Method for preparing polyvinyl alcohol film
Through electrospinning technology that combines ultrasonic treatment and functional nanoparticles, a nanofiber network structure is formed and cross-linked, which solves the problems of unstable film thickness and mechanical properties in the preparation of polyvinyl alcohol films, and achieves efficient and economical High performance membrane preparation.
Patent Information
- Application Number
- CN202411134833.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-22
AI Technical Summary
Traditional polyvinyl alcohol (PVA) film preparation methods are difficult to accurately control the film thickness, and suffer from unstable mechanical properties and insufficient flexibility. Existing improved methods often increase production costs or affect transparency.
It uses electrospinning technology that combines ultrasonic treatment and functional nanoparticles to form a nanofiber network structure, and improves mechanical strength and aging resistance through cross-linking treatment. The process is simple, low-cost, and suitable for industrial production.
It significantly improves the uniformity and mechanical properties of the film, improves the physical properties and environmental resistance of the film, achieves precise control of film thickness and mechanical stability, is suitable for high-demand applications, and the process is economical and environmentally friendly.
Smart Images

Figure CN118809899A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material preparation, and in particular to a method for preparing a polyvinyl alcohol film. Background Art
[0002] Polyvinyl alcohol (PVA) film is widely used in packaging materials, medical supplies, agriculture and other fields due to its excellent physical and chemical properties, such as high transparency, good mechanical strength and biodegradability. However, traditional PVA film preparation methods mainly include solution casting and hot pressing. These methods have some significant limitations in practical applications. Specifically, the solution casting method is difficult to accurately control the thickness of the film, and it is easy to cause shrinkage and unevenness of the film during the drying process, resulting in unstable mechanical properties. In addition, the flexibility and aging resistance of PVA film also need to be improved to meet more demanding application scenarios.
[0003] In response to the above problems, although some improvement methods in the prior art have improved the performance of PVA films to a certain extent, there are still many shortcomings. For example, the flexibility and aging resistance of the film can be improved by adding plasticizers and antioxidants, but new problems are often introduced, such as reduced transparency of the film or increased production costs. Another common problem is that traditional cross-linking treatment methods are complicated and costly, making it difficult to achieve large-scale production.
[0004] Therefore, there is an urgent need for an innovative PVA film preparation method that can overcome these difficulties in the prior art, improve the thickness uniformity, mechanical strength, flexibility and aging resistance of the film, and has a simple process, low cost and is suitable for industrial production. Summary of the invention
[0005] Based on the above purpose, the present invention provides a method for preparing a polyvinyl alcohol film.
[0006] A method for preparing a polyvinyl alcohol film comprises the following steps: S1: dissolving polyvinyl alcohol powder in water, stirring and heating until completely dissolved to form polyvinyl alcohol solution A; S2: ultrasonically treating the polyvinyl alcohol solution A; S3: adding functional nanoparticles to the polyvinyl alcohol solution A after ultrasonic treatment, and stirring thoroughly to form a mixed solution; S4: The mixed solution is made into a nanofiber membrane by electrospinning technology to form a uniform nanofiber network structure; S5: re-dissolving the nanofiber membrane formed by electrospinning in a certain amount of water to form a polyvinyl alcohol solution B, and casting the polyvinyl alcohol solution B onto a prepared substrate to control the thickness of the formed membrane; S6: drying the cast polyvinyl alcohol film under a constant temperature condition to completely evaporate the water in the film, thereby obtaining a preliminarily formed polyvinyl alcohol film; S7: placing the initially formed polyvinyl alcohol film in a cross-linking agent solution for cross-linking treatment, so that a cross-linking structure is formed between molecular chains of the polyvinyl alcohol film; S8: washing the cross-linked polyvinyl alcohol film to remove the residual cross-linking agent, and then drying at room temperature to obtain a final polyvinyl alcohol film.
[0007] Optionally, the S1 specifically includes: S11: Weigh polyvinyl alcohol powder and add it into deionized water at a ratio of 8-12 wt %; S12: stirring the mixture at room temperature for 20-30 minutes to allow the polyvinyl alcohol powder to be initially dissolved and evenly dispersed in the water; S13: heating the stirred mixture to 80-90° C. and maintaining the stirring speed at 300-500 rpm for 2-3 hours until the polyvinyl alcohol is completely dissolved to form a uniform and transparent polyvinyl alcohol solution A; S14: Cool the formed polyvinyl alcohol solution A to room temperature and continue stirring for 10-15 minutes.
