Wood structure material and preparation method thereof

By subjecting rotary-cut veneers to moist heat shaping treatment, resin impregnation and compression densification, combined with hot and cold pressing technology, the problem of low strength of thick veneers of artificial forest fast-growing wood was solved, and a high-strength wooden structure suitable for building structures was prepared. Material.

CN118809743AActive Publication Date: 2024-10-22INST OF WOOD INDUDTRY CHINESE ACAD OF FORESTRY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310421786.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

Thick veneers of artificial forest fast-growing wood cannot be directly used to make building structural materials. The material strength is low and it is difficult to meet the load-bearing requirements.

Method used

By pre-processing, moist heat shaping treatment, resin impregnation, compression densification and hot-pressing assembly of the rotary-cut veneer, combined with cold pressing technology, the static bending strength and elastic modulus of the material are improved to form a high-strength wooden structural material.

Benefits of technology

The prepared wooden structural material has high static bending strength and large elastic modulus, and can be used in building structures. It solves the problem of low material strength and improves the material preparation efficiency and gluing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809743A_ABST
    Figure CN118809743A_ABST
Patent Text Reader

Abstract

The invention provides a wood structure material and a preparation method thereof. The method comprises the steps that a rotary-cut veneer is pretreated, and a pretreated product is obtained; carrying out damp-heat setting treatment on the pretreated product; the product with the dynamic elastic modulus being 9000 MPa or above is selected as a damp-heat setting product; soaking the first moist heat setting product in a resin solution, and drying to obtain a dried product; compressing and densifying the dried product to obtain a densified veneer; selecting a second moist heat setting product, and enabling at least one surface of the second moist heat setting product to have a first adhesive; assembling and hot-pressing the densified veneer and the second damp and hot setting product with the first adhesive to obtain a first forming body; optionally, selecting a third damp and hot setting product, and carrying out assembly and hot pressing on the third damp and hot setting product and a second damp and hot setting product with a first adhesive to obtain a second forming body; and in the presence of a second adhesive, two first forming bodies are selected and subjected to cold pressing with a second forming body or sawn timber, and the wood structural material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a wood structural material and a preparation method thereof, in particular to a high-strength wood structural material made of an ultra-thick veneer and a preparation method thereof, belonging to the field of wood application. Background Art

[0002] With the reduction of forest resources in the world, high-quality large-diameter logs are increasingly in short supply, and the output of natural wood has dropped sharply. The high-value utilization of fast-growing wood from artificial forests has become an important way to alleviate the contradiction between wood supply and demand in my country. Due to the short growth cycle, most fast-growing woods are young woods, with problems such as loose materials, low density, easy cracking and low strength. Therefore, the application range of fast-growing wood is limited. It is usually used as a raw material for artificial boards such as fiberboard, particleboard, plywood and other artificial boards, indirectly used in homes and other fields, or used as a raw material for papermaking and building formwork. Although domestic and foreign scholars have developed corresponding processing and technologies to modify and functionalize fast-growing wood, such as compounding, consolidation, softening, plasticization, color treatment, anti-corrosion, flame retardant, etc., thereby broadening the application field of fast-growing wood. However, it is still difficult to use fast-growing wood in building structures.

[0003] Cross-laminated timber (CLT) is an engineered wood product. It is a structural material made of at least three layers of standard sawn timber bonded together orthogonally with adhesive. It has good physical and mechanical properties, high stability, and is not prone to cracking and deformation. It is widely used in wooden structures in Europe, North America and other places. However, CLT has strict requirements on raw materials, which must be graded solid sawn timber. Large-diameter timber is generally used abroad, while the diameter of my country's current artificial forests is relatively small, and the yield is relatively low. Thick veneer can realize the utilization of small-diameter fast-growing timber, and thick veneer can be used instead of standard sawn timber to manufacture engineering structural materials similar to CLT.

[0004] Since the material of artificial forest is relatively soft, the thick veneer cut from rotary cutting cannot meet the needs of structural materials. At present, thick veneer is only used to make thick core board for decorative materials. In addition, the hot pressing process is generally used to make large-scale wood composite materials from wood veneer. If the hot pressing process is used to make structural materials of a certain thickness from thick veneer, the heat transfer of the middle layer will be affected, thereby affecting the curing of the adhesive.

