Long-acting preservative treatment method for wood containing aromatic aldehyde and application
Through amination and Schiff base reaction with wood, the aromatic aldehyde compounds form chemical bonds with the wood cell wall, which solves the problem of difficulty in fixing the aromatic aldehyde antibacterial active ingredients in wood and achieves long-term antisepsis and environmental modification of wood. , improving its resistance to loss and flame retardancy.
Patent Information
- Application Number
- CN202411035978.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-22
AI Technical Summary
The porous structure of wood makes it difficult for natural antibacterial active ingredients such as aromatic aldehydes to be fixed, easily lost, and unable to exert long-lasting antiseptic effect. Moreover, traditional preservatives contain heavy metals or toxic compounds and have low environmental protection.
3-Aminopropyltriethoxysilane (APTES) is used to aminate the wood, and the aromatic aldehyde compounds form chemical bonds with the wood cell wall through the Schiff base reaction to improve its fixation and long-term effectiveness, and combine acetic acid and inorganic acid. Chemical agents are prepared from water ethanol and heated to achieve grafting and fixation of aromatic aldehydes.
It effectively improves the fixation and loss resistance of aromatic aldehyde antibacterial active ingredients, expands its application in the field of wood preservation, and the method is environmentally friendly and low-cost, and the hydrophobicity and flame retardancy of the wood are also improved.
Smart Images

Figure CN118809752A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wood modification, and in particular relates to a long-term antiseptic treatment method for wood containing aromatic aldehyde and application thereof. Background Art
[0002] Wood is widely used in all aspects of people's lives due to its advantages such as high strength-to-weight ratio, electrical and thermal insulation, thermal insulation, warm touch, and familiar patterns and colors. However, as a natural polymer material, wood is easily attacked by decay fungi, which leads to a decrease in its service life, causing economic losses and waste of resources. Wood preservative treatment can improve the corrosion resistance of wood and extend its service life. Chemical anti-corrosion in wood preservative treatment is one of the effective means to improve the corrosion resistance of wood. Existing wood preservatives are not combined with wood components through strong chemical bonds, which makes the wood preservatives easy to lose and difficult to achieve a long-lasting and effective anti-corrosion effect. In addition, some traditional preservatives contain heavy metal components or toxic compounds and are less environmentally friendly.
[0003] The improvement of public environmental awareness has promoted the development of environmentally friendly wood preservative treatment methods, and natural products with a wide range of sources, low toxicity and biodegradability have received increasing attention. Natural products with antibacterial activity can improve the antiseptic properties of wood while taking into account green environmental protection, and have become a current research hotspot. Aromatic aldehyde compounds such as vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde are used as food additives. They are low-toxic active compounds and pose no risk to human health and the environment when used in moderation. These four natural products have been industrialized and have low costs while taking into account environmental protection. For example, the price of food-grade vanillin is about 30¥ / kg. Studies have found that aromatic aldehyde compounds such as vanillin, cinnamaldehyde, syringaldehyde, etc. show antibacterial activity against wood decay fungi and have the prospect of being used in wood preservation.
[0004] However, the porous structure of wood is not conducive to the fixation of low molecular weight preservatives and small molecule natural products in wood. Therefore, the difficulty of fixing and easy loss of small molecule natural products such as vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde in wood is one of the technical difficulties in their application in wood preservation. When used outdoors, the antibacterial active ingredients impregnated in the pores of wood are easily lost with rainwater, resulting in a decrease in activity and failure to exert a long-term antiseptic effect. Therefore, improving the fixation of antibacterial active ingredients in wood is extremely important for long-term antiseptic. Summary of the invention
[0005] The purpose of the present invention is to provide a long-term antiseptic treatment method for wood containing aromatic aldehydes and its application, which can improve the fixation of aromatic aldehyde antibacterial active ingredients in wood and improve its long-term effectiveness; in addition, the treatment can also improve the hydrophobicity and flame retardancy of wood, so the method can also be used in wood flame retardant modification or wood waterproof modification.
[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a long-term antiseptic treatment method for wood containing aromatic aldehydes, comprising the following steps:
[0007] (1) soaking the wood to be treated in 3-aminopropyltriethoxysilane to prepare amination wood;
[0008] (2) dissolving the aromatic aldehyde in anhydrous ethanol and adding acetic acid to prepare a chemical agent for treating wood;
[0009] (3) The aminated wood is immersed in the chemical agent, and subjected to heating treatment under normal pressure or vacuum pressure conditions, so that the aromatic aldehyde is grafted onto the wood cell wall through 3-aminopropyltriethoxysilane to obtain the aromatic aldehyde grafted wood.