[0008] Optionally, the S2 specifically includes: S21: placing the polyvinyl alcohol solution A in a container of the ultrasonic treatment device, ensuring that the liquid level of the solution does not exceed two-thirds of the container; S22: setting the frequency of the ultrasonic treatment device to 20-40 kHz and adjusting the power to 200-400 watts; S23: starting the ultrasonic treatment equipment to perform ultrasonic treatment on the polyvinyl alcohol solution A for 10-20 minutes; S24: During the treatment process, the solution temperature is maintained at 30-40°C to avoid overheating; S25: After the ultrasonic treatment is completed, the polyvinyl alcohol solution A in the container is taken out and allowed to cool to room temperature.
[0009] Optionally, the S3 specifically includes: S31: weighing the functional nanoparticles according to a preset ratio, and slowly adding them into the polyvinyl alcohol solution A after ultrasonic treatment; S32: using a magnetic stirrer to mix solution A with the functional nanoparticles, the stirring speed is set to 200-400 rpm, and the initial stirring time is 10-15 minutes; S33: transferring the mixed solution to a high-speed stirring device, adjusting the stirring speed to 1000-1500 rpm, and continuing stirring for 30-45 minutes to form a uniform mixed solution; S34: After stirring, the mixed solution is allowed to stand for 5-10 minutes to eliminate bubbles.
[0010] Optionally, the functional nanoparticles include graphene oxide, titanium dioxide and carbon nanotubes, wherein the added ratio of graphene oxide is 0.5-1wt%; the added ratio of titanium dioxide is 1-2wt%; and the added ratio of carbon nanotubes is 0.2-0.5wt%.
[0011] Optionally, the S4 specifically includes: S41: The mixed solution is loaded into a syringe, and the needle diameter of the syringe is selected to be 0.2-0.5 mm; S42: Install the syringe on the electrospinning device and set the spinning voltage to 15-25 kV; S43: adjusting the injection rate to 0.5-1.5 mL / h and controlling the solution flow rate to ensure the stability of the spinning process; S44: placing the receiving device in front of the needle and adjusting the spinning distance to 10-20 cm; S45: starting the electrospinning device to allow the mixed solution to form nanofibers under the action of a high voltage field, and to accumulate layer by layer on a receiving device to form a uniform nanofiber network structure.
[0012] Optionally, the S5 specifically includes: S51: weighing the nanofiber membrane formed by electrospinning, and adding it into deionized water at a ratio of 10-15wt%; S52: heating the mixture to 80-90° C. and maintaining a stirring speed of 300-500 rpm for 1-2 hours until the nanofiber membrane is completely dissolved to form a uniform and transparent polyvinyl alcohol solution B; S53: Cooling the polyvinyl alcohol solution B to room temperature and continuing to stir for 10-15 minutes; S54: filtering the polyvinyl alcohol solution B through a filter to remove undissolved particles; S55: uniformly casting the filtered polyvinyl alcohol solution B onto the prepared substrate, using a scraper to evenly distribute the solution, and controlling the film thickness to be 50-150 μm; S56: placing the casted substrate in a dust-free environment, waiting for the water in the solution to partially evaporate, until a preliminarily formed wet film is formed.
[0013] Optionally, the S6 specifically includes: S61: placing the cast polyvinyl alcohol film together with the substrate in a constant temperature drying oven; S62: Setting the temperature of the constant temperature drying oven to 60-70°C; S63: Maintain a constant temperature environment in the drying oven and control the drying time to 4-8 hours to allow the water in the film to evaporate completely; S64: During the drying process, check the state of the film regularly to ensure that the film surface is evenly dried without bubbles or cracks; S65: After drying, the substrate is taken out from the drying oven, and the preliminarily formed polyvinyl alcohol film on the substrate is peeled off after the substrate is cooled to room temperature.
[0014] Optionally, the S7 specifically includes: S71: preparing a crosslinking agent solution, wherein the crosslinking agent is selected from glutaraldehyde, the concentration of which is 0.5-2 wt %, and dissolving it in deionized water, and stirring until completely dissolved; S72: placing the initially formed polyvinyl alcohol film into a cross-linking agent solution, and ensuring that the film is completely immersed in the solution; S73: At room temperature, keep the soaking time for 30-60 minutes; S74: After soaking, remove the cross-linked polyvinyl alcohol film with tweezers to avoid tearing or breaking.