[0005] Reference 1 discloses a solid wood composite board made of ultra-thick veneers, comprising two outer surface layers and a core layer therebetween, with adhesive provided between each layer of veneer; the core layer is composed of ultra-thick veneers with a thickness of 6mm-12mm, and the surface layer is composed of veneers with a thickness of 0.2mm-1.5mm. However, the solid wood composite board can only be used indoors, and cannot be used for load bearing or building houses.

[0006] Reference 2 discloses a method for producing high-performance veneer laminated materials with high elastic modulus, high dimensional stability, high wear resistance and low variability, which is divided into high and low grades or high, medium and low grades according to the dynamic elastic modulus MOE of the veneer. The veneer laminated materials are made of graded thin veneers as raw materials through high compression rate to manufacture engineering structural materials, but for thick veneers, even if they are graded, high compression rate cannot be achieved and the problem of their own soft material cannot be solved.

[0007] Therefore, it has become a technical problem to be solved urgently to study a wood structural material and a preparation method thereof so as to solve the problem that the thick veneer peeled from fast-growing wood of artificial forests cannot be directly used to manufacture structural materials.

[0008] References:

[0009] Reference 1: CN101524859A

[0010] Reference 2: CN103433983A Summary of the invention

[0011] Problem that the invention aims to solve

[0012] In view of the technical problems existing in the prior art, the object of the present invention is to provide a wooden structural material and a preparation method thereof, so as to solve the problem that the thick veneer peeled from fast-growing wood of artificial forests cannot be directly used to manufacture structural materials.

[0013] Solutions for solving problems

[0014] The present invention provides a method for preparing a wood structural material, which comprises the following steps:

[0015] Pre-treating the peeled veneer to obtain a pre-treated product;

[0016] The pre-treated product is subjected to a wet heat setting treatment; and the dynamic elastic modulus of the pre-treated product after the wet heat setting is detected, and the product having a dynamic elastic modulus of 9000 MPa or more is selected as the wet heat setting product;

[0017] Selecting at least one first wet heat setting product, dipping it in a resin solution and then drying it to obtain a dried product;

[0018] Compressing and densifying the dried product to obtain a densified veneer;

[0019] Selecting a second moist heat setting product, and providing at least one surface of the second moist heat setting product with a first adhesive;

[0020] Assembling and hot-pressing the densified veneer and the second wet-heat-setting product having the first adhesive, with the densified veneer being located on the surface layer, to obtain a first formed body;

[0021] Optionally, the third wet heat setting product is selected and hot-pressed with the second wet heat setting product having the first adhesive to obtain a second molded body;

[0022] In the presence of a second adhesive, two of the first molded bodies are selected and cold-pressed with the second molded body or sawn timber to obtain a wood structural material; wherein,

[0023] The second formed body or the sawn timber is located between two first formed bodies, and the densified veneers in the first formed bodies are all located far away from the second formed body or the sawn timber.

[0024] According to the preparation method of the present invention, the thickness of the rotary cut veneer is 6-20 mm; and / or the water content of the pre-treated product is 20-40%.

[0025] According to the preparation method of the present invention, the temperature of the wet heat setting treatment is 140-210° C.; the pressure of the wet heat setting treatment is 0.5-2.5 MPa; and the time of the wet heat setting treatment is 30-90 min.

[0026] According to the preparation method of the present invention, the mass fraction of the resin in the resin solution is 10%-30%; preferably, the resin comprises one or a combination of two or more selected from epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, and furfuryl alcohol resin; and / or

[0027] The moisture content of the dried product is 10%-15%.

[0028] According to the preparation method of the present invention, the compression rate of the compression and densification is 10-50%, the temperature of the compression and densification is 100-200° C., and the time of the compression and densification is 10-60 min.

[0029] According to the preparation method of the present invention, the dosage of the first adhesive is 150-350 g / m 2 ; and / or

[0030] The compression rate of the hot pressing is 1%-10%, the temperature of the hot pressing is 100-170° C., and the time of the hot pressing is 0.5-3 min / mm; and / or

[0031] The thickness of the first molded body is no more than 35 mm.