[0010] Furthermore, in step (1), the wood to be treated is immersed in 3-aminopropyltriethoxysilane and treated for 10-60 minutes under dry conditions.
[0011] Preferably, in step (2), the mass volume ratio of the aromatic aldehyde, acetic acid and anhydrous ethanol is (10-40) mg: (0.001-0.01) mg: 1 mL.
[0012] Preferably, in step (2), the aromatic aldehyde is one or more of vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde.
[0013] Preferably, in step (3), the normal pressure heating treatment conditions are: 40-80° C. normal pressure reaction for 4-12 hours.
[0014] Preferably, in step (3), the heating treatment conditions under vacuum pressure are: first treat under vacuum conditions of 0.07-0.08 MPa for 10-15 min, then pressurize to 0.7-0.9 MPa for 15-30 min, and finally react at normal pressure at 40-80°C for 4-12 h.
[0015] The present invention also provides application of the above-mentioned long-term antiseptic treatment method for wood containing aromatic aldehyde in antiseptic modification of wood, flame retardant modification of wood or waterproof modification of wood.
[0016] The present invention utilizes the Schiff base reaction of amination wood, uses an aminosilane coupling agent to react with the abundant hydroxyl groups of wood to amination the wood, and then causes the aromatic aldehyde to undergo a Schiff base reaction with the wood, thereby grafting the aromatic aldehyde onto the cell wall of the wood. The generation of Schiff base not only improves the antibacterial activity of the aromatic aldehyde compounds, but also improves the corrosion resistance and long-term effectiveness of the wood. Based on this, other aldehyde compounds except vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde can be grafted onto the cell wall of the wood using the same or similar technical scheme as the present invention, further expanding the application of aldehyde compounds in the field of wood preservation, and showing broad application prospects.
[0017] The wood preservative modification treatment method of the present invention is a two-step method, including immersion in 3-aminopropyl triethoxysilane (APTES) and heating and immersion treatment in an ethanol solution containing aromatic aldehydes. The aromatic aldehyde (taking vanillin as an example) is grafted onto the wood cell wall in the form of a Schiff base through APTES. The chemical reaction schematic diagram and chemical reaction formula involved are as follows: Figure 1 As shown, the process flow and principle diagram involved are as follows Figure 7 shown.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) The present invention can enable the environmentally friendly antiseptic and antibacterial active ingredients of aromatic aldehydes to form effective chemical bonds with the cell walls of wood, so that the antiseptic and antibacterial active ingredients are effectively fixed on the wood, improving its anti-loss property, solving the technical problem that small molecule natural antibacterial active ingredients such as aromatic aldehydes are difficult to fix and easy to lose in wood, and expanding the application of aromatic aldehyde compounds in the field of wood antiseptic technology.
[0020] 2) In the present invention, vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde are natural antibacterial active ingredients of plant origin, which are widely used in additives such as food flavors; the auxiliary agent used is a cheap and harmless silane coupling agent, and the chemical agent used is a new type of environmentally friendly wood preservative. Therefore, the method of the present invention is a green wood antiseptic modification method.
[0021] 3) Wood has low reactivity, and most surface chemical modification methods require high temperatures or complex reaction conditions. The present invention utilizes the high reactivity of APTES to aminize the inactive hydroxyl groups on the wood surface to improve its reactivity. The present invention uses a Schiff base reaction with mild reaction conditions to fix the four aromatic aldehydes on the wood surface. The method is simple in process and easy to implement.