[0015] Optionally, the S8 specifically includes: S81: washing the cross-linked polyvinyl alcohol film with deionized water for 10-15 minutes to remove residual cross-linking agent; S82: placing the cleaned polyvinyl alcohol film on a drying rack to allow moisture on its surface to drip dry naturally; S83: placing the film in a constant temperature drying oven, setting the temperature to 40-50°C, and drying for 4-6 hours to ensure that the water in the film is completely evaporated; S84: Regularly check the film during the drying process to ensure that the film surface is evenly dried without curling or deformation; S85: After drying, the temperature of the drying oven is lowered to room temperature. After the film is cooled to room temperature, the completely dried polyvinyl alcohol film is taken out and ensured to be free of cracks or damage, so as to obtain the final formed polyvinyl alcohol film.
[0016] Beneficial effects of the present invention: The present invention significantly improves the uniformity and mechanical properties of the PVA film by combining ultrasonic treatment, addition of functional nanoparticles and electrospinning technology. The ultrasonic treatment optimizes the dispersibility of the PVA solution, allowing the functional nanoparticles to be evenly distributed in the solution. The nanofiber membrane formed by the electrospinning technology has higher structural uniformity and mechanical strength. This series of treatments not only enhances the physical properties of the membrane, but also improves its ability to resist environmental influences, making it more suitable for demanding application environments.
[0017] The present invention, by re-dissolving the nanofiber membrane after spinning and casting, the thickness of the final membrane can be more accurately controlled, and the mechanical stability and aging resistance of the membrane are significantly improved through cross-linking treatment. The implementation cost of this method is relatively low, and the process is simple, which is suitable for large-scale industrial production. It provides a new way for the preparation of PVA membrane that is more efficient, economical and environmentally friendly, and has high practical value and market potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 A schematic diagram of a method for preparing a polyvinyl alcohol film according to an embodiment of the present invention; Figure 2 Schematic diagram of ultrasonic treatment process according to an embodiment of the present invention. DETAILED DESCRIPTION
[0020] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for more specific description of the embodiments, and are not intended to specifically limit the present invention.
[0021] It should be noted that the references to "one embodiment", "embodiment", "exemplary embodiments", "some embodiments" and the like in the specification indicate that the embodiments described may include specific features, structures or characteristics, but not every embodiment may include the specific features, structures or characteristics. In addition, when a specific feature, structure or characteristic is described in conjunction with an embodiment, it should be within the knowledge of a person skilled in the art to implement such feature, structure or characteristic in conjunction with other embodiments (whether or not explicitly described).
[0022] In general, a term can be understood, at least in part, from its use in context. For example, depending, at least in part, on the context, the term "one or more" as used herein can be used to describe any feature, structure, or characteristic in the singular sense, or can be used to describe a combination of features, structures, or characteristics in the plural sense. Additionally, the term "based on" can be understood as not necessarily intended to convey an exclusive set of factors, but can instead, depending, at least in part, on the context, allow for the presence of other factors that are not necessarily explicitly described.
[0023] Implemented 1 like Figure 1-Figure 2 As shown, a method for preparing a polyvinyl alcohol film comprises the following steps: S1: dissolving polyvinyl alcohol powder in water, stirring and heating until completely dissolved to form a uniform and transparent polyvinyl alcohol solution A; S2: ultrasonically treating the polyvinyl alcohol solution A to improve the uniformity and dispersibility of the solution; S3: adding functional nanoparticles to the polyvinyl alcohol solution A after ultrasonic treatment, and stirring sufficiently to make the nanoparticles evenly dispersed in the solution to form a mixed solution; S4: The mixed solution is made into a nanofiber membrane by electrospinning technology to form a uniform nanofiber network structure; S5: re-dissolving the nanofiber membrane formed by electrospinning in a certain amount of water to form a polyvinyl alcohol solution B, and casting the polyvinyl alcohol solution B onto a prepared substrate to control the thickness of the formed membrane; S6: drying the cast polyvinyl alcohol film under a constant temperature condition to completely evaporate the water in the film, thereby obtaining a preliminarily formed polyvinyl alcohol film; S7: placing the initially formed polyvinyl alcohol film in a cross-linking agent solution for cross-linking treatment, so that a cross-linking structure is formed between molecular chains of the polyvinyl alcohol film, thereby improving the mechanical strength and stability of the film; S8: washing the cross-linked polyvinyl alcohol film to remove the residual cross-linking agent, and then drying at room temperature to obtain a final polyvinyl alcohol film.