[0032] According to the preparation method of the present invention, the second adhesive comprises one or both of polyurethane or latex glue; and / or

[0033] The dosage of the second adhesive is 80-180g / m2 .

[0034] According to the preparation method of the present invention, the thickness of the second formed body or the sawn timber is not more than 35 mm.

[0035] According to the preparation method of the present invention, the cold pressing pressure is 1-2 MPa, the cold pressing time is 60-240 min, and the cold pressing temperature is 0-40°C.

[0036] The present invention also provides a wood structural material, which is prepared by the preparation method of the present invention.

[0037] Effects of the Invention

[0038] The wooden structural material prepared by the preparation method of the present invention has high static bending strength, large elastic modulus and high shear strength, and can be used in building structures.

[0039] The preparation method of the present invention classifies thick veneers and performs resin impregnation and densification treatment on the surface that is mainly subjected to stress, and uses a second molded body or sawn timber as the core layer that is less subjected to stress, thereby improving the static bending strength of the material through surface reinforcement and reasonable structural design.

[0040] The preparation method of the present invention can improve the preparation efficiency and gluing quality of the material by combining cold and hot pressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A schematic structural diagram of a first molded body of the present invention is shown;

[0042] Figure 2 A schematic structural diagram of another first molded body of the present invention is shown;

[0043] Figure 3 A schematic structural diagram of a second molded body of the present invention is shown;

[0044] Figure 4 A schematic structural diagram of a wood structural material of the present invention is shown;

[0045] Figure 5 A schematic structural diagram of another wooden structural material of the present invention is shown;

[0046] Figure 6 A structural schematic diagram of another wooden structural material of the present invention is shown. DETAILED DESCRIPTION

[0047] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0048] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0049] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0050] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0051] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0052] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0053] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 10-40°C.

[0054] The present invention first provides a method for preparing a wood structural material, which comprises the following steps:

[0055] Pre-treating the peeled veneer to obtain a pre-treated product;

[0056] The pre-treated product is subjected to a wet heat setting treatment; and the dynamic elastic modulus of the pre-treated product after the wet heat setting is detected, and the product having a dynamic elastic modulus of 9000 MPa or more is selected as the wet heat setting product;

[0057] The first wet heat setting product is selected, immersed in a resin solution and then dried to obtain a dried product;

[0058] Compressing and densifying the dried product to obtain a densified veneer;

[0059] Selecting a second moist heat setting product, and providing at least one surface of the second moist heat setting product with a first adhesive;

[0060] Assembling and hot-pressing the densified veneer and the second wet-heat-setting product having the first adhesive, with the densified veneer being located on the surface layer, to obtain a first formed body;

[0061] Optionally, the third wet heat setting product is selected and hot-pressed with the second wet heat setting product having the first adhesive to obtain a second molded body;

[0062] In the presence of a second adhesive, two of the first molded bodies are selected and cold-pressed with the second molded body or sawn timber to obtain a wood structural material; wherein,

[0063] The second formed body or the sawn timber is located between two first formed bodies, and the densified veneers in the first formed body and the second formed body are both located far away from the second formed body or the sawn timber.

[0064] In the present invention, the thick veneer is derived from one or a combination of two or more of poplar, eucalyptus, fir, larch, radiata pine and masson pine.

[0065] The first wet heat setting product, the second wet heat setting product and the third wet heat setting product described in the present invention all belong to wet heat setting products. In order to better distinguish, the first wet heat setting product, the second wet heat setting product and the third wet heat setting product are used to represent. In addition, in the present invention, the first wet heat setting product is generally one wet heat setting product; the second wet heat setting product and the third wet heat setting product are not limited to one, and are generally greater than or equal to one, for example: 1, 3, 5, 7, etc.

[0066] The preparation method of the present invention improves the static bending strength of the material by grading the thick veneer and performing resin impregnation and densification treatment on the veneer on the main stress-bearing surface, and adopts the second molded body or sawn timber as the core layer with less stress, and improves the static bending strength of the material through surface reinforcement and reasonable structural design. In addition, the preparation method of the present invention improves the preparation efficiency and gluing quality of the material by combining cold and hot pressing.