[0022] 4) The present invention does not reduce the excellent properties of wood such as mechanics, texture, color, etc., and the present invention allows the antiseptic and antibacterial components to form chemical bonds with the wood, which has better durability. Experiments have confirmed that four aromatic aldehydes, namely vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde, have significant inhibitory effects on wood decay fungi such as Trametes versicolor and Gloeophyllum trabeum. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram and chemical reaction formula of the chemical reaction involved in the grafting of aromatic aldehydes onto wood cell walls in the form of Schiff base via APTES in the present invention, (a) is a schematic diagram of the chemical reaction, and (b) is a chemical reaction formula;
[0024] Figure 2It is a schematic diagram of the growth of Coriolus versicolor and Glehnia littoralis cultured with the addition of high concentration (30 mg / mL) vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde grafted D-(+)-cellobiose and xylo-oligosaccharides obtained in Example 1;
[0025] Figure 3 1 is a comparison diagram of the water contact angle test results of the antiseptic treated wood prepared by the method of Example 5, (a) is a cross section, and (b) is a tangential section;
[0026] Figure 4 The equilibrium moisture content and moisture absorption and swelling resistance test results of the antiseptic treated wood prepared by the method of Example 5, (a) is the equilibrium moisture content, (b) is the moisture absorption and swelling resistance;
[0027] Figure 5 FTIR spectra of vanillin grafted wood (a and b) and vanillin grafted xylo-oligosaccharide (c and d) prepared by the methods of Example 5 and Example 1;
[0028] Figure 6 is a schematic diagram of the limiting oxygen index of four aromatic aldehyde grafted woods prepared by the method of Example 5;
[0029] Figure 7 It is the process flow and principle schematic diagram of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Since the test of wood antiseptic performance is time-consuming and not conducive to the definition of the reaction parameters of aromatic aldehyde-treated wood, Examples 1-3 use D-(+)-cellobiose and oligoxylose, which are model substances constituting wood, to replace wood, and provide a method for antibacterial treatment of a wood model substance containing aromatic aldehydes, and prepare aromatic aldehyde-treated wood model substances with different parameters. In addition, since wood components are complex and difficult to dissolve, it is not conducive to the characterization of the chemical structure of aromatic aldehyde-treated wood. The aromatic aldehyde-modified wood model substances obtained in Examples 1-3 are conducive to further proving the chemical bond between wood and aromatic aldehydes. Example 4 provides a test method for the antibacterial activity of treated wood model substances against wood decay fungi, which is used to define the effective range of reaction parameters of aromatic aldehyde-treated wood. Examples 5-7 provide methods for evaluating the corrosion resistance, dimensional stability, flame retardancy and other properties of aromatic aldehyde-treated wood prepared using parameters within the effective range and treated wood.
[0032] Example 1
[0033] A method for antibacterial treatment of a wood model containing aromatic aldehydes comprises the following steps:
[0034] (1) Weigh 5 g of xylo-oligosaccharide and soak it in 50 mL of APTES, react under dry conditions for 30 min, collect the precipitate by centrifugation, wash it with anhydrous ethanol several times, and then dry it to obtain amino-modified xylo-oligosaccharide;
[0035] (2) 3000 mg of vanillin and 0.5 mg of acetic acid were added to 100 mL of anhydrous ethanol and mixed and dissolved to prepare a chemical agent, wherein the concentration of vanillin in the chemical agent was 30 mg / mL;
[0036] (3) Weigh 3 g of amino-modified xylo-oligosaccharide and add it to the chemical agent. Condensation reflux is carried out at 60° C. for 4 h under normal pressure. After filtration, the obtained xylo-oligosaccharide is sonicated with ethanol until there is no ultraviolet absorption at 279 nm. Finally, it is dried at 60° C. and sealed for storage to obtain high-concentration (30 mg / mL) vanillin-grafted xylo-oligosaccharide.
[0037] According to the above method, vanillin was replaced with cinnamaldehyde, syringaldehyde and protocatechuic aldehyde, and oligoxylose was replaced with D-(+)-cellobiose, to prepare high concentration (30 mg / mL) of vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde grafted oligoxylose and D-(+)-cellobiose.
[0038] Example 2
[0039] A method for antibacterial treatment of a wood model containing aromatic aldehydes comprises the following steps:
[0040] (1) Weigh 5 g of xylo-oligosaccharide and soak it in 50 mL of APTES, react under dry conditions for 30 min, collect the precipitate by centrifugation, wash it with anhydrous ethanol several times, and then dry it to obtain amino-modified xylo-oligosaccharide;
[0041] (2) 2000 mg of vanillin and 0.3 mg of acetic acid were added to 100 mL of ethanol and mixed and dissolved to prepare a chemical agent, wherein the concentration of vanillin in the chemical agent was 20 mg / mL;
[0042] (3) Weigh 3 g of amino-modified xylo-oligosaccharide and add it to the chemical agent, condense and reflux at 60°C for 4 h under normal pressure, filter the obtained xylo-oligosaccharide, sonicate it with ethanol until there is no ultraviolet absorption at 279 nm, and finally dry it at 60°C and seal it to obtain medium concentration (20 mg / mL) vanillin-grafted xylo-oligosaccharide.