[0024] S1 specifically includes: S11: Weigh polyvinyl alcohol powder and add it into deionized water at a ratio of 10 wt %; S12: stirring the mixture at room temperature for 25 minutes to allow the polyvinyl alcohol powder to be initially dissolved and evenly dispersed in the water; S13: heating the stirred mixture to 85° C. and maintaining the stirring speed at 400 rpm for 2.5 hours until the polyvinyl alcohol is completely dissolved to form a uniform and transparent polyvinyl alcohol solution A; S14: The formed polyvinyl alcohol solution A was cooled to room temperature and continued to be stirred for 13 minutes to ensure the uniformity of the solution.
[0025] S2 specifically includes: S21: placing the polyvinyl alcohol solution A in a container of the ultrasonic treatment device, ensuring that the liquid level of the solution does not exceed two-thirds of the container; S22: setting the frequency of the ultrasonic treatment device to 30 kHz and adjusting the power to 300 watts; S23: starting the ultrasonic treatment equipment to perform ultrasonic treatment on the polyvinyl alcohol solution A for 15 minutes; S24: During the treatment process, the solution temperature is maintained at 35°C and the temperature is controlled by an external cooling system to avoid overheating; S25: After the ultrasonic treatment is completed, the polyvinyl alcohol solution A in the container is taken out and the next step is performed after the solution is cooled to room temperature.
[0026] S3 specifically includes: S31: weighing the functional nanoparticles according to a preset ratio, and slowly adding them into the polyvinyl alcohol solution A after ultrasonic treatment; S32: using a magnetic stirrer to mix solution A with the functional nanoparticles, the stirring speed is set to 300 rpm, and the initial stirring time is 13 minutes, so that the nanoparticles are initially dispersed in the solution; S33: transferring the mixed solution to a high-speed stirring device, adjusting the stirring speed to 1200 rpm, and continuing stirring for 40 minutes to ensure that the functional nanoparticles are evenly dispersed in the polyvinyl alcohol solution A to form a uniform mixed solution; S34: After the stirring is completed, the mixed solution is allowed to stand for 8 minutes to eliminate bubbles, and then the next step is performed.
[0027] The functional nanoparticles include graphene oxide, titanium dioxide and carbon nanotubes, wherein the added ratio of graphene oxide is 0.8wt%; the added ratio of titanium dioxide is 1.5wt%; and the added ratio of carbon nanotubes is 0.3wt%.
[0028] S4 specifically includes: S41: The mixed solution is loaded into a syringe, and the needle diameter of the syringe is selected to be 0.3 mm; S42: Install the syringe on the electrospinning device and set the spinning voltage to 20 kV; S43: adjusting the injection rate to 1 mL / h and controlling the solution flow rate to ensure the stability of the spinning process; S44: placing a receiving device (such as a rotating cylinder or a flat plate) in front of the needle, adjusting the spinning distance to 15 cm, and collecting the fibers; S45: starting the electrospinning device to allow the mixed solution to form nanofibers under the action of a high voltage field, and to accumulate layer by layer on a receiving device to form a uniform nanofiber network structure.
[0029] S5 specifically includes: S51: weighing the nanofiber membrane formed by electrospinning, and adding it into deionized water at a ratio of 13 wt %; S52: heating the mixture to 85° C. and maintaining the stirring speed at 400 rpm for 1.5 hours until the nanofiber membrane is completely dissolved to form a uniform and transparent polyvinyl alcohol solution B; S53: Cooling the polyvinyl alcohol solution B to room temperature and continuing to stir for 13 minutes to ensure the uniformity of the solution; S54: filtering the polyvinyl alcohol solution B through a filter to remove undissolved particles; S55: uniformly casting the filtered polyvinyl alcohol solution B onto the prepared substrate, using a scraper to evenly distribute the solution, and controlling the film thickness to be 100 μm; S56: The casted substrate is placed in a dust-free environment, and the water in the solution is allowed to partially evaporate until a preliminarily formed wet film is formed, and then the next step is performed.
[0030] S6 specifically includes: S61: placing the cast polyvinyl alcohol film together with the substrate in a constant temperature drying oven; S62: Setting the temperature of the constant temperature drying oven to 65°C; S63: Maintain a constant temperature environment in a drying oven and control the drying time to 6 hours to allow the water in the film to evaporate completely; S64: During the drying process, check the state of the film regularly to ensure that the film surface is evenly dried without bubbles or cracks; S65: After drying, the substrate is taken out of the drying oven, and after cooling to room temperature, the preliminarily formed polyvinyl alcohol film on the substrate is peeled off to ensure that the film is intact and ready for the next step.
