Efficient core-removing method for ceramic core
By controlling the pressure cycle change of the potassium hydroxide solution, efficient core removal of ceramic cores is achieved, solving the problems of low and incomplete core removal efficiency in the existing technology, and improving the core removal efficiency and efficiency of alumina-based ceramic cores. Integrity.
Patent Information
- Application Number
- CN202411141062.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-22
AI Technical Summary
The existing coring method for alumina-based ceramic cores has problems of low core removal efficiency and incompleteness. In particular, the normal pressure alkali boiling method takes a long time and the alkali solution of the high temperature and high pressure alkali boiling method is easy to vaporize, resulting in insufficient core removal reaction.
Potassium hydroxide solution is used as the core-removing alkali solution, and by controlling the pressure increase-pressure holding-pressure reduction cycle, the pressure and time are adjusted, and the electric pressure regulating valve is used to achieve efficient core removal of the ceramic core. The specific steps are included in the scheduled React under pressure for a certain period of time, and repeat pressurization to high pressure and depressurization to low pressure several times.
It improves the core removal efficiency and integrity of ceramic cores, ensures efficient removal of complex channels, and reduces the consumption of alkali solution and the risk of residual alkali solution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic core stripping, and in particular to a method for efficiently stripping a ceramic core. Background Art
[0002] With the development of industrial technology, higher requirements are put forward for the heat resistance of hollow blades for aircraft engines. The existing method of improving heat resistance is mainly to optimize the cooling channel inside the hollow blade, so that a complex air-cooled internal channel is formed inside the blade to improve the cooling efficiency. In order to prepare the complex air-cooled internal channel inside the blade, a ceramic core with a corresponding complex air-cooled internal channel structure is required. The main material of the ceramic core is usually alumina, and the core removal method for alumina-based ceramic cores is alkali boiling, including normal pressure alkali boiling and high temperature and high pressure alkali boiling. Due to the high chemical stability of alumina, the core removal efficiency of normal pressure alkali boiling is slow and it takes a long time; high temperature and high pressure alkali boiling is carried out at a certain temperature and pressure, and the alkali solution will continue to vaporize in the working tank. Continuous pressurization and pressure relief will cause the loss of alkali solution, so there is a risk that the alkali solution is lower than the casting, resulting in too much residual ceramic core hindering the core removal reaction.
[0003] Therefore, providing a ceramic core de-coring method with high de-coring efficiency is of great significance for the research and development of hollow blades for high-performance aero-engines. Summary of the invention
[0004] The purpose of the present invention is to provide a method for efficiently removing ceramic cores, so as to solve the problems of low efficiency and incomplete removal of cores in the existing methods of removing cores by alkali boiling at normal pressure and alkali boiling at high temperature and high pressure.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for efficiently removing a ceramic core, comprising the following steps:
[0007] Place the casting in the core-removing kettle, add alkali solution and heat to the core-removing temperature, so that the pressure in the core-removing kettle is maintained at a predetermined value F. 1 , at the predetermined value F 1 The reaction time T 1 Then the pressure in the core removal kettle is increased to a predetermined value F 2 , at the predetermined value F 2 The reaction time T 2 Then the pressure in the core removal kettle is reduced to a predetermined value F 1 , at the predetermined value F 1 The reaction time T 3 ; Repeatedly pressurize to the preset value F 2 and reduce the voltage to a predetermined value F 1The process is repeated 3 to 6 times to complete the efficient core stripping of the ceramic core.
[0008] Preferably, in the above-mentioned method for efficiently removing a ceramic core, the alkali solution is a potassium hydroxide solution; and the mass concentration of the alkali solution is 25-44%.
[0009] Preferably, in the above-mentioned method for efficiently removing the ceramic core, the removal temperature is 350-400°C.
[0010] Preferably, in the above-mentioned method for efficiently removing a ceramic core, the predetermined value F 1 is 5 to 10 MPa; the reaction time is T 1 0.5~1.5h.
[0011] Preferably, in the above-mentioned method for efficiently removing a ceramic core, the predetermined value F 2 is 15-25MPa; the reaction time T 2 1 to 2 hours.
[0012] Preferably, in the above-mentioned method for efficiently removing the ceramic core, the reaction time T 3 0.5~2h.
[0013] Preferably, in the above-mentioned method for efficiently removing a ceramic core, the pressure is increased to a predetermined value F 2 The rate is 0.5~2MPa / min.
[0014] Preferably, in the above-mentioned method for efficiently removing a ceramic core, the pressure is reduced to a predetermined value F 1 The rate is 1~3MPa / min.