[0043] Example 3
[0044] A method for antibacterial treatment of a wood model containing aromatic aldehydes comprises the following steps:
[0045] (1) Weigh 5 g of xylo-oligosaccharide and soak it in 50 mL of APTES solution, react it under dry conditions for 30 min, collect the precipitate by centrifugation, wash it with anhydrous ethanol several times, and then dry it to obtain amino-modified xylo-oligosaccharide;
[0046] (2) 1000 mg of vanillin and 0.5 mg of acetic acid were added to 100 mL of ethanol and mixed and dissolved to prepare a chemical agent, wherein the concentration of vanillin in the chemical agent was 10 mg / mL;
[0047] (3) Weigh 3 g of amino-modified oligoxylose and add it to the chemical agent to react at 60° C. under condensation reflux and normal pressure for 4 h. After filtration, the obtained oligoxylose is sonicated with ethanol until there is no ultraviolet absorption at 279 nm. Finally, it is dried at 60° C. and sealed to obtain low-concentration (10 mg / mL) vanillin-grafted oligoxylose.
[0048] Example 4
[0049] This example gives an evaluation experiment of the antibacterial activity of aromatic aldehyde grafted wood model on wood decay fungi. The high concentration (30 mg / mL) of four aldehyde compounds grafted with xylooligosaccharides or D-(+)-cellobiose obtained in Example 1 was placed on a clean bench for UV sterilization for 15 minutes in advance. After sterilization, 1.44 g was added to 48 mL of sterilized potato agar medium (PDA) and mixed evenly to prepare a culture medium containing 30 mg / mL modified xylooligosaccharides or D-(+)-cellobiose (inhibitory concentration of 30 mg / mL), aiming at selecting the optimal wood model for reaction with aromatic aldehydes; vanillin grafted xylooligosaccharides As a representative example, the final antibacterial concentrations of the high concentration (30 mg / mL) vanillin-grafted xylooligosaccharides obtained in Example 1 and mixed with the culture medium were 30 mg / mL, 20 mg / mL and 10 mg / mL, respectively, for the purpose of defining the antibacterial concentration range; the high concentration (30 mg / mL), medium concentration (20 mg / mL) and low concentration (10 mg / mL) vanillin-grafted xylooligosaccharides obtained in Examples 1-3 were mixed with the culture medium according to the above steps and the final antibacterial concentration was 30 mg / mL, for the purpose of defining the aromatic aldehyde reaction concentration.
[0050] The evenly dissolved culture medium containing the modified substance was transferred to a culture dish with a pipette and mixed. After solidification, 4.4 mm active fungus cakes of wood white rot fungus Trametes versicolor and wood brown rot fungus Gloeophyllum trabeum were inoculated. The diameter of the fungus ring and the growth of the two fungi were recorded on days 2, 6, 10, and 14.
[0051] like Figure 2As shown, the four aromatic aldehyde grafted oligoxylose (hemicellulose model) prepared by the method described in Example 1 showed strong antibacterial activity against wood decay fungi, while aromatic aldehyde grafted D-(+)-cellobiose (cellulose model) had no antibacterial activity against wood decay fungi, and guaiacol (lignin model) itself showed strong antibacterial activity against wood decay fungi, and the occurrence of the reaction could not be judged by the antibacterial activity of the grafted product. This indicates that the binding component of the method described in Example 1 with wood may be hemicellulose, and therefore, oligoxylose was selected as a representative model of wood.
[0052] Table 1 Antibacterial activity test results of aromatic aldehyde grafted oligoxylose obtained in Example 1 against wood decay fungi at different antibacterial concentrations
[0053]
[0054] As shown in Table 1, when the concentration (inhibitory concentration) of vanillin grafted xylo-oligosaccharide obtained in Example 1 in the culture medium was 30 and 20 mg / mL, the growth of two wood decay fungi could be completely inhibited, and the mycelial diameter did not grow after 14 days of culture. When the inhibitory concentration was reduced to 10 mg / mL, the antibacterial activity decreased significantly, and the mycelial diameters of the white rot fungus-Coriolus versicolor and the brown rot fungus-Gromyces fasciatus reached 47.2 mm and 49.0 mm after 14 days of culture. The results showed that the minimum inhibitory concentration of vanillin grafted xylo-oligosaccharide in vitro mediated by APTES should be greater than 10 mg / mL.