[0031] S7 specifically includes: S71: preparing a crosslinking agent solution, wherein the crosslinking agent is selected from glutaraldehyde, and the concentration is 1 wt %, and the crosslinking agent is dissolved in deionized water, and stirred until completely dissolved; S72: placing the initially formed polyvinyl alcohol film into a cross-linking agent solution, and ensuring that the film is completely immersed in the solution; S73: Keep the immersion time at room temperature for 45 minutes, and gently stir the solution periodically during the process to ensure that the crosslinker is evenly exposed to every part of the membrane; S74: After soaking, remove the cross-linked polyvinyl alcohol film with tweezers to avoid tearing or breaking.
[0032] S8 specifically includes: S81: washing the cross-linked polyvinyl alcohol film with deionized water for 13 minutes to remove residual cross-linking agent; S82: placing the cleaned polyvinyl alcohol film on a drying rack to allow moisture on its surface to drip dry naturally; S83: placing the film in a constant temperature drying oven, setting the temperature to 45°C and the drying time to 5 hours to ensure that the water in the film is completely evaporated; S84: Regularly check the film during the drying process to ensure that the film surface is evenly dried without curling or deformation; S85: After drying, the temperature of the drying oven is lowered to room temperature. After the film is cooled to room temperature, the completely dried polyvinyl alcohol film is taken out and ensured to be free of cracks or damage, so as to obtain the final formed polyvinyl alcohol film.
[0033] Example 2 Step 1: First, we weighed 8g of polyvinyl alcohol powder and added it to 100mL of deionized water with a concentration of 8wt%. Stirred it at room temperature for 20 minutes to dissolve the polyvinyl alcohol powder and evenly disperse it. Next, heated the mixture to 80°C and maintained the stirring speed at 300rpm for 2 hours to ensure that the polyvinyl alcohol was completely dissolved to form a transparent solution. Finally, cooled the solution to room temperature and continued to stir for 10 minutes to facilitate the next step. Step 2: Place the prepared polyvinyl alcohol solution A into a container of an ultrasonic treatment device, adjust the device power to 200 watts, set the frequency to 20 kHz, and perform ultrasonic treatment for 10 minutes. During the process, ensure that the temperature of the solution is maintained at 35°C to avoid affecting the properties of the solution due to excessive temperature; Step 3: Slowly add functional nanoparticles, including graphene oxide (0.5wt%), titanium dioxide (1wt%) and carbon nanotubes (0.2wt%), to the ultrasonically treated polyvinyl alcohol solution A, stir at 200rpm for 10 minutes using a magnetic stirrer, then transfer the mixed solution to a high-speed stirring device, adjust the stirring speed to 1000rpm, and continue stirring for 30 minutes to ensure that the nanoparticles are completely dispersed. After the stirring is completed, the mixed solution is allowed to stand for 5 minutes to eliminate bubbles; Step 4: The obtained mixed solution was loaded into a syringe with a needle diameter of 0.2 mm. The syringe was installed on the electrospinning device, the spinning voltage was set to 15 kV, the injection rate was adjusted to 0.5 mL / h, the solution flow rate was controlled to ensure the stability of the spinning process, and the receiving device was placed 10 cm in front of the needle to form a uniform nanofiber network structure; Step 5: The nanofiber membrane obtained by electrospinning was redissolved in deionized water at a ratio of 10 wt%, heated to 80 °C, and stirred at 300 rpm for 1 hour until the nanofiber membrane was completely dissolved to form a uniform and transparent polyvinyl alcohol solution B. The solution was cooled to room temperature and stirred for 10 minutes, then filtered through a filter to remove undissolved particles. Finally, the filtered solution B was evenly cast onto the prepared substrate, and the solution was evenly distributed using a scraper to control the film thickness to 50 μm. Step 6: Place the cast substrate in a constant temperature drying oven, set the drying temperature to 60°C, maintain a constant temperature environment in the drying oven, control the drying time to 4 hours, and allow the moisture in the film to evaporate completely. Check the state of the film regularly during the drying process to ensure that the film surface is evenly dried without bubbles or cracks; Step 7: Prepare a crosslinker solution, select glutaraldehyde as the crosslinker, the concentration is 0.5wt%, soak the preliminarily formed polyvinyl alcohol film in the crosslinker solution, ensure that the film is completely immersed, and keep the immersion time at room temperature for 30 minutes. After the immersion is completed, gently remove the polyvinyl alcohol film with tweezers to avoid tearing or damage; Step 8: Wash the cross-linked polyvinyl alcohol film with deionized water for 10 minutes to remove residual cross-linking agent. After washing, place the film on a drying rack to allow the surface moisture to drip dry naturally. Then place the film in a constant temperature drying oven with a set temperature of 40°C and a drying time of 4 hours to ensure that the moisture in the film is completely evaporated. Check the film regularly during the drying process to ensure that the film surface is evenly dried without curling or deformation. After drying, lower the drying oven temperature to room temperature. After the film cools to room temperature, take out the completely dried polyvinyl alcohol film to obtain the final polyvinyl alcohol film.