[0015] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0016] The present invention uses potassium hydroxide solution as the core-deleting alkali solution, controls the core-deleting pressure to change in a cycle of pressure increase-pressure maintenance-pressure reduction during the core-deleting process, and controls the corresponding time of pressure increase-pressure maintenance-pressure reduction, so that the core-deleting alkali solution and the ceramic core have good wettability, and the complex channels in the ceramic core can also achieve efficient core-deleting. DETAILED DESCRIPTION
[0017] The present invention provides a method for efficiently removing a ceramic core, comprising the following steps:
[0018] Place the casting in the core-removing kettle, add alkali solution and heat to the core-removing temperature, so that the pressure in the core-removing kettle is maintained at a predetermined value F. 1 , at the predetermined value F 1 The reaction time T 1Then the pressure in the core removal kettle is increased to a predetermined value F 2 , at the predetermined value F 2 The reaction time T 2 Then the pressure in the core removal kettle is reduced to a predetermined value F 1 , at the predetermined value F 1 The reaction time T 3 ; Repeatedly pressurize to the preset value F 2 and reduce the voltage to a predetermined value F 1 The process is repeated 3 to 6 times to complete the efficient core stripping of the ceramic core.
[0019] In the present invention, the pressure in the core removal kettle is adjusted by an electric pressure regulating valve.
[0020] In the present invention, the core removal kettle is a conventional commercially available core removal kettle in the art, which has the functions of sealing, corrosion resistance and high temperature resistance.
[0021] In the present invention, the alkali solution is preferably a potassium hydroxide solution; the mass concentration of the alkali solution is preferably 25-44%, more preferably 30-40%, and more preferably 35%.
[0022] In the present invention, the core removal temperature is preferably 350 to 400°C, more preferably 360 to 390°C, and even more preferably 380°C.
[0023] In the present invention, the predetermined value F 1 Preferably, it is 5 to 10 MPa, more preferably 7 to 9 MPa, and more preferably 8 MPa; the reaction time T 1 It is preferably 0.5 to 1.5 h, more preferably 1 to 1.5 h, and even more preferably 1.5 h.
[0024] In the present invention, the predetermined value F 2 Preferably, it is 15 to 25 MPa, more preferably 18 to 24 MPa, and more preferably 22 MPa; the reaction time T 2 It is preferably 1 to 2 hours, more preferably 1.5 to 2 hours, and even more preferably 2 hours.
[0025] In the present invention, the reaction time T 3 It is preferably 0.5 to 2 h, more preferably 1 to 2 h, and even more preferably 1.5 h.
[0026] In the present invention, the pressure is increased to a predetermined value F 2 The rate is preferably 0.5 to 2 MPa / min, more preferably 0.5 to 1.5 MPa / min, and even more preferably 1 MPa / min.
[0027] In the present invention, the voltage is reduced to a predetermined value F 1 The rate is preferably 1 to 3 MPa / min, more preferably 1.5 to 3 MPa / min, and even more preferably 2 MPa / min.
[0028] In the present invention, the repeated pressurization to a predetermined value F 2 and reduce the voltage to a predetermined value F 1 The process of 3 to 6 times also includes: cooling to room temperature, depressurizing the core-removing kettle, taking out the casting, and rinsing the casting with water.
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] This embodiment provides a method for efficiently removing a ceramic core, comprising the following steps:
[0032] The casting was placed in a core-removing kettle, a potassium hydroxide solution with a mass concentration of 30% was added as a core-removing alkali solution, and the temperature was heated to a core-removing temperature of 380°C. The pressure in the core-removing kettle was maintained at 6MPa through an electric pressure regulating valve, and the reaction was carried out at a pressure of 6MPa for 1h;
[0033] Then, the pressure in the core-removing reactor was increased to 20 MPa at a rate of 1 MPa / min through an electric pressure regulating valve, and the pressure was maintained at 20 MPa for 1 hour;
[0034] Then, the pressure in the core-removing kettle was reduced to 6 MPa at a rate of 2 MPa / min through an electric pressure regulating valve, and the reaction was carried out at a pressure of 6 MPa for 0.5 h;
[0035] Repeat the above process of increasing the pressure to 20 MPa and maintaining the pressure for reaction and reducing the pressure to 6 MPa and reacting for 4 times;
[0036] Finally, cool to room temperature, release the pressure of the core-removing kettle to normal pressure, take out the casting, and rinse the casting with 30°C water for 3 times to complete the efficient core-removal of the ceramic core.
[0037] Example 2
[0038] This embodiment provides a method for efficiently removing a ceramic core, comprising the following steps:
[0039] The casting was placed in a core-removing kettle, a potassium hydroxide solution with a mass concentration of 40% was added as a core-removing alkali solution, and the temperature was heated to a core-removing temperature of 400°C. The pressure in the core-removing kettle was maintained at 10MPa through an electric pressure regulating valve, and the reaction was carried out at a pressure of 10MPa for 0.5h;
[0040] Then, the pressure in the core-removing kettle was increased to 20 MPa at a rate of 1.5 MPa / min through an electric pressure regulating valve, and the pressure was maintained at 20 MPa for 2 h;
[0041] Then, the pressure in the core-removing kettle was reduced to 10 MPa at a rate of 2 MPa / min through an electric pressure regulating valve, and the reaction was carried out at a pressure of 10 MPa for 1 hour;
[0042] Repeat the above process of increasing the pressure to 20 MPa and carrying out pressure-maintaining reaction and reducing the pressure to 10 MPa and carrying out reaction 3 times;
[0043] Finally, cool to room temperature, release the pressure of the core-removing kettle to normal pressure, take out the casting, and rinse the casting with 40°C water for 3 times to complete the efficient core-removal of the ceramic core.