[0055] Table 2 Antibacterial activity test results of different concentrations of aromatic aldehyde grafted xylooligosaccharides obtained in Examples 1-3 against wood decay fungi
[0056]
[0057] As shown in Table 2, the xylo-oligosaccharides grafted with vanillin at different concentrations (30, 20, 10 mg / mL) prepared by the method described in Examples 1-3 showed certain antibacterial activity against wood decay fungi, and the mycelium diameter did not increase after 14 days of culture. This is because both vanillin and APTES can improve the antibacterial activity of xylo-oligosaccharides against wood decay fungi. The results show that in the grafting reaction, the grafting of vanillin at a concentration greater than 10 mg / mL can significantly improve the antibacterial activity of xylo-oligosaccharides against wood decay fungi.
[0058] Example 5
[0059] A method for long-term antiseptic treatment of wood containing aromatic aldehydes comprises the following steps:
[0060] (1) Soaking a poplar wood block (Populus tomentosa) in 100 mL of APTES and reacting it for 30 min under dry conditions, washing the wood block with anhydrous ethanol for multiple times and drying it to obtain an amino-treated wood block;
[0061] (2) 6000 mg of vanillin and 1 mg of acetic acid were added to 200 mL of ethanol and mixed and dissolved to prepare a chemical agent;
[0062] (3) The aminated wood block is added to the chemical agent, and the wood block is impregnated for 15 minutes under vacuum conditions of 0.02-0.03 MPa (relative vacuum degree -0.08 to -0.07 MPa), and then the pressure is increased to 0.8 MPa and the pressure is maintained for impregnation for 30 minutes. After impregnation, the wood block is taken out and reacted at 60°C for 4 hours under condensation reflux and normal pressure. The grafted wood block is repeatedly washed with water and ethanol, and ultrasonicated with ethanol until there is no ultraviolet absorption at 279 nm. Finally, it is dried at 60°C and sealed to obtain the vanillin-grafted Populus tomentosa wood.
[0063] According to the above method, vanillin was replaced with cinnamaldehyde, syringaldehyde and protocatechuic aldehyde respectively to prepare cinnamaldehyde, syringaldehyde and protocatechuic aldehyde grafted poplar wood.
[0064] Example 6
[0065] This example gives the antiseptic performance test of the antiseptic treated wood prepared by the wood antiseptic technology after the loss rate test. Test method: Place the treated Populus tomentosa wood obtained in Example 5 in an oven at 40-60°C and dry to constant weight, then place in a beaker for loss rate test, add deionized water to immerse the test material below the deionized water level, and stir continuously; first replace the deionized water once every 6h, 24h, and 48h, and then replace the deionized water once every 48h, for a total of 366h.
[0066] The grafted wood obtained in Example 5 after the above loss test was subjected to a corrosion resistance test. Gloeophyllum trabeum and Trametes versicolor were used as the test species, and Populus tomentosa was used as the test material. The control was a Populus tomentosa sample that had not been modified.
[0067] The test was carried out using the method of GB / T 13942.1-2009 “Durability of wood - Part 1: Laboratory test method for natural corrosion resistance”. The test results are shown in Table 3.
[0068] The calculation formula of mass loss rate R1 is:
[0069] R1%=(M1-M2) / M1%
[0070] Where: M1—the total dry mass of modified wood after anti-loss test;
[0071] M2—Total dry mass of modified wood after anti-loss test and corrosion resistance test.
[0072] Table 3 Corrosion resistance test results of anticorrosion treated Populus tomentosa prepared by the method of Example 5
[0073]
[0074]
[0075] As shown in Table 3, the control is a sample that has not been treated with preservatives. The mass loss rate of the sample exposed to the white rot fungus Trametes versicolor reached 55.1%, and the mass loss rate of the sample exposed to the brown rot fungus Gloeophyllum trabeum reached 25.4%. After the loss test, the mass loss of the material exposed to Trametes versicolor and Gloeophyllum trabeum reached 56.0% and 37.5%, respectively. APTES treatment can also improve the corrosion resistance of wood, which may be due to the blockage of wood pores by the unreacted APTES polymerized by hydrolysis. However, the corrosion resistance of APTES-treated wood decreased after loss, which may be due to the dissolution of self-polymerized APTEES that blocked the pores.