[0067] In some specific embodiments, the rotary cut veneer of the present invention is an ultra-thick veneer, that is, a log rotary cut wood thick veneer. Specifically, the thickness of the rotary cut veneer is 6-20 mm, for example: 8 mm, 10 mm, 12 mm, 15 mm, 18 mm, etc. The present invention solves the problem that the artificial forest fast-growing wood rotary cut thick veneer cannot be directly used to manufacture structural materials by using high-strength wood structural materials manufactured by ultra-thick veneers.

[0068] The present invention first pre-treats the peeled veneer to obtain a pre-treated product; specifically, the present invention does not specifically limit the pre-treatment, as long as the moisture content of the pre-treated product can be 20-40%, for example: 22%, 25%, 28%, 30%, 32%, 35%, 38%, etc. Specifically, in the present invention, the peeled veneer can be steamed and then naturally dried to obtain a pre-treated product with a moisture content of 20-40%.

[0069] Further, the pretreatment product is subjected to a wet heat setting treatment; and the dynamic elastic modulus of the pretreatment product after the wet heat setting is detected, and the product with a dynamic elastic modulus of 9000 MPa or more is selected as the wet heat setting product. When the product with a dynamic elastic modulus of 9000 MPa or more is used as the wet heat setting product, the overall mechanical properties of the obtained wood structural material are excellent.

[0070] In some specific embodiments, the temperature of the wet heat setting treatment is 140-210°C, for example: 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, etc.; the pressure of the wet heat setting treatment is 0.5-2.5MPa, for example: 0.8MPa, 1MPa, 1.2MPa, 1.5MPa, 1.8MPa, 2MPa, 2.2MPa, etc.; the time of the wet heat setting treatment is 30-90min, for example: 40min, 50min, 60min, 70min, 80min, etc. Through the wet heat setting treatment, the pre-treated product can be set and flattened.

[0071] Furthermore, a first wet heat setting product is selected, immersed in a resin solution and then dried to obtain a dry product; by immersing the first wet heat setting product in a resin solution, the resin can fill the pores such as vessels and cell cavities in the wood, thereby increasing the density of the wood and improving the mechanical properties.

[0072] In some specific embodiments, the mass fraction of the resin in the resin solution is 10%-30%, for example: 12%, 15%, 18%, 20%, 22%, 25%, 28%, etc.; preferably, the resin includes one or a combination of two or more selected from epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, furfuryl alcohol resin. Preferably, the moisture content of the dried product is 10%-15%, for example: 11%, 12%, 13%, 14%, etc.

[0073] Furthermore, the dried product is compressed and densified to obtain a densified veneer. The inventors of the present invention have found that the pores inside the veneer can be further reduced, the density of the veneer can be increased, and the mechanical properties of the veneer can be improved by compression and densification.

[0074] In some specific embodiments, the compression rate of the compression densification is 10-50%, for example: 15%, 20%, 25%, 30%, 35%, 40%, 45%, etc.; the temperature of the compression densification is 100-200°C, for example: 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, etc.; the time of the compression densification is 10-60min, for example: 20min, 30min, 40min, 50min, etc.

[0075] Furthermore, the densified veneer and the second wet-heat shaping product having the first adhesive are assembled and hot-pressed, and the densified veneer is located on the surface layer to obtain a first formed body.

[0076] In some specific embodiments, the amount of the first adhesive is 150-350 g / m 2 , 170g / m 2 , 200g / m 2 , 220g / m 2 , 250g / m 2 , 280g / m 2 , 300g / m 2 , 320g / m 2 In general, the first adhesive of the present invention can be a hot pressing adhesive. When the thickness of the pressed material is small, the hot pressing efficiency is high and curing can be achieved in a short time. Specifically, in the present invention, the first adhesive is selected from one or a combination of two or more of isocyanate, phenolic resin, urea-formaldehyde resin, and melamine formaldehyde resin.

[0077] Specifically, the compression rate of the hot pressing is 1%-10%, for example: 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% and the like; the temperature of the hot pressing is 100-170°C, for example: 110°C, 120°C, 130°C, 140°C, 150°C, 160°C and the like; the time of the hot pressing is 0.5-3min / mm, for example: 0.7min / mm, 1min / mm, 1.2min / mm, 1.5min / mm, 1.8min / mm, 2min / mm, 2.2min / mm, 2.5min / mm, 2.8min / mm and the like.