[0044] Example 3
[0045] This embodiment provides a method for efficiently removing a ceramic core, comprising the following steps:
[0046] The casting was placed in a core-removing kettle, and a potassium hydroxide solution with a mass concentration of 25% was added as a core-removing alkali solution. The solution was heated to a core-removing temperature of 360°C, and the pressure in the core-removing kettle was maintained at 8MPa by an electric pressure regulating valve. The reaction was carried out at a pressure of 8MPa for 1.5h.
[0047] Then, the pressure in the core-removing kettle was increased to 22 MPa at a rate of 2 MPa / min through an electric pressure regulating valve, and the pressure was maintained at 22 MPa for 1.5 h;
[0048] Then, the pressure in the core-removing kettle was reduced to 8 MPa at a rate of 1 MPa / min through an electric pressure regulating valve, and the reaction was carried out at a pressure of 8 MPa for 2 h;
[0049] Repeat the above process of increasing the pressure to 22 MPa and carrying out pressure-maintaining reaction and reducing the pressure to 8 MPa and carrying out reaction 6 times;
[0050] Finally, cool to room temperature, release the pressure of the core-removing kettle to normal pressure, take out the casting, and rinse the casting with 30°C water for 4 times to complete the efficient core-removal of the ceramic core.
[0051] Example 4
[0052] This embodiment provides a method for efficiently removing a ceramic core, comprising the following steps:
[0053] The casting was placed in a core-removing kettle, a potassium hydroxide solution with a mass concentration of 35% was added as a core-removing alkali solution, and the temperature was heated to a core-removing temperature of 390°C. The pressure in the core-removing kettle was maintained at 9MPa by an electric pressure regulating valve, and the reaction was carried out at a pressure of 9MPa for 1.5h;
[0054] Then, the pressure in the core-removing kettle was increased to 25 MPa at a rate of 1.5 MPa / min through an electric pressure regulating valve, and the pressure was maintained at 25 MPa for 2 h;
[0055] Then, the pressure in the core-removing kettle was reduced to 9 MPa at a rate of 3 MPa / min through an electric pressure regulating valve, and the reaction was carried out at a pressure of 9 MPa for 2 h;
[0056] Repeat the above process of increasing the pressure to 25 MPa and carrying out pressure-maintaining reaction and reducing the pressure to 9 MPa and carrying out reaction 3 times;
[0057] Finally, cool to room temperature, release the pressure of the core-removing kettle to normal pressure, take out the casting, and rinse the casting with 35°C water for 4 times to complete the efficient core-removal of the ceramic core.
[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for efficiently removing a ceramic core, characterized in that: The following steps are involved: The casting is placed in a core-removing kettle, and after adding alkali solution, it is heated to the core-removing temperature, so that the pressure in the core-removing kettle is maintained at a predetermined value F1, and reacts at the pressure of the predetermined value F1 for a certain time T1; then the pressure in the core-removing kettle is increased to a predetermined value F2, and reacts at the pressure of the predetermined value F2 for a certain time T2; then the pressure in the core-removing kettle is reduced to a predetermined value F1, and reacts at the pressure of the predetermined value F1 for a certain time T3; the process of increasing the pressure to the predetermined value F2 and reducing the pressure to the predetermined value F1 is repeated 3 to 6 times, and the efficient core-removing of the ceramic core is completed.
2. A method for efficiently removing a ceramic core according to claim 1, characterized in that: The alkali solution is potassium hydroxide solution; the mass concentration of the alkali solution is 25-44%.
3. A method for efficiently removing a ceramic core according to claim 2, characterized in that: The core removal temperature is 350-400°C.
4. A method for efficiently removing a ceramic core according to claim 3, characterized in that: The predetermined value F1 is 5 to 10 MPa; the reaction time T1 is 0.5 to 1.5 h.
5. A method for efficiently removing a ceramic core according to claim 1 or 4, characterized in that: The predetermined value F2 is 15-25 MPa; the reaction time T2 is 1-2 hours.
6. A method for efficiently removing a ceramic core according to claim 5, characterized in that: The reaction time T3 is 0.5 to 2 hours.
7. A method for efficiently removing a ceramic core according to claim 3, characterized in that: The rate of increasing the pressure to the predetermined value F2 is 0.5-2 MPa / min.
8. A method for efficiently removing a ceramic core according to claim 7, characterized in that: The rate of reducing the pressure to the predetermined value F1 is 1-3 MPa / min.