[0076] The vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde grafted wood obtained in Example 5 have a corrosion resistance to Coriolus versicolor and Glechoma spp. of above level II, among which the vanillin and cinnamaldehyde grafted wood have a corrosion resistance to Glechoma spp. of level I. After the loss test, the vanillin and cinnamaldehyde grafted wood have a corrosion resistance to Coriolus versicolor and Glechoma spp. of level I, which indicates that the wood preservative treatment method described in Example 5 can significantly improve the loss resistance of vanillin and cinnamaldehyde in wood, and make the corrosion resistance of treated wood play a long-term role. After the loss test, the corrosion resistance level of the syringaldehyde grafted wood to Coriolus versicolor and Glechoma spp. decreased significantly compared with the non-loss wood, indicating that the wood preservative treatment method described in Example 5 cannot significantly improve the loss resistance of syringaldehyde in wood. After the loss test, the corrosion resistance level of protocatechuic aldehyde grafted wood to Coriolus versicolor decreased significantly, while the corrosion resistance level to Glehnia littoralis remained at level I, which may be related to concentration sensitivity. It shows that the protocatechuic aldehyde grafted wood prepared by the wood preservative treatment method described in Example 5 can significantly improve the corrosion resistance of wood to Glehnia littoralis.
[0077] The results of Example 6 show that the wood preservative treatment method described in Example 5 can significantly improve the anti-loss property of vanillin and cinnamaldehyde in wood. After the loss, the corrosion resistance of the vanillin or cinnamaldehyde grafted wood is Class I strong corrosion resistance.
[0078] Example 7
[0079] This example gives a test on the hydrophobicity and dimensional stability of antiseptic treated wood. Test method: The air-dried treated white poplar obtained in Example 5 is used to measure the water contact angle of its cross section and tangential section using an SDC-100 contact angle meter. A sessile drop method is used to drop 5 μL of ultra-clean water on the cross section or tangential section of the wood sample and the water contact angle is recorded at 30 seconds. The treated white poplar obtained in Example 5 is placed in an oven at 105°C and dried until absolutely dry, then immersed in water for 4 days to balance, and the size and mass before and after treatment are measured. The equilibrium moisture content (EMC) and moisture absorption and swelling resistance (ASE) are calculated according to the following formulas.
[0080] EMC (%) = (M3-M4) / M3×100%
[0081] ΔV(%)=(V1-V2) / V1×100%
[0082] ASE(%)=(ΔV0-ΔV1) / ΔV1×100%
[0083] Where: EMC is the equilibrium moisture content of wood, %; M3 is the mass of wood sample before treatment, g; M4 is the mass of wood sample after treatment, g; ΔV is the increase rate of wood volume, %; V1 is the volume of wood sample before treatment, mm 3 ; V2 is the volume of the treated wood sample, mm 3 ; ASE is the moisture absorption and swelling resistance, %; ΔV0 is the material volume increase rate, %; ΔV1 is the processed material volume increase rate, %.
[0084] Example 7 The hydrophobicity and dimensional stability of the antiseptic treated wood obtained in Example 5 were tested. Figure 3 The water contact angles of the cross section and tangential section of Populus tomentosa wood grafted with different aromatic aldehydes are given. The four aromatic aldehyde grafting treatments can significantly increase the water contact angle of the wood. The water contact angles of the cross section and tangential section of the treated wood are both higher than 90°, reaching the hydrophobic level, which indicates that the antiseptic treatment method can significantly improve the hydrophobicity of the wood.
[0085] Figure 4 The equilibrium moisture content and moisture absorption and swelling resistance of different aromatic aldehyde grafted white poplar wood after soaking in water are given. The four aromatic aldehyde grafting treatments can significantly reduce the water absorption rate of wood, and the equilibrium moisture content after soaking is lower than that of the raw material. The four aromatic aldehyde grafting treatments can significantly improve the moisture absorption and swelling resistance of wood, among which vanillin grafted wood has the best effect. This shows that the antiseptic treatment method can significantly improve the hydrophobicity and dimensional stability of wood. The improvement of hydrophobicity is also one of the reasons for the improvement of wood corrosion resistance.
