Mildew-proof antibacterial composite board and preparation method thereof
Through the composite board technology of modified straw, bamboo particles and wood particles, combined with specific additives, the problem of environmental impact and material performance reduction of wooden board production is solved, and high-strength, antibacterial and mildew-proof and low-cost board production is achieved.
Patent Information
- Application Number
- CN202410924865.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-22
AI Technical Summary
The production of wooden boards requires extensive deforestation, resulting in ecological and environmental impacts, but substitution with other materials will reduce the toughness, strength, plasticity and safety of the boards.
Modified straw, bamboo particles and wood particles are used to press the board layers, combined with silicate, silica, aluminum trichloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt and zinc borate, and connected by adhesives To form a composite board, the modified wood particles are located on the top side, the modified bamboo particles are located in the middle, and the modified straw pressed board layer is located on the bottom side, and are dried, mixed and pressed.
It improves the toughness, strength, antibacterial and anti-mildew properties of the board, reduces raw material procurement costs, and reduces the impact on the environment while maintaining a comfortable experience.
Smart Images

Figure CN118809744A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of board production, and in particular to a mildew-proof and antibacterial composite board and a preparation method thereof. Background Art
[0002] Plates are flat rectangular building material panels made into standard sizes and are widely used in the construction industry, usually as components of walls, ceilings or floors. At the same time, plates also refer to metal plates made by forging, rolling or casting. They are divided into thin plates, medium plates, thick plates, extra thick plates, etc.
[0003] In the prior art, most of the boards are mainly produced from wood, but the production of wood boards requires a large amount of deforestation to obtain raw materials, which is easy to affect the local ecological environment. However, using other materials instead will lead to a decrease in the toughness, strength, plasticity and safety of the boards. Therefore, a mildew-proof and antibacterial composite board and its preparation method are needed to meet people's needs. Summary of the invention
[0004] The purpose of the present invention is to provide a mildew-proof and antibacterial composite board and a preparation method thereof, so as to solve the problem that the production of wood boards proposed in the above background technology requires a large amount of deforestation to obtain raw materials, which is easy to affect the local ecological environment, but the use of other materials instead will lead to a decrease in the toughness, strength, plasticity and safety of the boards.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solutions: a mildew-proof and antibacterial composite board material and a preparation method thereof, wherein the mildew-proof and antibacterial composite board material comprises a modified straw pressed board layer, a modified bamboo particle pressed board layer, a modified wood particle pressed board layer and an adhesive, wherein the adhesive connects the modified straw pressed board layer, the modified bamboo particle pressed board layer and the modified wood particle pressed board layer, the modified wood particle pressed board layer is located on the top side, the modified bamboo particle pressed board layer is located in the middle, and the modified straw pressed board layer connected by the adhesive is located on the bottom side.
[0006] Preferably, the modified wood particle pressed board comprises wood particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, 200 parts of wood particles, 10 parts of silicate, 10 parts of silicon dioxide, 15 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0007] Preferably, the modified bamboo particle pressed board comprises bamboo particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, 200 parts of bamboo particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0008] Preferably, the modified straw particle pressed board layer comprises straw particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, the ingredients include 200 parts of straw pellets, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0009] The following steps are included Step 1: Raw material preparation The raw material wood blocks or board particles are initially crushed and screened to remove impurities to prevent dust, metal debris and powder from affecting subsequent production and processing.
[0010] Step 2: Raw material pretreatment The raw material wood blocks or board particles are crushed into particles of uniform specifications and sieved using a 300-mesh sieve.
[0011] Step 3: Drying The screened wood particles of the same specification are dried using drying equipment to ensure that the moisture content of the wood particles is between 5% and 10%, and then dried using a microwave dryer at 80°C for 5 minutes.
[0012] Step 4: Mixing raw materials It is necessary to mix 200 parts of straw particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate under vacuum conditions, and keep stirring continuously for 60 minutes.
[0013] Step 5: Suppression Preheat the press to 120°C to 140°C, transfer the mixture produced in step 4 to the press, and press the mixture for 5 to 15 minutes to fully fill the mold with the mixture to obtain a pressed plate. Repeat steps 1 to 5 to produce modified straw pressed board layers and modified bamboo particle pressed board layers.