[0078] Furthermore, in the present invention, the thickness of the first molded body is not more than 35 mm.

[0079] Optionally, a third wet heat setting product is selected and hot pressed with the second wet heat setting product having the first adhesive to obtain a second molded body. Specifically, the compression rate of the hot pressing is 1%-10%, for example: 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, etc.; the temperature of the hot pressing is 100-170°C, for example: 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, etc.; the time of the hot pressing is 0.5-3min / mm, for example: 0.7min / mm, 1min / mm, 1.2min / mm, 1.5min / mm, 1.8min / mm, 2min / mm, 2.2min / mm, 2.5min / mm, 2.8min / mm, etc.

[0080] In the present invention, the method of assembling the first molded body and the second molded body is not particularly limited, and the assembly can be performed as required. Specifically, the wood grains between the veneers can be substantially parallel (e.g. Figure 2 ), or it may be roughly vertical (as shown in Figure 1 That is, the present invention can realize the production of wooden structural materials by assembling the blanks along the grain, or by assembling the blanks in a crisscross pattern.

[0081] Finally, in the presence of the second adhesive, two first molded bodies are selected and cold pressed with the second molded body or sawn timber to obtain a wood structure material; wherein the second molded body is located between the two first molded bodies, and the densified veneers in the first molded bodies are located away from the second molded body or the sawn timber. In the present invention, the second adhesive can be a cold-pressed adhesive. When the pressed thickness is large, the effect of the thickness on heat transfer can be ignored and the adhesive can be cured at room temperature, but the time is longer than that of the first adhesive.

[0082] In some specific embodiments, the second adhesive comprises one or both of polyurethane and latex adhesive. Specifically, the amount of the second adhesive is 80-180 g / m 2 , 90g / m 2 , 100g / m 2 , 110g / m 2 , 120g / m 2 , 130g / m 2 , 140g / m 2 , 150g / m 2 , 160g / m 2 , 170g / m 2 wait.

[0083] Specifically, the thickness of the second molded body or the sawn timber is not more than 35 mm. In the present invention, the performance of the second molded body and the sawn timber is not as good as that of the first molded body, and thus can be used as a neutral layer that is substantially free of stress. The present invention does not specifically limit the number of the second molded body and / or the sawn timber, and can be set as needed, generally 1, 3, 5, etc.

[0084] In some specific embodiments, the cold pressing pressure is 1-2MPa, for example: 1.2MPa, 1.5MPa, 1.8MPa, etc.; the cold pressing time is 60-240min, for example: 80min, 100min, 120min, 150min, 180min, 200min, 220min, etc.; the cold pressing temperature is 0-40℃, for example: 5℃, 10℃, 15℃, 20℃, 25℃, 30℃, 35℃, etc.

[0085] Furthermore, the present invention also provides a wooden structural material, which is prepared by the preparation method of the present invention.

[0086] Example

[0087] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0088] Example 1

[0089] 1) The radiata pine logs were rotary cut into 8 mm thick wood veneers, which were steamed and then naturally dried to a moisture content of 30%.

[0090] 2) subjecting the peeled radiata pine veneer to a wet heat setting treatment; wherein the treatment temperature of the wet heat setting treatment is 170° C., the pressure of the wet heat setting treatment is 1 MPa, and the time of the wet heat setting treatment is 60 min.

[0091] 3) According to the dynamic elastic modulus MOE (measured by a dynamic elastic modulus measuring instrument using a resonance method) of each flattened thick veneer, the veneers are divided into two grades: high (≥9000MPa) and low (<9000MPa), and the high-grade thick veneer is selected as the wet heat setting product.

[0092] 4) A wet heat setting product is impregnated with a resin solution and then dried to obtain a dried product. The resin is a phenolic resin, and the mass fraction of the phenolic resin in the resin solution used for impregnation is 20%; the moisture content of the dried product is 10%.

[0093] 5) The dried product is compressed and densified to obtain a densified veneer. The compression and densification process is as follows: the compression rate of the compression and densification is 10%, the compression and densification temperature is 160° C., and the compression and densification time is 30 minutes.