[0086] Figure 5The FTIR spectra of vanillin grafted wood and vanillin grafted xylo-oligosaccharide prepared by the methods of Example 5 and Example 1 are given. Figure 5 a and 5b show that compared with the raw material and APTES-treated wood, the vanillin-grafted wood -1 A new absorption peak appeared at , which may be attributed to the C=O stretching vibration of vanillin or the newly generated C=N stretching vibration. Further verification is needed by the grafting model. Figure 5 c and 5d, compared with APTES-treated xylooligosaccharides, vanillin-grafted xylooligosaccharides have a -1 、1588cm -1 、1514cm -1 、1286cm -1 New absorption peaks appeared at 1643 and 1588 cm -1 The absorption peaks at 1514 and 1286 cm are considered to be the stretching vibrations of -C=N (amide I) and NH (amide II). -1 The absorption peaks at are considered to be the C=C stretching and CO stretching vibrations of the aromatic skeleton, indicating the progress of the Schiff base reaction and the successful grafting of vanillin with oligoxylose or wood.
[0087] Figure 6 The limiting oxygen index of the vanillin grafted wood prepared by the method of Example 5 tested in Example 7 is given. The higher the oxygen concentration required for combustion, the better the flame retardant performance. Figure 6 It can be seen that the limiting oxygen index of the four aromatic aldehyde grafted wood is significantly higher than that of the original material (22.3%), indicating that the four aromatic aldehyde grafting can significantly improve the flame retardancy of wood. Among them, protocatechuic aldehyde has the best effect, with a limiting oxygen index of 32.7%.
Claims
1. A method for long-term antiseptic treatment of wood containing aromatic aldehydes, characterized in that: The following steps are involved: (1) soaking the wood to be treated in 3-aminopropyltriethoxysilane to prepare amination wood; (2) dissolving the aromatic aldehyde in anhydrous ethanol and adding acetic acid to prepare a chemical agent for treating wood; (3) The aminated wood is immersed in the chemical agent, and subjected to heating treatment under normal pressure or vacuum pressure conditions, so that the aromatic aldehyde is grafted onto the wood cell wall through 3-aminopropyltriethoxysilane to obtain the aromatic aldehyde grafted wood.
2. A method for long-term antiseptic treatment of wood containing aromatic aldehydes according to claim 1, characterized in that: In step (1), the wood to be treated is immersed in 3-aminopropyltriethoxysilane and treated for 10-60 minutes under dry conditions.
3. A method for long-term antiseptic treatment of wood containing aromatic aldehydes according to claim 1 or 2, characterized in that: In step (2), the mass volume ratio of the aromatic aldehyde, acetic acid and anhydrous ethanol is (10-40) mg: (0.001-0.01) mg: 1 mL.
4. A method for long-term antiseptic treatment of wood containing aromatic aldehydes according to claim 1 or 2, characterized in that: In step (2), the aromatic aldehyde is one or more of vanillin, cinnamaldehyde, syringaldehyde and protocatechuic aldehyde.
5. A method for long-term antiseptic treatment of wood containing aromatic aldehydes according to claim 1 or 2, characterized in that: In step (3), the normal pressure heating treatment conditions are: 40-80° C. normal pressure reaction for 4-12 hours.
6. A method for long-term antiseptic treatment of wood containing aromatic aldehydes according to claim 1 or 2, characterized in that: In step (3), the heating treatment conditions under vacuum pressure are: first treat at 0.07-0.08Mpa vacuum conditions for 10-15min, then pressurize to 0.7-0.9Mpa for 15-30min, and finally react at 40-80°C under normal pressure for 4-12h.
7. Use of the long-term wood antiseptic treatment method containing aromatic aldehydes as described in any one of claims 1 to 6 in wood antiseptic modification, wood flame retardant modification or wood waterproof modification.
Citation Information
Patent Citations
Method for union modification of wood by treating cell walls through silicon-containing compound and filling cell cavities with polymer
CN102001116A
Preparation method for water-borne cinnamic aldehyde-based wood protective agents
CN106272789A
Antiseptic treatment technology for woodware
CN107398971A
Antimicrobial coatings
WO2025017233A1