, so the use of coated sand to prepare the riser will not destroy the water supply performance of the water supply agent, and will not affect its subsequent use. (3) Further, when the high-temperature molten metal is injected into the riser, the water supply agent loses the crystal water, the water molecules are absorbed by the quicklime to generate heat, and at the same time, the aluminum powder and the coke powder undergo oxidation reaction to release a large amount of heat; and the heat preservation agent will prevent the heat dissipation and play a role in heat preservation. (4) Existing insulating risers or heating risers are large in size and low in strength, and require special protective measures for long-distance transportation, resulting in high transportation costs. However, the heating coated sand in the present invention is not restricted by transportation conditions and is only used to prepare risers when they are needed. It can produce various complex risers and meet the needs of different specific sizes. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the structure of the exothermic coated sand prepared in the present invention.

[0024] In the figure: 1. silica sand aggregate layer; 2. phenolic resin layer; 3. curing agent layer; 4. lubricant and water supply agent layer; 5. heating layer. DETAILED DESCRIPTION

[0025] The following content is combined with the embodiments to clearly and completely describe the technical solution of the present application so that those skilled in the art can fully understand the present application. Obviously, the described embodiments are only some preferred embodiments of the present application, rather than all embodiments. Any equivalent transformation or substitution made to the following implementation modes by those of ordinary skill in the art without creative work belongs to the protection scope of the present application.

[0026] Ordinal numbers used in this application, such as "first", "second", etc., are only used for descriptive purposes to distinguish similar objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. The phenolic resin used in the embodiment is a granular thermoplastic phenolic resin commonly used in the art, such as phenolic resins with models PF-1901, PF-1902, PF-1904, PF-9082, PF-9083, etc.

[0027] Example 1

[0028] A kind of exothermic coated sand, which is composed of 1000 parts of silica sand aggregate, 20 parts of phenolic resin (phenolic resin accounts for 2% of silica sand aggregate), 3 parts of curing agent (curing agent accounts for 15% of phenolic resin), 1.2 parts of lubricant (lubricant accounts for 6% of phenolic resin) and 8 parts of exothermic agent (exothermic agent accounts for 0.8% of silica sand aggregate) by mass. The exothermic agent is composed of 1.6 parts of heat preservation agent, 0.4 parts of combustion aid, 0.9 parts of oxidant, 3.9 parts of heating agent and 1.2 parts of water supply agent; wherein the heat preservation agent is diatomaceous earth, the combustion aid is coke powder, the oxidant is potassium permanganate, the heating agent is a mixture of 1.6 parts of aluminum powder and 2.3 parts of quicklime; the water supply agent is copper sulfate pentahydrate. The curing agent is urotropine. The lubricant is calcium stearate. The mesh size of the components of all the exothermic agents is 500 mesh.

[0029] The method for preparing the exothermic coated sand comprises the following steps:

[0030] S1. Add silica sand aggregate into the sand mixing barrel and heat it to 120℃.

[0031] S2. Add phenolic resin into a sand mixing barrel, stir and mix evenly, use the sand temperature to melt the solid particles of phenolic resin, and coat the surface of silica sand aggregate to obtain the first coated silica sand.

[0032] S3, add an aqueous solution of a curing agent into the sand mixing barrel (prepare 3 parts of the curing agent into a 30 wt % aqueous solution), and mix it evenly with the first coated silica sand to obtain a second coated silica sand; at this time, the temperature of the mixture in the sand mixing barrel is reduced to below 80°C.

[0033] S4. Add lubricant and water supply agent into the sand mixing barrel, stir and mix evenly to obtain the third coated silica sand.

[0034] S5, adding the heat preservation agent, combustion aid, oxidant and heat supply agent into the sand mixing bucket, mixing evenly, so that the other heat supply agent components except the water supply agent are evenly coated on the surface of the third coated silica sand, and obtaining Figure 1 The heat-generating coated sand shown is composed of a silica sand aggregate layer 1, a phenolic resin layer 2, a curing agent layer 3, a lubricant and water supply agent layer 4, and a heat supply layer 5 from the inside to the outside.