[0014] Step 5: Plywood The three types of boards are installed together using adhesive in the order of modified wood particle pressed board on the top side, modified bamboo particle pressed board in the middle, and modified straw pressed board on the bottom side. The connecting surfaces of the boards need to be polished with coarse sandpaper to create a bonding surface of suitable flatness. The adhesive is epoxy resin glue and needs to be left for 24 hours or dried after bonding.
[0015] The beneficial effects of the present invention are: In the present invention, pressing is used to replace part of the production materials of the board with straw and bamboo. These two materials have a fast regeneration speed, have little impact on the local environment or are even beneficial. In addition, the surface part of the board is still made of wood material, so that the comfort of use of the board will not change, reducing the impact on the quality of the board.
[0016] In the present invention, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt and zinc borate are added in the production of the board, thereby enhancing the strength of the straw, bamboo and wood particles, so that the toughness, strength and bending performance of the supported board are improved, and the finished board has good antibacterial and mildew-proof properties.
[0017] In the present invention, since straw, bamboo and wood particles are used as raw materials, the purchase cost of the raw materials is also reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention provides a structural schematic diagram of a mildew-proof and antibacterial composite board and a preparation method thereof. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Example
[0020] A mildew-proof and antibacterial composite board and a preparation method thereof, comprising a mildew-proof and antibacterial composite board comprising a modified straw pressed board layer, a modified bamboo particle pressed board layer, a modified wood particle pressed board and an adhesive, wherein the adhesive connects the modified straw pressed board layer, the modified bamboo particle pressed board layer and the modified wood particle pressed board, the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board layer is located in the middle, and the modified straw pressed board layer connected by the adhesive is located on the bottom side.
[0021] Further, the modified wood particle pressed board includes wood particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, 200 parts of wood particles, 10 parts of silicate, 10 parts of silicon dioxide, 15 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0022] Further, the modified bamboo particle pressed board includes bamboo particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, 200 parts of bamboo particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0023] Furthermore, the modified straw particle pressed board layer includes straw particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, the ingredients include 200 parts of straw pellets, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
[0024] Furthermore, a method for preparing a mildew-proof and antibacterial composite board comprises the following steps: Step 1: Raw material preparation The raw material wood blocks or board particles are initially crushed and screened to remove impurities to prevent dust, metal debris and powder from affecting subsequent production and processing.
[0025] Step 2: Raw material pretreatment The raw material wood blocks or board particles are crushed into particles of uniform specifications and sieved using a 300-mesh sieve.
[0026] Step 3: Drying The screened wood particles of the same specification are dried using drying equipment to ensure that the moisture content of the wood particles is between 5% and 10%, and then dried using a microwave dryer at 80°C for 5 minutes.
[0027] Step 4: Mixing of raw materials It is necessary to mix 200 parts of straw particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate under vacuum conditions, and keep stirring continuously for 60 minutes.
[0028] Step 5: Suppression Preheat the press to 120°C to 140°C, transfer the mixture produced in step 4 to the press, and press the mixture for 5 to 15 minutes to fully fill the mold with the mixture to obtain a pressed plate. Repeat steps 1 to 5 to produce modified straw pressed board layers and modified bamboo particle pressed board layers.
[0029] Step 5: Plywood The three types of boards are installed together using adhesive in the order of modified wood particle pressed board on the top side, modified bamboo particle pressed board in the middle, and modified straw pressed board on the bottom side. The connecting surfaces of the boards need to be polished with coarse sandpaper to create a bonding surface of suitable flatness. The adhesive is epoxy resin glue and needs to be left for 24 hours or dried after bonding. Example
[0030] The mildew-proof and antibacterial composite board comprises a modified straw pressed board layer, a modified bamboo particle pressed board layer, a modified wood particle pressed board and an adhesive, wherein the modified straw pressed board layer, the modified bamboo particle pressed board layer and the modified wood particle pressed board are connected by the adhesive, the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board layer is located in the middle, and the modified straw pressed board layer connected by the adhesive is located on the bottom side.