[0034] Example 3 Step 1: First, we weighed 12g of polyvinyl alcohol powder and added it to 100mL of deionized water with a concentration of 12wt%. Stirred it at room temperature for 30 minutes to dissolve the polyvinyl alcohol powder and evenly disperse it. Next, heated the mixture to 90°C and maintained the stirring speed at 500rpm for 3 hours to ensure that the polyvinyl alcohol was completely dissolved to form a transparent solution. Finally, cooled the solution to room temperature and continued to stir for 15 minutes to facilitate the next step. Step 2: Place the prepared polyvinyl alcohol solution A into a container of an ultrasonic treatment device, adjust the device power to 400 watts, set the frequency to 40 kHz, and perform ultrasonic treatment for 20 minutes. During the process, ensure that the temperature of the solution is maintained at 35°C to avoid affecting the properties of the solution due to excessive temperature; Step 3: Slowly add functional nanoparticles, including graphene oxide (1wt%), titanium dioxide (2wt%) and carbon nanotubes (0.5wt%), to the ultrasonically treated polyvinyl alcohol solution A, stir at 400 rpm for 15 minutes using a magnetic stirrer, then transfer the mixed solution to a high-speed stirring device, adjust the stirring speed to 1500 rpm, and continue stirring for 45 minutes to ensure that the nanoparticles are completely dispersed. After the stirring is completed, the mixed solution is allowed to stand for 10 minutes to eliminate bubbles; Step 4: The obtained mixed solution was loaded into a syringe with a needle diameter of 0.5 mm. The syringe was installed on the electrospinning device, the spinning voltage was set to 25 kV, the injection rate was adjusted to 1.5 mL / h, the solution flow rate was controlled to ensure the stability of the spinning process, and the receiving device was placed 20 cm in front of the needle to form a uniform nanofiber network structure; Step 5: The nanofiber membrane obtained by electrospinning was redissolved in deionized water at a ratio of 15 wt%, heated to 90 °C, and stirred at 500 rpm for 2 hours until the nanofiber membrane was completely dissolved to form a uniform and transparent polyvinyl alcohol solution B. The solution was cooled to room temperature and stirred for 15 minutes, then filtered through a filter to remove undissolved particles. Finally, the filtered solution B was evenly cast onto the prepared substrate, and the solution was evenly distributed using a scraper to control the film thickness to 150 μm. Step 6: Place the cast substrate in a constant temperature drying oven, set the drying temperature to 70°C, maintain a constant temperature environment in the drying oven, control the drying time to 8 hours, and allow the moisture in the film to evaporate completely. Check the state of the film regularly during the drying process to ensure that the film surface is evenly dried without bubbles or cracks; Step 7: Prepare a crosslinker solution, select glutaraldehyde as the crosslinker, and the concentration is 2wt%. Soak the preliminarily formed polyvinyl alcohol film in the crosslinker solution to ensure that the film is completely immersed and keep the immersion time at room temperature for 60 minutes. After the immersion is completed, gently remove the polyvinyl alcohol film with tweezers to avoid tearing or damage. Step 8: Wash the cross-linked polyvinyl alcohol film with deionized water for 15 minutes to remove residual cross-linking agent. After washing, place the film on a drying rack to allow the surface moisture to drip dry naturally. Then place the film in a constant temperature drying oven with a set temperature of 50°C and a drying time of 6 hours to ensure that the moisture in the film is completely evaporated. Check the film regularly during the drying process to ensure that the film surface is evenly dried without curling or deformation. After drying, lower the drying oven temperature to room temperature. After the film cools to room temperature, take out the completely dried polyvinyl alcohol film to obtain the final polyvinyl alcohol film.