[0035] Example 2

[0036] A kind of exothermic coated sand, which is composed of 1000 parts of silica sand aggregate, 10 parts of phenolic resin (phenolic resin accounts for 1% of silica sand aggregate), 1.3 parts of curing agent (curing agent accounts for 13% of phenolic resin), 0.5 parts of lubricant (lubricant accounts for 5% of phenolic resin) and 5 parts of exothermic agent (exothermic agent accounts for 0.5% of silica sand aggregate) by weight. The exothermic agent is composed of 1.1 parts of heat preservation agent, 0.38 parts of combustion aid, 0.5 parts of oxidant, 2.48 parts of heating agent and 0.54 parts of water supply agent; wherein the heat preservation agent is diatomaceous earth, the combustion aid is coke powder, the oxidant is potassium permanganate, the heating agent is a mixture of 1.48 parts of aluminum powder and 1 part of quicklime; the water supply agent is zinc sulfate heptahydrate. The curing agent is hexamethylenetetramine. The lubricant is magnesium stearate. The mesh size of all components of the exothermic agent is 300 mesh.

[0037] The preparation method of the exothermic coated sand in this embodiment is basically the same as that in Embodiment 1, except that the amount and particle size of each raw material are different and the silica sand aggregate is heated to 110° C. in step S1.

[0038] Example 3

[0039] A kind of exothermic coated sand, which is composed of 1000 parts of silica sand aggregate, 30 parts of phenolic resin (phenolic resin accounts for 3% of silica sand aggregate), 4.8 parts of curing agent (curing agent accounts for 16% of phenolic resin), 2.1 parts of lubricant (lubricant accounts for 7% of phenolic resin) and 10 parts of exothermic agent (exothermic agent accounts for 1% of silica sand aggregate) by weight. The exothermic agent is composed of 2.95 parts of heat preservation agent, 0.55 parts of combustion aid, 1.4 parts of oxidant, 4.1 parts of heating agent and 1 part of water supply agent; wherein the heat preservation agent is diatomaceous earth, the combustion aid is coke powder, the oxidant is potassium permanganate, the heating agent is a mixture of 2.1 parts of aluminum powder and 2 parts of quicklime; the water supply agent is manganese sulfate heptahydrate. The curing agent is urotropine. The lubricant is calcium stearate. The mesh size of all components of the exothermic agent is 400 mesh.

[0040] The preparation method of the exothermic coated sand in this embodiment is basically the same as that in Embodiment 1, except that the amount and particle size of each raw material are different and the silica sand aggregate is heated to 130° C. in step S1.

[0041] Example 4

[0042] A kind of exothermic coated sand, which is composed of 1000 parts of silica sand aggregate, 25 parts of phenolic resin (phenolic resin accounts for 2.5% of silica sand aggregate), 3.5 parts of curing agent (curing agent accounts for 14% of phenolic resin), 1.5 parts of lubricant (lubricant accounts for 6% of phenolic resin) and 6 parts of exothermic agent (exothermic agent accounts for 0.6% of silica sand aggregate) by weight. The exothermic agent is composed of 1.2 parts of heat preservation agent, 0.3 parts of combustion aid, 0.9 parts of oxidant, 3 parts of heat supply agent and 0.6 parts of water supply agent; wherein the heat preservation agent is diatomaceous earth, the combustion aid is coke powder, the oxidant is potassium permanganate, the heat supply agent is a mixture of 1.2 parts of aluminum powder and 1.8 parts of quicklime; the water supply agent is copper sulfate pentahydrate. The curing agent is urotropine. The lubricant is magnesium stearate. The mesh size of the components of all the exothermic agents is 270 mesh.

[0043] The preparation method of the exothermic coated sand in this embodiment is basically the same as that in Embodiment 1, except that the amount and particle size of each raw material are different.

[0044] Comparative Example 1

[0045] The composition of the exothermic coated sand in this comparative example is the same as that in Example 1, and the preparation method comprises the following steps:

[0046] P1. Add silica sand aggregate into the sand mixing barrel and heat to 130℃.

[0047] P2. Add phenolic resin into the sand mixing barrel, stir and mix evenly, use the sand temperature to melt the solid particles of phenolic resin and coat the surface of silica sand aggregate.