[0031] Further, the modified wood particle pressed board includes wood particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and essential oil; Calculated by weight, 200 parts of wood particles, 10 parts of silicate, 10 parts of silicon dioxide, 15 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of essential oil.
[0032] Further, the modified bamboo particle pressed board includes bamboo particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and essential oil; Calculated by weight, 200 parts of bamboo particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of essential oil.
[0033] Furthermore, the modified straw particle pressed board layer includes straw particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and essential oil; Calculated by weight, the ingredients include 200 parts of straw pellets, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of essential oil.
[0034] Furthermore, a method for preparing a mildew-proof and antibacterial composite board comprises the following steps: Step 1: Raw material preparation The raw material wood blocks or board particles are initially crushed and screened to remove impurities to prevent dust, metal debris and powder from affecting subsequent production and processing.
[0035] Step 2: Raw material pretreatment The raw material wood blocks or board particles are crushed into particles of uniform specifications and sieved using a 300-mesh sieve.
[0036] Step 3: Drying The screened wood particles of the same specification are dried using drying equipment to ensure that the moisture content of the wood particles is between 5% and 10%, and then dried using a microwave dryer at 80°C for 5 minutes.
[0037] Step 4: Mixing of raw materials It is necessary to mix 200 parts of straw particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of essential oil under vacuum conditions, and keep stirring continuously for 60 minutes.
[0038] Step 5: Suppression Preheat the press to 120°C to 140°C, transfer the mixture produced in step 4 to the press, and press the mixture for 5 to 15 minutes to fully fill the mold with the mixture to obtain a pressed plate. Repeat steps 1 to 5 to produce modified straw pressed board layers and modified bamboo particle pressed board layers.
[0039] Step 5: Plywood The three types of boards are installed together using adhesive in the following order: the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board is located in the middle, and the modified straw pressed board is located on the bottom side. The connecting surface of the board needs to be polished with coarse sandpaper to obtain a bonding surface of appropriate flatness. The adhesive is epoxy resin glue, which needs to be left for 24 hours or dried after bonding. This method of producing wooden boards can emit different wood aromas depending on the added essential oils, thereby satisfying the preferences of different users for the boards, making the boards have a variety of unique wood aromas and improving the economic value of the boards. Example
[0040] The mildew-proof and antibacterial composite board comprises a modified straw pressed board layer, a modified bamboo particle pressed board layer, a modified wood particle pressed board and an adhesive, wherein the modified straw pressed board layer, the modified bamboo particle pressed board layer and the modified wood particle pressed board are connected by the adhesive, the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board layer is located in the middle, and the modified straw pressed board layer connected by the adhesive is located on the bottom side.
[0041] Further, the modified wood particle pressed board includes wood particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and wood dye; Calculated by weight, 200 parts of wood particles, 10 parts of silicate, 10 parts of silicon dioxide, 15 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of wood dye.
[0042] Further, the modified bamboo particle pressed board includes bamboo particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and wood dye; Calculated by weight, the ingredients include 200 parts of bamboo particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of wood dye.
[0043] Furthermore, the modified straw particle pressed board layer includes straw particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, zinc borate, and wood dye; Calculated by weight, the ingredients include 200 parts of straw pellets, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of wood dye.
[0044] Furthermore, a method for preparing a mildew-proof and antibacterial composite board comprises the following steps: Step 1: Raw material preparation The raw material wood blocks or board particles are initially crushed and screened to remove impurities to prevent dust, metal debris and powder from affecting subsequent production and processing.
[0045] Step 2: Raw material pretreatment The raw material wood blocks or board particles are crushed into particles of uniform specifications and sieved using a 300-mesh sieve.
[0046] Step 3: Drying The screened wood particles of the same specification are dried using drying equipment to ensure that the moisture content of the wood particles is between 5% and 10%, and then dried using a microwave dryer at 80°C for 5 minutes.
[0047] Step 4: Mixing raw materials It is necessary to mix 200 parts of straw particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, 5 parts of zinc borate, and 10 parts of essential oil under vacuum conditions, and keep stirring continuously for 60 minutes.
[0048] Step 5: Suppression Preheat the press to 120°C to 140°C, transfer the mixture produced in step 4 to the press, and press the mixture for 5 to 15 minutes to fully fill the mold with the mixture to obtain a pressed plate. Repeat steps 1 to 5 to produce modified straw pressed board layers and modified bamboo particle pressed board layers.