[0094] 6) Take another 4 wet heat setting products and apply phenolic resin adhesive on the surface of the wet heat setting products. The coating amount of the phenolic resin adhesive is 150g / m 2 , single-sided coating. The densified veneer is placed on the surface layer, and hot-pressed with another 4 layers of veneers coated with adhesive to obtain a first molded body with a thickness of 35 mm and a surface layer of a dense layer ( Figure 2 As shown). The compression rate of the hot pressing is 5%, the temperature of the hot pressing is 150°C, and the time of the hot pressing is 1 min / mm. The assembly form is that the wood grains of the veneers are roughly parallel.

[0095] 7) The five wet heat-setting products were coated with phenolic resin and hot-pressed to obtain a second molded body with a thickness of 35 mm ( Figure 3 The coating amount of the phenolic resin adhesive is 150g / m 2 , single-sided coating. The compression rate of hot pressing is 8%, the temperature of hot pressing is 150°C, and the time of hot pressing is 1min / mm. The assembly form is that the wood grains between the veneers are roughly vertical.

[0096] 8) Coating the surfaces of the first molded body and the second molded body with polyurethane adhesive. The surface of the densified single plate of the first molded body is not coated with adhesive. The coating amount of the polyurethane adhesive is 100g / m 2 , double-sided coating.

[0097] 9) The two first molded bodies are used as the upper and lower layers, wherein the densified veneer in the first molded body is located away from the second molded body, and the second molded body is used as the core layer, and then cold-pressed to obtain a wood structure material with a thickness of 105 mm, as follows Figure 4 As shown. The assembly structure of the wood structural material is an orthogonal assembly structure of the first molding body and the second molding body. The cold pressing pressure is 1MPa, the cold pressing time is 120min, and the cold pressing temperature is 25℃.

[0098] Example 2

[0099] 1) The radiata pine logs were rotary cut into 8 mm thick wood veneers, which were steamed and then naturally dried to a moisture content of 30%.

[0100] 2) subjecting the peeled radiata pine veneer to a wet heat setting treatment; wherein the treatment temperature of the wet heat setting treatment is 170° C., the pressure of the wet heat setting treatment is 1.8 MPa, and the time of the wet heat setting treatment is 30 min.

[0101] 3) According to the dynamic elastic modulus MOE (measured by a dynamic elastic modulus measuring instrument using a resonance method) of each flattened thick veneer, the veneers are divided into two grades: high (≥9000MPa) and low (<9000MPa), and the high-grade thick veneer is selected as the wet heat setting product.

[0102] 4) A wet heat setting product is impregnated with a resin solution and then dried to obtain a dried product. The resin is a phenolic resin, and the mass fraction of the phenolic resin in the resin solution used for impregnation is 20%; the moisture content of the dried product is 10%.

[0103] 5) The dried product is compressed and densified to obtain a densified veneer. The compression and densification process is as follows: the compression rate of the compression and densification is 10%, the compression and densification temperature is 160° C., and the compression and densification time is 30 minutes.

[0104] 6) Take another 4 wet heat setting products and apply phenolic resin adhesive on the surface of the wet heat setting products. The coating amount of the phenolic resin adhesive is 150g / m 2 , single-sided coating. The densified veneer is placed on the surface layer, and hot-pressed with another 4 layers of veneers coated with adhesive to obtain a first molded body with a thickness of 35 mm and a surface layer of a dense layer ( Figure 2 As shown). The compression rate of the hot pressing is 5%, the temperature of the hot pressing is 150°C, and the time of the hot pressing is 1 min / mm. The assembly form is that the wood grains of the veneers are roughly parallel.

[0105] 7) The first molded body and the 35 mm thick sawn timber are coated with polyurethane adhesive. The surface of the densified veneer of the first molded body is not coated with adhesive. The coating amount of the polyurethane adhesive is 150 g / m 2 , double-sided coating.

[0106] 8) The two first molded bodies are used as the upper and lower layers, wherein the densified veneer in the first molded body is located away from the second molded body, and the sawn wood is the core layer, and then cold pressed to obtain a wood structure material with a thickness of 105 mm, as follows Figure 5 As shown. The assembly structure of the wood structural material is that the first forming body and the second forming body are parallel to each other. The cold pressing pressure is 1 MPa, the cold pressing time is 60 minutes, and the cold pressing temperature is 25°C.