[0048] P3. Add other heating agent components except water supply agent into the sand mixing barrel and stir to mix evenly.

[0049] P4. Add water supply agent into the sand mixing barrel and stir to mix evenly.

[0050] P5. Add the aqueous solution of curing agent into the sand mixing barrel (prepare the curing agent into a 30wt% aqueous solution before use) and stir to mix evenly.

[0051] P6. Add lubricant into the sand mixing barrel and stir to mix evenly to obtain heating coated sand.

[0052] Comparative Example 2

[0053] The composition of the exothermic coated sand in this comparative example is the same as that in Example 1, and the preparation method comprises the following steps:

[0054] Q1. Add silica sand aggregate into the sand mixing barrel and heat it to 130℃.

[0055] Q2. Mix the other components of the heating agent except the water supply agent evenly, preheat to 120℃, then add them into the sand mixing barrel and stir to mix evenly.

[0056] Q3. Add phenolic resin into the sand mixing barrel and stir to mix evenly.

[0057] Q4. Add the aqueous solution of water supply agent and curing agent into the sand mixing barrel (prepare the curing agent into a 30wt% aqueous solution before use), and stir to mix evenly.

[0058] Q5. Add lubricant into the sand mixing barrel, stir and mix evenly to obtain exothermic coated sand.

[0059] Coated sand performance and application performance test

[0060] Take the exothermic coated sand prepared in Examples 1 to 4 and Comparative Examples 1 to 2, as well as the commercially available ordinary coated sand (without exothermic function, purchased from Xinyi Tianwei Coated Sand Industrial Co., Ltd.) and the existing exothermic coated sand (prepared according to the method disclosed in patent application CN107252872A), and test the room temperature tensile strength, hot tensile strength, average fineness and melting point according to the method in JB / T8583-2008 "Coated Sand for Casting". The test results are shown in Table 1. The exothermic coated sand prepared in Examples 1 to 4 and Comparative Examples 1 to 2, as well as the commercially available ordinary coated sand (without exothermic function, purchased from Xinyi Tianwei Coated Sand Industrial Co., Ltd.), and the existing exothermic coated sand (prepared according to the method disclosed in patent application CN107252872A) were prepared into risers according to the following methods, and the high temperature duration of the risers and the shrinkage rate of the castings were tested. The test results are shown in Table 2.

[0061] Preparation method of exothermic riser: heat the metal molds to 200-230°C respectively, inject the above-mentioned different coated sand particles respectively, heat the coated sand for 1-2 minutes, and the binder and curing agent on the surface of the sand particles react chemically to solidify, and then separate from the mold to obtain the exothermic riser.

[0062] Table 1 Test results of coated sand performance

[0063]

[0064]

[0065] In order to avoid the influence of the particle size of silica sand aggregate, the coated sand in Table 1 ensures that the average fineness is basically the same. It can be seen from Table 1 that the strength of the exothermic coated sand prepared in the embodiment is higher than the strength of the exothermic coated sand prepared in the comparative example. The preparation methods of Example 1, Comparative Example 1 and Comparative Example 2 are different, the components are the same, and the strength of the coated sand is different, which shows that even with the same components, the change of the preparation method will affect the strength of the coated sand. This is because after changing the preparation method of the exothermic coated sand, the exothermic agent in Comparative Example 1 blocks the chemical reaction of the phenolic resin and the curing agent, resulting in hindered curing, reduced strength, and higher melting point; the exothermic agent in Comparative Example 2 will block the coating effect of the resin on the silica sand aggregate and reduce the strength. The room temperature tensile strength and hot tensile strength of the exothermic coated sand prepared in the present invention are comparable to or even higher than those of ordinary coated sand available on the market. This shows that the components of the exothermic coated sand in the present invention are operated according to the preparation method in the present invention, which will not affect the strength of the coated sand, and may even help to improve the strength of the coated sand.