[0049] Step 5: Plywood The three types of boards are installed together using adhesive in the following order: the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board is located in the middle, and the modified straw pressed board is located on the bottom side. The connecting surface of the board needs to be polished with coarse sandpaper to obtain a bonding surface of appropriate flatness. The adhesive is epoxy resin glue, which needs to be left for 24 hours or dried after bonding. This method of producing wooden boards can show different wood colors, as well as colors that existing wood does not have, depending on the added wood dyes, thereby better meeting the needs of users and improving the economic value of the boards.
[0050] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A mildew-proof and antibacterial composite board and a preparation method thereof, characterized in that: The mildew-proof and antibacterial composite board comprises a modified straw pressed board layer, a modified bamboo particle pressed board layer, a modified wood particle pressed board and an adhesive, wherein the adhesive connects the modified straw pressed board layer, the modified bamboo particle pressed board layer and the modified wood particle pressed board, the modified wood particle pressed board is located on the top side, the modified bamboo particle pressed board layer is located in the middle, and the modified straw pressed board layer connected by the adhesive is located on the bottom side.
2. The mildew-proof and antibacterial composite board and the preparation method thereof according to claim 1, characterized in that: The modified wood particle pressed board comprises wood particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, 200 parts of wood particles, 10 parts of silicate, 10 parts of silicon dioxide, 15 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
3. The mildew-proof and antibacterial composite board and the preparation method thereof according to claim 1, characterized in that: The modified bamboo particle pressed board comprises bamboo particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt and zinc borate; Calculated by weight, 200 parts of bamboo particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
4. The mildew-proof and antibacterial composite board and the preparation method thereof according to claim 1, characterized in that: The modified straw particle pressed board layer comprises straw particles, silicate, silicon dioxide, aluminum chloride, epoxy resin, paraffin, gypsum powder, copper quaternary ammonium salt, and zinc borate; Calculated by weight, the ingredients include 200 parts of straw pellets, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate.
5. The method for preparing a mildew-proof and antibacterial composite board according to claim 1, characterized in that: The following steps are included Step 1: Raw material preparation The raw material wood blocks or board particles are initially crushed and screened to remove impurities to prevent dust, metal debris and powder from affecting subsequent production and processing. Step 2: Raw material pretreatment The raw material wood blocks or board particles are crushed into particles of uniform specifications and sieved using a 300-mesh sieve. Step 3: Drying The screened wood particles of the same specification are dried using drying equipment to ensure that the moisture content of the wood particles is between 5% and 10%, and then dried using a microwave dryer at 80°C for 5 minutes. Step 4: Mixing of raw materials It is necessary to mix 200 parts of straw particles, 5 parts of silicate, 5 parts of silicon dioxide, 5 parts of aluminum chloride, 20 parts of epoxy resin, 5 parts of paraffin, 10 parts of gypsum powder, 5 parts of copper quaternary ammonium salt, and 5 parts of zinc borate under vacuum conditions, and keep stirring continuously for 60 minutes. Step 5: Suppression Preheat the press to 120°C to 140°C, transfer the mixture produced in step 4 to the press, and press the mixture for 5 to 15 minutes to fully fill the mold with the mixture to obtain a pressed plate. Repeat steps 1 to 5 to produce modified straw pressed board layers and modified bamboo particle pressed board layers. Step 5: Plywood The three types of boards are installed together using adhesive in the order of modified wood particle pressed board on the top side, modified bamboo particle pressed board in the middle, and modified straw pressed board on the bottom side. The connecting surfaces of the boards need to be polished with coarse sandpaper to create a bonding surface of suitable flatness. The adhesive is epoxy resin glue and needs to be left for 24 hours or dried after bonding.
Citation Information
Patent Citations
Method for producing timber floor through waste
CN107053421A
Artificial board containing straw surface layer and wood core layer
CN108177207A
Preparation method of composite laminated wood
CN109249491A
Plant straw ecological board and preparation method thereof
CN113580314A
Cabinet plate and manufacturing process thereof
CN116333510A