[0035] Table 1 Comparison of performance parameters of polyvinyl alcohol film finished products It can be seen from Table 1 above that Example 1 is the best example and exhibits the best performance in all performance test items, including tensile strength, elongation at break, air permeability, thermal stability, UV resistance, water vapor permeability and resistance to microbial erosion. Although Examples 2 and 3 are similar in some performance indicators, they are still lower than Example 1 as a whole, indicating that the preparation method of Example 1 is more suitable for producing high-performance polyvinyl alcohol film, which makes it more advantageous in high-demand application fields.
[0036] Table 2 Comparison of economic index parameters of finished polyvinyl alcohol film It can be seen from Table 2 above that Example 1 shows better performance than Examples 2 and 3 in various aspects such as production cost, production time, material utilization rate, energy consumption, product stability, environmental impact and recyclability. Specifically, Example 1 has the lowest production cost, which makes it more cost-effective; Example 1 has the shortest production time, which improves production efficiency; Example 1 has the highest material utilization rate, indicating that its production process has the least material waste; Example 1 has the lowest energy consumption, indicating that its production process is more energy-efficient; the product of Example 1 has the longest stability, which means that it has higher durability and reliability; Example 1 has the lowest CO2 emissions and the smallest burden on the environment; The product of Example 1 is easiest to recycle, which meets the current requirements of environmental protection and sustainable development.
[0037] In summary, Example 1 shows better performance than other examples in terms of technology and economy, and is the preferred method for producing high-performance polyvinyl alcohol film.
[0038] The present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention. In order to make the public have a thorough understanding of the present invention, specific details are described in detail in the following preferred embodiments of the present invention, but those skilled in the art can fully understand the present invention without the description of these details. In addition, in order to avoid unnecessary confusion about the essence of the present invention, well-known methods, processes, procedures, components and circuits are not described in detail.
[0039] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a polyvinyl alcohol film, characterized in that: The following steps are involved: S1: dissolving polyvinyl alcohol powder in water, stirring and heating until completely dissolved to form polyvinyl alcohol solution A; S2: ultrasonically treating the polyvinyl alcohol solution A; S3: adding functional nanoparticles to the polyvinyl alcohol solution A after ultrasonic treatment, and stirring thoroughly to form a mixed solution; S4: The mixed solution is made into a nanofiber membrane by electrospinning technology to form a uniform nanofiber network structure; S5: re-dissolving the nanofiber membrane formed by electrospinning in a certain amount of water to form a polyvinyl alcohol solution B, and casting the polyvinyl alcohol solution B onto a prepared substrate to control the thickness of the formed membrane; S6: drying the cast polyvinyl alcohol film under a constant temperature condition to completely evaporate the water in the film, thereby obtaining a preliminarily formed polyvinyl alcohol film; S7: placing the initially formed polyvinyl alcohol film in a cross-linking agent solution for cross-linking treatment, so that a cross-linking structure is formed between molecular chains of the polyvinyl alcohol film; S8: washing the cross-linked polyvinyl alcohol film to remove the residual cross-linking agent, and then drying at room temperature to obtain a final polyvinyl alcohol film.
2. A method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S1 specifically includes: S11: Weigh polyvinyl alcohol powder and add it into deionized water at a ratio of 8-12 wt %; S12: stirring the mixture at room temperature for 20-30 minutes to allow the polyvinyl alcohol powder to be initially dissolved and evenly dispersed in the water; S13: heating the stirred mixture to 80-90° C. and maintaining the stirring speed at 300-500 rpm for 2-3 hours until the polyvinyl alcohol is completely dissolved to form a uniform and transparent polyvinyl alcohol solution A; S14: Cool the formed polyvinyl alcohol solution A to room temperature and continue stirring for 10-15 minutes.
3. A method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S2 specifically includes: S21: placing the polyvinyl alcohol solution A in a container of the ultrasonic treatment device, ensuring that the liquid level of the solution does not exceed two-thirds of the container; S22: setting the frequency of the ultrasonic treatment device to 20-40 kHz and adjusting the power to 200-400 watts; S23: starting the ultrasonic treatment equipment to perform ultrasonic treatment on the polyvinyl alcohol solution A for 10-20 minutes; S24: During the treatment process, the solution temperature is maintained at 30-40°C to avoid overheating; S25: After the ultrasonic treatment is completed, the polyvinyl alcohol solution A in the container is taken out and allowed to cool to room temperature.