[0107] Example 3

[0108] 1) The radiata pine logs were rotary cut into 8 mm thick wood veneers, which were steamed and then naturally dried to a moisture content of 30%.

[0109] 2) subjecting the peeled radiata pine veneer to a wet heat setting treatment; wherein the treatment temperature of the wet heat setting treatment is 150° C., the pressure of the wet heat setting treatment is 1 MPa, and the time of the wet heat setting treatment is 60 min.

[0110] 3) According to the dynamic elastic modulus MOE (measured by a dynamic elastic modulus measuring instrument using a resonance method) of each flattened thick veneer, the veneers are divided into two grades: high (≥9000MPa) and low (<9000MPa), and the high-grade thick veneer is selected as the wet heat setting product.

[0111] 4) A wet heat setting product is impregnated with a resin solution and then dried to obtain a dried product. The resin is a phenolic resin, and the mass fraction of the phenolic resin in the resin solution used for impregnation is 10%; the moisture content of the dried product is 10%.

[0112] 5) The dried product is compressed and densified to obtain a densified veneer. The compression and densification process is as follows: the compression rate of the compression and densification is 8%, the compression and densification temperature is 140° C., and the compression and densification time is 30 minutes.

[0113] 6) Take another 4 wet heat setting products and apply phenolic resin adhesive on the surface of the wet heat setting products. The coating amount of the phenolic resin adhesive is 180g / m 2 , single-sided coating. The densified veneer is placed on the surface layer, and hot-pressed with another 4 layers of veneers coated with adhesive to obtain a first molded body with a thickness of 35 mm and a surface layer of a dense layer ( Figure 1 As shown). The compression rate of hot pressing is 10%, the temperature of hot pressing is 150°C, and the time of hot pressing is 1 min / mm. The assembly form is that the wood grains between the veneers are approximately vertical.

[0114] 7) The five wet heat-setting products were coated with phenolic resin and hot pressed to obtain a second molded body with a thickness of 35 mm. The coating amount of the phenolic resin adhesive was 150 g / m 2 , single-sided coating. The compression rate of hot pressing is 8%, the temperature of hot pressing is 150°C, and the time of hot pressing is 1min / mm. The assembly form is that the wood grains between the veneers are roughly vertical.

[0115] 8) Coating the surfaces of the first molded body and the second molded body with polyurethane adhesive. The surface of the densified single plate of the first molded body is not coated with adhesive. The coating amount of the polyurethane adhesive is 100g / m 2 , double-sided coating.

[0116] 9) The two first molded bodies are used as the upper and lower layers, wherein the densified veneer in the first molded body is located away from the second molded body, and the second molded body is used as the core layer, and then cold-pressed to obtain a wood structure material with a thickness of 105 mm, as follows Figure 6 As shown. The assembly structure of the wood structural material is an orthogonal assembly structure of the first molding body and the second molding body. The cold pressing pressure is 1MPa, the cold pressing time is 120min, and the cold pressing temperature is 25℃.

[0117] Comparative Example

[0118] 1) The radiata pine logs were rotary cut into 8 mm thick wood veneers, which were steamed and then naturally dried to a moisture content of 30%.

[0119] 2) subjecting the peeled radiata pine veneer to a wet heat setting treatment to obtain a wet heat setting product; wherein the wet heat setting treatment temperature is 170° C., the wet heat setting treatment pressure is 1 MPa, and the wet heat setting treatment time is 60 min.

[0120] 3) Coat the surface of the wet heat setting product with phenolic resin adhesive at a coating amount of 150g / m 2 , single-sided coating.

[0121] The 5-layer adhesive-coated wet heat-setting product is assembled and hot-pressed to obtain a 35 mm thick molded body. The hot pressing process is under the conditions of a compression rate of 10%, a hot pressing temperature of 150° C., and a hot pressing time of 1 min / mm. The assembly form is that the wood grains between the veneers are roughly parallel or vertical.

[0122] 4) Coating polyurethane adhesive on the surface of the molded body, wherein the assembly form is that the wood grain between the veneers is roughly parallel, and the surface of the molded body is not coated with adhesive, and the coating amount is 100g / m 2 , double-sided coating.