[0066] Table 2 Performance test results of riser

[0067] High temperature duration (seconds) Casting shrinkage rate (%) Example 1 132 0.07 Example 2 117 0.10 Example 3 134 0.06 Example 4 123 0.08 Comparative Example 1 105 0.32 Comparative Example 2 102 0.36 Commercially available ordinary coated sand 43 1.65 Existing heating coated sand 75 0.82

[0068] The high temperature duration in Table 2 refers to the time after the coated sand or the heating coated sand is prepared into a riser, molten iron at 1400°C is injected, and the temperature of the molten iron is monitored all the time until the temperature of the molten iron drops to 1350°C; the longer the time, the better the thermal insulation effect of the riser. The shrinkage rate of the casting in Table 2 refers to the proportion of pores appearing in the thick and large parts of the casting. The larger the shrinkage rate, the poorer the shrinkage compensation effect of the riser, the insufficient molten metal for shrinkage compensation, and the reduced density of the casting. It can be seen from Table 2 that compared with the heating coated sand in the prior art, the thermal insulation performance of the riser prepared by the heating coated sand prepared in the present invention is significantly improved, and the shrinkage rate of the casting is significantly reduced.

[0069] The above-described embodiments are only preferred embodiments of the present application and are not intended to limit the scope of protection of the present application. For any person skilled in the art, the present application may have various changes and modifications. Any simple equivalent changes and modifications made based on the scope of protection of the present application and the contents of the specification should be included in the scope of protection of the present application.

Claims

1. A kind of exothermic coated sand, characterized in that: The exothermic coated sand is composed of silica sand aggregate, phenolic resin, curing agent, lubricant and exothermic agent; the exothermic agent is composed of thermal insulation agent, combustion aid, oxidant, heat supply agent and water supply agent; the water supply agent is at least one of copper sulfate pentahydrate, zinc sulfate heptahydrate and manganese sulfate heptahydrate; the mass of the exothermic agent accounts for 0.5% to 1% of the mass of the silica sand aggregate.

2. The exothermic coated sand according to claim 1, characterized in that: In terms of mass percentage, the phenolic resin accounts for 1% to 3% of the silica sand aggregate, the curing agent accounts for 13% to 16% of the phenolic resin, and the lubricant accounts for 5% to 7% of the phenolic resin.

3. The exothermic coated sand according to claim 1, characterized in that: The heat-insulating agent is diatomaceous earth, the combustion-supporting agent is coke powder, the oxidizing agent is potassium permanganate, and the heating agent is aluminum powder and quicklime.

4. The exothermic coated sand according to claim 2, characterized in that: In terms of mass percentage, the composition of the heating agent is: 20% to 30% diatomaceous earth, 5% to 8% coke powder, 10% to 15% potassium permanganate, 20% to 30% aluminum powder, 20% to 30% quicklime, and 10% to 15% water supply agent.

5. The exothermic coated sand according to claim 1, characterized in that: The mesh sizes of the components of the exothermic agent are all ≥300 meshes.

6. The exothermic coated sand according to claim 5, characterized in that: The mesh sizes of the components of the exothermic agent are all between 300 and 500 meshes.

7. The exothermic coated sand according to claim 1, characterized in that: The curing agent is hexamethylenetetramine; or / and the lubricant is calcium stearate or / and magnesium stearate.

8. The method for preparing the exothermic coated sand according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, heating the silica sand aggregate to 110-130° C.; S2, adding the phenolic resin to the heated silica sand aggregate, mixing evenly, so that the silica sand aggregate is coated with the phenolic resin to obtain a first coated silica sand; S3, uniformly mixing the first coated silica sand and the aqueous solution of the curing agent to obtain second coated silica sand; S4, mixing the second coated silica sand, the lubricant and the water supply agent evenly to obtain third coated silica sand; S5. Evenly mix the thermal insulation agent, the combustion aid, the oxidant, the heating agent and the third coated silica sand to obtain the heat-generating coated sand; the structure of the heat-generating coated sand is composed of a silica sand aggregate layer, a phenolic resin layer, a curing agent layer, a lubricant and water supply agent layer, and a heating layer from the inside to the outside.

9. Use of the exothermic coated sand according to any one of claims 1 to 7 in the preparation of exothermic risers and / or thermal insulation risers.