4. A method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S3 specifically includes: S31: weighing the functional nanoparticles according to a preset ratio, and slowly adding them into the polyvinyl alcohol solution A after ultrasonic treatment; S32: using a magnetic stirrer to mix solution A with the functional nanoparticles, the stirring speed is set to 200-400 rpm, and the initial stirring time is 10-15 minutes; S33: transferring the mixed solution to a high-speed stirring device, adjusting the stirring speed to 1000-1500 rpm, and continuing stirring for 30-45 minutes to form a uniform mixed solution; S34: After stirring, the mixed solution is allowed to stand for 5-10 minutes to eliminate bubbles.
5. A method for preparing a polyvinyl alcohol film according to claim 4, characterized in that: The functional nanoparticles include graphene oxide, titanium dioxide and carbon nanotubes, wherein the added ratio of graphene oxide is 0.5-1wt%; the added ratio of titanium dioxide is 1-2wt%; and the added ratio of carbon nanotubes is 0.2-0.5wt%.
6. The method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S4 specifically includes: S41: The mixed solution is loaded into a syringe, and the needle diameter of the syringe is selected to be 0.2-0.5 mm; S42: Install the syringe on the electrospinning device and set the spinning voltage to 15-25 kV; S43: adjusting the injection rate to 0.5-1.5 mL / h and controlling the solution flow rate to ensure the stability of the spinning process; S44: placing the receiving device in front of the needle and adjusting the spinning distance to 10-20 cm; S45: starting the electrospinning device to allow the mixed solution to form nanofibers under the action of a high voltage field, and to accumulate layer by layer on a receiving device to form a uniform nanofiber network structure.
7. A method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S5 specifically includes: S51: weighing the nanofiber membrane formed by electrospinning, and adding it into deionized water at a ratio of 10-15wt%; S52: heating the mixture to 80-90° C. and maintaining a stirring speed of 300-500 rpm for 1-2 hours until the nanofiber membrane is completely dissolved to form a uniform and transparent polyvinyl alcohol solution B; S53: Cooling the polyvinyl alcohol solution B to room temperature and continuing to stir for 10-15 minutes; S54: filtering the polyvinyl alcohol solution B through a filter to remove undissolved particles; S55: uniformly casting the filtered polyvinyl alcohol solution B onto the prepared substrate, using a scraper to evenly distribute the solution, and controlling the film thickness to be 50-150 μm; S56: placing the casted substrate in a dust-free environment, waiting for the water in the solution to partially evaporate, until a preliminarily formed wet film is formed.
8. The method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S6 specifically includes: S61: placing the cast polyvinyl alcohol film together with the substrate in a constant temperature drying oven; S62: Setting the temperature of the constant temperature drying oven to 60-70°C; S63: Maintain a constant temperature environment in the drying oven and control the drying time to 4-8 hours to allow the water in the film to evaporate completely; S64: During the drying process, check the state of the film regularly to ensure that the film surface is evenly dried without bubbles or cracks; S65: After drying, the substrate is taken out from the drying oven, and the preliminarily formed polyvinyl alcohol film on the substrate is peeled off after the substrate is cooled to room temperature.
9. The method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S7 specifically includes: S71: preparing a crosslinking agent solution, wherein the crosslinking agent is selected from glutaraldehyde, the concentration of which is 0.5-2 wt %, and dissolving it in deionized water, and stirring until completely dissolved; S72: placing the initially formed polyvinyl alcohol film into a cross-linking agent solution, and ensuring that the film is completely immersed in the solution; S73: At room temperature, keep the soaking time for 30-60 minutes; S74: After soaking, remove the cross-linked polyvinyl alcohol film with tweezers to avoid tearing or breaking.
10. The method for preparing a polyvinyl alcohol film according to claim 1, characterized in that: The S8 specifically includes: S81: washing the cross-linked polyvinyl alcohol film with deionized water for 10-15 minutes to remove residual cross-linking agent; S82: placing the cleaned polyvinyl alcohol film on a drying rack to allow moisture on its surface to drip dry naturally; S83: placing the film in a constant temperature drying oven, setting the temperature to 40-50°C, and drying for 4-6 hours to ensure that the water in the film is completely evaporated; S84: Regularly check the film during the drying process to ensure that the film surface is evenly dried without curling or deformation; S85: After drying, the temperature of the drying oven is lowered to room temperature, and after the film is cooled to room temperature, the completely dried polyvinyl alcohol film is taken out, and it is ensured that there are no cracks or damages, so as to obtain the final formed polyvinyl alcohol film.