[0123] 5) The two molded bodies with roughly parallel wood grains are used as the upper and lower layers, and the other molded body with roughly vertical wood grains between the veneers is used as the core layer and cold pressed to obtain a wood structure composite material with a thickness of 105 mm. The cold pressing pressure is 1 MPa, the cold pressing time is 120 minutes, and the cold pressing temperature is 25°C.

[0124] Performance Testing

[0125] The static bending strength and elastic modulus of the material were tested according to GB / T 17657-2013. The results are shown in Table 1.

[0126] Table 1

[0127] category Static bending strength / MPa Elastic modulus / MPa Example 1 60.43 13924 Example 2 58.27 13328 Example 3 50.36 12237 Comparative Example 1 28.64 10753

[0128] It can be seen from Example 1 and Example 3 in Table 1 that the use of the first molded body with a dense surface layer of the present invention can improve the static bending strength and elastic modulus compared with the wood structure composite material of Comparative Example 1. It can be seen from Example 2 that the use of the second molded body or sawn timber in the core layer of the wood structure composite material has little effect on its static bending strength and elastic modulus.

[0129] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0130] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a wood structural material, characterized in that: The following steps are involved: Pre-treating the peeled veneer to obtain a pre-treated product; Performing a wet heat setting treatment on the pretreated product; and detecting the dynamic elastic modulus of the pretreated product after the wet heat setting, and selecting the product with a dynamic elastic modulus of 9000 MPa or more as the wet heat setting product; The first wet heat setting product is selected, immersed in a resin solution and then dried to obtain a dried product; Compressing and densifying the dried product to obtain a densified veneer; Selecting a second moist heat setting product, and providing at least one surface of the second moist heat setting product with a first adhesive; Assembling and hot-pressing the densified veneer and the second wet-heat-setting product having the first adhesive, with the densified veneer being located on the surface layer, to obtain a first formed body; Optionally, the third wet heat setting product is selected and hot-pressed with the second wet heat setting product having the first adhesive to obtain a second molded body; In the presence of a second adhesive, two of the first molded bodies are selected and cold-pressed with the second molded body or sawn timber to obtain a wood structural material; wherein, The second formed body or the sawn timber is located between two first formed bodies, and the densified veneers in the first formed bodies are all located far away from the second formed body or the sawn timber.

2. The preparation method according to claim 1, characterized in that: The thickness of the peeled veneer is 6-20 mm; and / or the moisture content of the pre-treated product is 20-40%.

3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the wet heat setting treatment is 140-210° C.; the pressure of the wet heat setting treatment is 0.5-2.5 MPa; and the time of the wet heat setting treatment is 30-90 min.

4. The preparation method according to any one of claims 1 to 3, characterized in that In the resin solution, the mass fraction of the resin is 10%-30%; preferably, the resin comprises one or a combination of two or more selected from epoxy resin, phenolic resin, urea-formaldehyde resin, melamine formaldehyde resin, and furfuryl alcohol resin; and / or The moisture content of the dried product is 10%-15%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The compression rate of the compression and densification is 10-50%, the temperature of the compression and densification is 100-200° C., and the time of the compression and densification is 10-60 minutes.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The dosage of the first adhesive is 150-350g / m 2 ; and / or The compression rate of the hot pressing is 1%-10%, the temperature of the hot pressing is 100-170° C., and the time of the hot pressing is 0.5-3 min / mm; and / or The thickness of the first molded body is no more than 35 mm.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The second adhesive comprises one or both of polyurethane and latex glue; and / or The dosage of the second adhesive is 80-180g / m 2 .

8. The preparation method according to any one of claims 1 to 7, characterized in that: The thickness of the second formed body or the sawn timber is not more than 35 mm.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The cold pressing pressure is 1-2 MPa, the cold pressing time is 60-240 min, and the cold pressing temperature is 0-40°C.

10. A wooden structural material, prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of colored surface compressive plate

    CN101664949A

  • Method for manufacturing high intensity plywood for engineering structure by utilizing fast growing wood

    CN103991113A

  • Method for compressing and compacting wood materials in vacuum

    CN109591122A

  • Wood structure material and preparation method thereof

    CN111975889A

  • Preparation method of two-dimensional woven environment-friendly and high-strength wood-based composite material

    CN112077954A